Method for preparing active calcium carbonate by utilizing phosphogypsum

Through flotation and acid leach reaction, phosphogypsum is converted into active calcium carbonate with high purity and high whiteness, which solves the problems of high energy consumption and complicated steps when preparing calcium carbonate in the prior art, and achieves high efficiency calcium carbonate preparation improves its performance in filler applications.

CN118894545APending Publication Date: 2024-11-05HUBEI YANGTZE RIVER RESOURCE RECYCLING & EQUIP INNOVATION CENT CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202410840564.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-27
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

The prior art has problems of high energy consumption, cumbersome steps and low conversion efficiency when using phosphogypsum to prepare light calcium carbonate, which leads to its limited promotion in industrial use.

Method used

Through flotation pretreatment, acid leach reaction, flotation and ammonium bicarbonate reaction steps, phosphogypsum is converted into high-purity and high-white active calcium carbonate, and flotation agents and ammonium bicarbonate react to improve calcium carbonate by using flotation agents and ammonium bicarbonate reaction to improve calcium carbonate. hydrophobic properties.

Benefits of technology

It realizes the effective removal of impurities in phosphogypsum, improves the purity and whiteness of calcium carbonate, improves its dispersion performance as a filler, with purity reaching more than 95%, whiteness reaching more than 90%, and simplifies the process flow.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a method for preparing active calcium carbonate by utilizing phosphogypsum, which comprises the following steps: carrying out acid leaching on floated phosphogypsum to obtain anhydrous gypsum, carrying out flotation purification, adding ammonium bicarbonate to react with ammonia water to obtain calcium carbonate, and finally carrying out flotation to obtain the active calcium carbonate. The surface of the prepared active calcium carbonate is coated with a layer of active substances, so that the active calcium carbonate has good hydrophobic performance, the dispersing performance of the active calcium carbonate serving as filler can be improved, the purity of the active calcium carbonate can reach 95% or above, and the whiteness of the active calcium carbonate can reach 90% or above.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of phosphogypsum resource utilization, and specifically relates to a method for preparing active calcium carbonate by utilizing phosphogypsum. Background Art

[0002] Phosphogypsum is a solid waste with calcium sulfate dihydrate as the main component produced during the wet production of phosphoric acid. About 4 to 6 tons of phosphogypsum are produced for every ton of phosphoric acid produced. At present, my country's annual phosphogypsum emissions exceed 70 million tons, and the cumulative emissions exceed 500 million tons. The comprehensive utilization rate of phosphogypsum is less than 50%, resulting in a large amount of phosphogypsum being piled up in the open air, occupying a large amount of land. In addition, phosphogypsum also contains a variety of harmful impurities such as phosphorus, fluorine, magnesium, iron and organic matter. Any discharge and long-term accumulation will cause soil and water pollution, leading to serious environmental problems. Therefore, it is necessary to study the resource utilization of phosphogypsum, develop and optimize the application of phosphogypsum, and turn it into treasure.

[0003] As a calcium source, phosphogypsum can be converted into calcium carbonate through a series of chemical reactions. Calcium carbonate is a common chemical raw material, which is mainly used as a filler and can be widely used in industries and fields such as plastics, papermaking, and rubber. Although my country is one of the countries with extremely rich calcium carbonate resources, in order to reduce environmental damage and maintain ecological balance, calcium carbonate resources in many places cannot be mined in large quantities. The traditional carbonization method for preparing light calcium carbonate requires limestone or marble to be calcined, digested with water, introduced with CO2 to generate precipitation, dehydrated, dried, and crushed. Not only is the energy consumption high, but the quality of the obtained light calcium carbonate is greatly affected by factors such as limestone raw materials, calcination fuel, and process water. Therefore, the preparation of light calcium carbonate using solid waste phosphogypsum rich in calcium ions as raw material not only reduces the consumption of natural mineral resources limestone and marble, but also provides a new direction for the industrial production of resource utilization of phosphogypsum.

[0004] At present, there are many studies on the methods of preparing light calcium carbonate using phosphogypsum. There is a method of preparing light calcium carbonate by calcining and digesting phosphogypsum calcium slag at high temperature to obtain refined calcium hydroxide emulsion, and then introducing CO2; there is a process of preparing light calcium carbonate by leaching desulfurized calcium slag with ammonium chloride and carbonizing it; there is a process of preparing calcium chloride by leaching calcium carbonate slag with hydrochloric acid, and then adding carbonate to deep process calcium chloride to prepare calcium carbonate; there is also a method of synthesizing light calcium carbonate by phase transfer-precipitation pathway using SG as a phase transfer agent. Some of these existing methods have problems such as high experimental energy consumption and cannot be widely used; some have disadvantages such as cumbersome steps, low leaching and conversion efficiency, which are not conducive to industrial application and promotion. Summary of the invention

[0005] In view of the shortcomings of the prior art, the object of the present invention is to provide a method for preparing activated calcium carbonate using phosphogypsum with simple process and high purity and whiteness of calcium carbonate.

