Production method of lithium iron phosphate
The reduction of floc carbon in lithium iron phosphate through isostatic pressure and low temperature carbonization technology has solved the problem of floc carbon affecting electrochemical performance and safety performance in the prior art, and achieved the effect of improving electrochemical performance and safety performance, while maintaining the Stability of other performances.
Patent Information
- Application Number
- CN202410942945.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-07-15
AI Technical Summary
When the prior art reduces floc carbon in lithium iron phosphate, it usually affects its other properties, such as energy density and power density. It is difficult to effectively reduce floc carbon without changing the original process parameters, thereby affecting electrochemistry. Performance and safety performance.
Isostatic pressure and low temperature carbonization technology are used to carbonize the lithium iron phosphate material at a pressure of 10 to 200 MPa and a temperature of 250 to 450°C for 1 to 5 hours to reduce the formation of carbon bubbles and thus reduce the generation of floc carbon.
Effectively reduce floc carbon in lithium iron phosphate, improve its discharge specific capacity and safety performance, and does not change its internal structure and composition, maintain other properties such as energy density and power density, which are simple to operate, low cost and production efficiency. high.
Smart Images

Figure CN118894513A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium iron phosphate preparation, and more specifically, to a production method of lithium iron phosphate. Background Art
[0002] Lithium-ion battery is a new type of secondary battery. Its positive electrode material is usually lithium iron phosphate, which is an olivine-structured lithium-ion battery positive electrode material. It has the advantages of good safety performance, long cycle life, and environmental friendliness. It is widely used in electric vehicles, power tools and other fields. However, lithium iron phosphate has poor conductivity and often needs to be carbon-coated to improve its conductivity. Currently, lithium iron phosphate is generally carbon-coated by pyrolysis of organic carbon sources. These organic carbon sources will form different forms of carbon under high-temperature pyrolysis. Some are tightly coated on the surface of lithium iron phosphate particles with a high degree of graphitization. The other is free at a distance from the lithium iron phosphate particles, which is called flocculent carbon. These flocculent carbons have poor conductivity and thermal conductivity, which will affect the electrochemical properties of lithium iron phosphate and its safety performance during use. Therefore, how to effectively reduce the flocculent carbon in lithium iron phosphate and improve its electrochemical performance is an important issue facing the current lithium iron phosphate preparation technology.
[0003] The prior art also discloses methods for reducing flocculent carbon. For example, the invention patent with publication number CN112768688A discloses a lithium iron phosphate material, a preparation method thereof and a lithium ion battery, comprising the following steps: (1) dispersing reaction raw materials containing lithium, iron and phosphorus, a carbon source and a binder in a solvent and mixing them to obtain a mixture; (2) granulating the mixture to obtain a precursor; (3) pre-calcining the precursor under an oxidizing atmosphere to obtain a pre-calcined product; (4) sintering the pre-calcined product under a protective atmosphere to obtain the lithium iron phosphate material; the inventive method adds a binder during the mixing stage to increase the compactness of the primary particles during subsequent granulation, and pre-calcines the binder in an oxidizing atmosphere before sintering to remove the binder, thereby avoiding the generation of more flocculent carbon after the binder decomposes during high-temperature sintering under a protective atmosphere, promoting the crystal growth of the primary particles inside the secondary particles, and improving the material cycle stability.
[0004] For another example, publication number CN116885327A discloses a recycling process for positive electrode materials of lithium-ion batteries, which removes impurities such as moisture and free carbon by high-temperature baking; the invention patent with publication number CN101371383A mixes graphite powder particles, carbon black and asphalt carbide, kneads the mixture, and then calcines the mixture at 1000°C or higher in a non-oxidizing atmosphere to carbonize it, using asphalt to increase the compactness and oxidative decomposition at high temperature to remove free carbon. During the carbonization process of lithium iron phosphate, the temperature is high and there will be impurities, which seriously affect the high-rate electrochemical performance of the lithium iron phosphate material.
[0005] In summary, the current methods for reducing flocculent carbon are mainly to promote the full pyrolysis of the carbon source by increasing the pyrolysis temperature of the carbon source, or to remove surface free carbon under auxiliary gas, and to improve the dispersion and compactness of the carbon source by adding binders and other substances to lithium iron phosphate, thereby reducing the generation of flocculent carbon. However, these methods change the original process parameters and add other substances, which may affect other properties of lithium iron phosphate, such as energy density, power density, etc. Therefore, how to effectively reduce the flocculent carbon in lithium iron phosphate without affecting other properties of lithium iron phosphate is an important challenge facing the current lithium iron phosphate preparation technology. Summary of the invention
[0006] In view of the above, the present invention provides a method for producing lithium iron phosphate, which can effectively reduce the flocculent carbon in lithium iron phosphate and improve its electrochemical properties and safety performance such as discharge specific capacity without affecting other properties of lithium iron phosphate.