[0006] To achieve the above object, the present invention adopts the following technical solution:

[0007] The present invention provides a method for preparing activated calcium carbonate using phosphogypsum, comprising the following steps:

[0008] S1. Slurrying the phosphogypsum with water, adding a first flotation agent for flotation pretreatment, filtering and drying to obtain a first product;

[0009] S2. reacting the first product with an acid, filtering and drying after the reaction to obtain a second product;

[0010] S3. The second product is slurried with water, and the first flotation agent is added for flotation. After the flotation, the product is sieved, and the product under the sieve is filtered and dried to obtain a third product;

[0011] S4. The third product was slurried with water, ammonium bicarbonate and aqueous ammonia were added, and the reaction was stirred and filtered and dried to obtain a fourth product;

[0012] S5. Add water to the fourth product to make a pulp, add a second flotation agent to carry out flotation, filter and dry to obtain the activated calcium carbonate.

[0013] Furthermore, in step S1, the first flotation agent is composed of a first frother, a first collector and water in a mass ratio of 1:2:97, the first frother is tributyl phosphate, and the first collector is a mixture of one or both of linoleic acid and sodium dodecyl sulfate; the first flotation agent accounts for 0.5% to 5% of the mass of the phosphogypsum.

[0014] Furthermore, the first collector is composed of linoleic acid and sodium dodecyl sulfate in a mass ratio of 3:1.

[0015] Furthermore, in step S2, the acid is sulfuric acid, hydrochloric acid or a mixture of both.

[0016] Furthermore, the acid is composed of sulfuric acid and hydrochloric acid in a mass ratio of 3:1.

[0017] Furthermore, in step S2, the mass concentration of the acid is 10% to 60%, the solid-liquid mass ratio of the first product to the acid is 1:1 to 10; the reaction temperature is 60 to 120° C., and the reaction time is 0.5 to 8 h.

[0018] Furthermore, in step S3, the first flotation reagent accounts for 0.5% to 5% of the mass of the second product.

[0019] Furthermore, in step S4, the molar ratio of the third product to the ammonium bicarbonate and the ammonia water is 1:1-10:1-10, the mass fraction of the ammonia water is 5%-30%, and the solid-liquid ratio of the third product to water is 1:1-10; the reaction temperature of the third product with the ammonium bicarbonate and the ammonia water is 10-70°C, and the reaction time is 0.5-8h.

[0020] Furthermore, in step S5, the second flotation reagent is composed of a second collector and water in a mass ratio of 4:96, the second collector is at least one of dodecylamine and oleic acid, and the second flotation reagent accounts for 0.5% to 10% of the mass of the fourth product.

[0021] Furthermore, the second collector is composed of dodecylamine and oleic acid in a mass ratio of 3:1.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] The invention converts phosphogypsum (CaSO4·2H2O) into anhydrous gypsum CaSO4 through the first flotation, acid leaching and the second flotation, so that a large amount of impurities in the phosphogypsum can be effectively removed, and the whiteness and purity of the gypsum are greatly improved, laying a foundation for the conversion of calcium carbonate; calcium carbonate is obtained by reacting ammonium bicarbonate, ammonia water and anhydrous gypsum, and active calcium carbonate with a layer of active material coated on the surface is obtained through the third flotation, so that the active calcium carbonate has good hydrophobicity, can improve the dispersibility of the active calcium carbonate as a filler, and the purity of the active calcium carbonate can reach more than 95%, and the whiteness of the active calcium carbonate can reach more than 90%. DETAILED DESCRIPTION

[0024] The present invention is further described in detail below in conjunction with specific embodiments so that those skilled in the art can more clearly understand the present invention. The examples are only used to explain the present invention and are not used to limit the scope of the present invention. In the embodiments of the present invention, unless otherwise specified, all raw material components are commercially available products well known to those skilled in the art; unless otherwise specified, the technical means used are conventional means well known to those skilled in the art.