[0007] The present invention provides a method for producing lithium iron phosphate, comprising the steps of raw material batching, grinding, spray drying and high-temperature sintering, wherein an isostatic pressing carbonization step is added between the spray drying and high-temperature sintering steps: the spray-dried lithium iron phosphate material is carbonized at a pressure of 10 to 200 MPa and a temperature of 250 to 450° C. for 1 to 5 hours.
[0008] The raw materials are prepared according to the molar ratio of lithium carbonate, iron phosphate and carbon source of 1:1:1.
[0009] The carbon source is selected from one or two of glucose, sucrose and PEG2000.
[0010] The grinding time was 8 h and the rotation speed was 500 rpm.
[0011] The inlet temperature of the spray drying was 250°C, the outlet temperature was 100°C, and the rotation speed of the atomizing disk was 30,000 rpm.
[0012] The high temperature sintering is carried out in a protective atmosphere, the sintering temperature is 800°C, and the constant temperature sintering time is 6 hours.
[0013] In the process of preparing lithium iron phosphate, the added carbon source is an organic carbon source, and its decomposition step is indispensable. Then in the process of carbon source decomposition, i.e., carbonization, the organic carbon source is decomposed by heat, and gas is produced in the process. Because it is in a molten state when heated, the gas will escape from the inside in the form of bubbles, thus forming carbon bubbles. The flocculent carbon is mainly formed because the carbon bubbles formed in the process make the carbon in the carbon source away from the coating, i.e., lithium iron phosphate, and thus attached to the surface of the lithium iron phosphate material. Due to its poor electrical conductivity and thermal conductivity, it will affect the electrochemical properties of lithium iron phosphate and its safety performance in use. Therefore, eliminating flocculent carbon is of great significance to improving the performance of lithium iron phosphate.
[0014] Therefore, the present invention proposes to carry out isostatic pressing and low-temperature carbonization. Isostatic pressing means that the entire surface of the material has the same pressure under the same pressure, that is, the same pressure is applied to the entire surface of the entire lithium iron phosphate carbon-coated particles; isostatic pressing and low-temperature carbonization means applying a certain pressure and temperature to the lithium iron phosphate material to perform low-temperature decomposition of the carbon source to form a carbon-coated material. Because the same pressure is applied to the surface of the material, the compactness between the particles is effectively improved and the gaps between the particles are reduced. Therefore, it is difficult to form large-volume carbon bubbles during the low-temperature carbonization process, and the generation of carbon bubbles is effectively inhibited, thereby reducing the detachment of carbon components from the particle surface, and then reducing the generation of flocculent carbon. The reduction of flocculent carbon can effectively improve the electrochemical properties of lithium iron phosphate.
[0015] The isostatic carbonization process of lithium iron phosphate in the present invention requires appropriate pressure, temperature and time, wherein too low pressure will lead to incomplete elimination of carbon bubbles and fail to achieve a good treatment effect, and too high pressure will cause deformation of particles, which not only affects the final performance of lithium iron phosphate, but also has a large energy consumption; and appropriate temperature and time are crucial to the carbonization process, too low temperature and too short time will lead to incomplete decomposition of the carbon source, and there will be residual components that continue to decompose, which is not conducive to the performance of lithium iron phosphate, but too high temperature will lead to violent decomposition of the carbon source, resulting in poor carbon coating effect on the surface of the particles, and also reduce the performance of lithium iron phosphate; wherein the carbonization temperature can be set according to the decomposition temperature of the specific carbon source to ensure the carbonization effect, such as the decomposition temperatures of glucose, sucrose, and PEG2000 are 180°C, 250°C and 200°C, respectively, therefore, because the pressure of isostatic carbonization is higher than normal pressure, generally 100-200°C is increased on the basis of the decomposition temperature as the carbonization temperature of isostatic carbonization.
[0016] The beneficial effects of the present invention are: (1) The present invention uses isostatic low-temperature carbonization to place the dry lithium iron phosphate material under a specific pressure and temperature for a suitable period of time for carbonization, which can effectively reduce the generation of carbon bubbles during the carbonization process and eliminate the flocculent carbon in the lithium iron phosphate, thereby improving the electrochemical properties of the lithium iron phosphate, such as the discharge specific capacity, and the safety performance; (2) The present invention uses a physical method to reduce the flocculent carbon in lithium iron phosphate, which will not change the internal structure and composition of lithium iron phosphate. Therefore, while reducing the flocculent carbon, it will not affect other properties of lithium iron phosphate such as energy density and power density; (3) The present invention has simple operation steps, does not require complicated equipment and processes, has low production costs, and has short production time and high production efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 This is a SEM image of the lithium iron phosphate prepared in Example 3 of the present invention.