[0025] Example 1

[0026] The present embodiment provides a method for preparing activated calcium carbonate using phosphogypsum, comprising the following steps:

[0027] 1) 200 g of phosphogypsum was added with 467 mL of water for slurrying, and 4 g of flotation reagent (tributyl phosphate: linoleic acid: water mass ratio 1:2:97) was added for flotation pretreatment, and 120 g of the first product was obtained after filtration and drying;

[0028] 2) 120 g of the first product was reacted with 720 g of 10% sulfuric acid at 95° C. for 0.5 h. After the reaction was completed, 86.4 g of the second product was obtained by filtering and drying;

[0029] 3) 86.4 g of the second product was slurried with 201 mL of water, and 2 g of flotation agent (tributyl phosphate: linoleic acid: water mass ratio of 1:2:97) was added to carry out flotation. After the flotation, the mixture was sieved with a 100-mesh sieve, and the sieve was filtered and dried to obtain 73.44 g of the third product;

[0030] 4) 85.3 g of ammonium bicarbonate and 183.6 g of 10% ammonia water were stirred evenly in a reaction container; 73.44 g of the third product was slurried with 80 mL of water, added to the reaction container and reacted at 55° C. for 4 h. After the reaction was completed, 52.88 g of the fourth product was filtered and dried;

[0031] 5) 52.88 g of the fourth product was slurried with 125 mL of water, and 1 g of a flotation agent (oleic acid: water mass ratio 4:96) was added for flotation, and the activated calcium carbonate was obtained by filtering and drying.

[0032] Example 2

[0033] The present embodiment provides a method for preparing activated calcium carbonate using phosphogypsum, comprising the following steps:

[0034] 1) 200 g of phosphogypsum was added with 467 mL of water for slurrying, and 6 g of flotation reagent (tributyl phosphate: sodium dodecyl sulfate: water mass ratio 1:2:97) was added for flotation pretreatment, and 135 g of the first product was obtained after filtration and drying;

[0035] 2) 135 g of the first product was reacted with 540 g of a 45% by mass mixture of sulfuric acid and hydrochloric acid (sulfuric acid: hydrochloric acid mass ratio 3:1) at 60° C. for 4 h. After the reaction was completed, the mixture was filtered and dried to obtain 94.5 g of the second product;

[0036] 3) 94.5 g of the second product was slurried with 220 mL of water, and 2 g of flotation agent (tributyl phosphate: sodium dodecyl sulfate: water mass ratio of 1:2:97) was added to carry out flotation. After the flotation, the mixture was sieved with a 100-mesh sieve, and the sieve was filtered and dried to obtain 85.1 g of the third product;

[0037] 4) 148.3 g of ammonium bicarbonate and 70.92 g of 30% ammonia water were stirred evenly in a reaction container; 85.1 g of the third product was slurried with 510 mL of water, added to the reaction container and reacted at 25° C. for 6 h. After the reaction was completed, 61.1 g of the fourth product was filtered and dried;

[0038] 5) 61.1 g of the fourth product was slurried with 142 mL of water, and 5 g of a flotation agent (dodecylamine: water mass ratio 4:96) was added to perform flotation, and the activated calcium carbonate was obtained by filtering and drying.

[0039] Example 3

[0040] The present embodiment provides a method for preparing activated calcium carbonate using phosphogypsum, comprising the following steps:

[0041] 1) 200 g of phosphogypsum was added with 467 mL of water for slurrying, and 2 g of flotation reagent (tributyl phosphate: linoleic acid: sodium dodecyl sulfate: water mass ratio of 1:1.5:0.5:97) was added for flotation pretreatment, and 140 g of the first product was obtained after filtration and drying;

[0042] 2) 140 g of the first product was reacted with 140 g of 60% hydrochloric acid at 120° C. for 6 h. After the reaction was completed, 91.2 g of the second product was obtained by filtering and drying;

[0043] 3) 91.2 g of the second product was slurried with 212 mL of water, and 1 g of a flotation agent (tributyl phosphate: linoleic acid: sodium dodecyl sulfate: water mass ratio of 1:1.5:0.5:97) was added to carry out flotation. After the flotation, the mixture was sieved with a 100-mesh sieve, and the sieve was filtered and dried to obtain 73.87 g of the third product;

[0044] 4) 42.91 g of ammonium bicarbonate and 184.7 g of 20% ammonia water were stirred evenly in a reaction container; 73.87 g of the third product was slurried with 665 mL of water, added to the reaction container and reacted at 65° C. for 1 h. After the reaction was completed, 30 g of the fourth product was filtered and dried;

[0045] 5) 30 g of the fourth product was slurried with 70 mL of water, and 1.2 g of a flotation agent (dodecylamine: oleic acid: water mass ratio 3:1:96) was added to perform flotation, and the activated calcium carbonate was obtained by filtering and drying.

[0046] Comparative Example 1

[0047] This comparative example is based on Example 1, except that there is no step 2) sulfuric acid leaching and step 3) flotation step, and the first product after the flotation pretreatment of phosphogypsum is directly reacted with ammonium bicarbonate and ammonia water, and the obtained reaction product is then floated, and the reaction conditions, reagents and dosage ratios remain unchanged.