[0018] Figure 2 This is a SEM image of the lithium iron phosphate prepared in Example 4 of the present invention.
[0019] Figure 3 This is a SEM image of the lithium iron phosphate prepared in Example 5 of the present invention.
[0020] Figure 4 This is a SEM image of the lithium iron phosphate prepared in Example 6 of the present invention.
[0021] Figure 5 It is a SEM picture of the lithium iron phosphate prepared in Comparative Example 1 of the present invention.
[0022] Figure 6 It is a SEM picture of the lithium iron phosphate prepared in Comparative Example 2 of the present invention. DETAILED DESCRIPTION
[0023] The embodiments of the present application will be described in more detail below. The application can be implemented in various forms, and should not be construed as being limited to the embodiments set forth herein, but rather these embodiments are provided to provide a more thorough and complete understanding of the present application. It should be understood that the embodiments of the present application are only for exemplary purposes and are not intended to limit the scope of protection of the present application.
[0024] The embodiment of the present invention is implemented according to the following technical scheme, and the specific steps include: (1) preparing raw materials according to a molar ratio of lithium carbonate, iron phosphate and carbon source of 1:1:1, and then putting the prepared raw materials into a ball mill for grinding, the grinding time is 8 hours, the rotation speed is 500 rpm, and a ground material is obtained, wherein the carbon source is one or two of glucose, sucrose and PEG2000; (2) spray drying the ground material, wherein the inlet temperature of the spray drying is 250° C., the outlet temperature is 100° C., and the speed of the atomizing disk is 30,000 rpm to obtain a dry lithium iron phosphate material; (3) placing the dry lithium iron phosphate material in an isostatic pressing sintering furnace at a pressure of 10 to 200 MPa and a temperature of 250 to 450° C. for carbonization for 1 to 5 hours to obtain an isostatically pressed carbonized material; (4) The isostatically carbonized material is placed in a box-type atmosphere furnace and sintered under a protective atmosphere at a sintering temperature of 800° C. and a constant temperature sintering time of 6 h to obtain the final lithium iron phosphate material.
[0025] Table 1 shows the specific process conditions of Examples 1 to 8 of the present invention and Comparative Examples 1 to 2 and the performance test results of the obtained lithium iron phosphate. Figures 1 to 6 is a SEM image of lithium iron phosphate prepared in Examples 3 to 6 of the present invention and Comparative Examples 1 to 2, wherein Figures 1 to 4 is a SEM image of lithium iron phosphate prepared by the method of the present invention in Examples 3 to 6, Figures 5-6 This is a SEM image of lithium iron phosphate obtained in Examples 1 to 2 without isostatic pressing and low-temperature carbonization treatment.
[0026] Table 1 Specific process conditions of Examples 1 to 8 of the present invention and Comparative Examples 1 to 2 and performance test results of the prepared lithium iron phosphate.
[0027] It can be seen from Table 1 that the performance of the lithium iron phosphate prepared by the method of the present invention in Examples 1 to 8 is significantly better than that of the lithium iron phosphate prepared by Comparative Examples 1 to 2 without isostatic carbonization treatment. Figures 1 to 6 It can also be seen that the flocculent carbon on the surface of the lithium iron phosphate prepared by the method of the present invention is significantly less than the flocculent carbon on the surface of the lithium iron phosphate prepared without isostatic carbonization treatment, indicating that the method of the present invention can effectively eliminate the flocculent carbon. At the same time, the elimination of the flocculent carbon can effectively reduce the powder resistivity of the lithium iron phosphate. The reduction of the powder resistivity of the lithium iron phosphate will increase its electron transmission rate, thereby improving its electrical conductivity and increasing its discharge specific capacity. This fully proves that the method of the present invention can effectively eliminate the flocculent carbon in the lithium iron phosphate and effectively improve the electrochemical performance of the lithium iron phosphate.
[0028] Among them, under the same pressure, the performance of lithium iron phosphate after carbonization treatment at a temperature of 350°C and a time of 3h is better, indicating that suitable carbonization temperature and time have a better effect on the elimination of flocculent carbon; and pressure is essential for the elimination of flocculent carbon and the improvement of the electrochemical performance of lithium iron phosphate. As shown in Examples 1 to 5 and Comparative Examples 1 to 2, all of them use glucose as the carbon source, among which Comparative Example 1 is subjected to a carbonization treatment at a temperature of 350°C and a time of 3h, but no pressure is applied. The electrochemical performance of the lithium iron phosphate obtained is better than that of the lithium iron phosphate obtained in Comparative Example 2 without isostatic carbonization treatment. This is because adding a low-temperature carbonization treatment before high-temperature sintering will make the carbon The source reacts more gently during the melting and decomposition process, reducing the generation of carbon bubbles, thereby reducing flocculent carbon to a certain extent and improving the electrochemical performance of lithium iron phosphate, but it still has a powder resistivity of up to 48.75Ω·cm and a low discharge specific capacity of 155.275mAh / g. After applying pressure, the powder resistivity of lithium iron phosphate is reduced to less than 20Ω·cm, and the specific capacity is greater than 156mAh / g. Among them, the lithium iron phosphate obtained by carbonization treatment at pressures of 10MPa, 100MPa and 200MPa, temperature of 350℃ and time of 3h has better electrochemical performance, with a resistivity of only 6~9Ω·cm and a specific capacity of more than 160mAh / g. Figures 1 to 3 It can also be seen that there is very little flocculent carbon on its surface, indicating that the appropriate carbonization pressure further suppresses the generation of carbon bubbles during the melting and decomposition process of the carbon source, thereby having a more significant effect on the elimination of flocculent carbon in lithium iron phosphate and the improvement of electrochemical performance.
[0029] In addition, due to the difference in carbon sources, the elimination effect of flocculent carbon on the surface of lithium iron phosphate prepared in Examples 6 to 8 and its electrochemical performance are relatively poor compared with those in Examples 1 to 5. Figures 1 to 4 It can also be seen that the surface flocculent carbon in Example 6 is relatively more than that in Examples 3 to 5, and the performance of the lithium iron phosphate is also relatively high; at the same time, the elimination effect of the flocculent carbon and the electrochemical performance of the lithium iron phosphate are also better than the electrochemical performance of the lithium iron phosphate obtained without isostatic carbonization treatment, which also shows that the elimination of the flocculent carbon has a positive effect on improving the electrochemical performance of the lithium iron phosphate.
[0030] In summary, the lithium iron phosphate material obtained by the isostatic pressing low-temperature carbonization treatment at a pressure of 10 to 200 MPa, a temperature of 250 to 450° C., and a time of 1 to 5 h in the method of the present invention contains less flocculent carbon and thus has better electrochemical properties.
[0031] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can easily think of changes or substitutions within the technical scope disclosed in this application, which should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.
Claims
1. A method for producing lithium iron phosphate, comprising the steps of raw material batching, grinding, spray drying and high temperature sintering, It is characterized in that An isostatic pressing carbonization step is added between the spray drying and high-temperature sintering steps: the spray-dried lithium iron phosphate material is carbonized at a pressure of 10 to 200 MPa and a temperature of 250 to 450° C. for 1 to 5 hours.
2. A method for producing lithium iron phosphate according to claim 1, It is characterized in that The raw materials are prepared according to the molar ratio of lithium carbonate, iron phosphate and carbon source of 1:1:
1.
3. A method for producing lithium iron phosphate according to any one of claims 1 or 2, It is characterized in that The carbon source is selected from one or two of glucose, sucrose and PEG2000.
4. A method for producing lithium iron phosphate according to claim 1, It is characterized in that The grinding time is 8 hours and the rotation speed is 500 rpm.
5. A method for producing lithium iron phosphate according to claim 1, It is characterized in that The inlet temperature of the spray drying is 250°C, the outlet temperature is 100°C, and the rotation speed of the atomizing disk is 30000rpm.
6. A method for producing lithium iron phosphate according to claim 1, It is characterized in that The high temperature sintering is carried out in a protective atmosphere, the sintering temperature is 800° C., and the constant temperature sintering time is 6 hours.
Citation Information
Patent Citations
Preparation method of lithium iron phosphate, lithium iron phosphate and lithium ion battery
CN107359336A
Silicon-based composite negative electrode material for lithium ion battery and preparation method thereof, and lithium ion battery negative electrode containing same
CN108123111A
Lithium iron phosphate positive electrode material, preparation method thereof and lithium ion battery
CN115072694A
Biochar / silicon negative electrode material as well as preparation method and application thereof
CN118039882A
Positive electrode material, all solid-state battery, and methods respectively for producing positive electrode material and all-solid state battery
US20150249264A1