[0048] Comparative Example 2

[0049] The difference between this comparative example and Example 1 is that there is no step 5), and the other steps are the same.

[0050] Comparative Example 3

[0051] The method of this comparative example is basically the same as that of Example 1, except that the reaction temperature of step 4) of this comparative example is 75°C.

[0052] Comparative Example 4

[0053] This comparative example is to prepare light calcium carbonate according to the process route disclosed in patent CN116654969A, comprising the following steps:

[0054] 1) Grind the phosphogypsum until it passes through a 120-mesh sieve, wash it with deionized water, put it in an oven to dry, and then take it out for use;

[0055] 2) Add 25% ammonia water and deionized water in a volume ratio of 3:20 into the reactor, introduce carbon dioxide, control the carbon introduction rate to be 160 ml / L, and react for 3 minutes to obtain an ammonium bicarbonate solution;

[0056] 3) reacting phosphogypsum and ammonium bicarbonate solution in a reactor at 40° C., stirring at 300 r / min for 120 min, and filtering to obtain solid A;

[0057] 4) reacting solid A with hydrochloric acid having a concentration of 2 mol / L at a molar mass ratio of 1:2, and filtering to obtain a pure calcium chloride solution;

[0058] 5) reacting the ammonium bicarbonate solution with the purified calcium chloride solution for 90 minutes, and obtaining high-purity calcium carbonate after filtering.

[0059] The performance of the calcium carbonate obtained in the examples of the present invention and the comparative examples was tested, and the results are shown in Table 1.

[0060] Table 1

[0061] Test items purity Whiteness Sedimentation volume mL / g Example 1 96.3% 94% 2.9 Example 2 95.8% 93% 2.9 Example 3 95.2% 93% 2.8 Comparative Example 1 87.2% 84% 2.5 Comparative Example 2 94.1% 90% 2.2 Comparative Example 3 90.1% 91% 2.6 Comparative Example 4 95% 92% 2.4

[0062] From the comparison between Example 1 and Comparative Example 1, it can be seen that the purity and whiteness of the calcium carbonate obtained in Comparative Example 1 without acid leaching and flotation process are significantly lower. The main reason is that acid leaching can not only remove part of the colored impurities, but also expose the impurities inside the crystals during the re-crystallization of calcium sulfate dihydrate to anhydrous calcium sulfate, and the impurities are further removed by flotation, and finally anhydrous gypsum with higher purity and whiteness is obtained. On this basis, the purity and whiteness of calcium carbonate converted from anhydrous gypsum are also higher.

[0063] From the comparison between Example 1 and Comparative Example 2, it can be seen that the sedimentation volume of the calcium carbonate after flotation is larger, indicating that the reagent forms a coating on the surface of the calcium carbonate, increasing its hydrophobicity in water and better dispersibility in water, so the sedimentation volume is larger.

[0064] From the comparison between Example 1 and Comparative Example 3, it can be seen that when the reaction temperature of the conversion step is too high, the degree of conversion of anhydrous gypsum into calcium carbonate becomes lower, which is manifested in a decrease in the purity of calcium carbonate, indicating that too high a temperature will cause the decomposition of ammonium bicarbonate and thus reduce the conversion of calcium carbonate.

[0065] From the comparison between the embodiment of the present invention and comparative example 4, it can be seen that the activated calcium carbonate prepared by the present invention has higher purity and whiteness, and a larger sedimentation volume. The present invention does not need to first carbonize the phosphogypsum and then purify it, but directly obtains high-purity calcium carbonate by a one-step carbonization reaction, and at the same time forms a coating on the surface of the calcium carbonate by flotation, thereby increasing its hydrophobicity in water.

[0066] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing activated calcium carbonate using phosphogypsum, characterized in that: The following steps are involved: S1. Slurrying the phosphogypsum with water, adding a first flotation agent for flotation pretreatment, filtering and drying to obtain a first product; S2. reacting the first product with an acid, filtering and drying after the reaction to obtain a second product; S3. The second product is slurried with water, and the first flotation agent is added for flotation. After the flotation, the product is sieved, and the product under the sieve is filtered and dried to obtain a third product; S4. The third product was slurried with water, ammonium bicarbonate and aqueous ammonia were added, and the reaction was stirred and filtered and dried to obtain a fourth product; S5. Add water to the fourth product to make a pulp, add a second flotation agent to carry out flotation, filter and dry to obtain the activated calcium carbonate.

2. The method for preparing activated calcium carbonate using phosphogypsum according to claim 1, characterized in that: In step S1, the first flotation reagent is composed of a first frother, a first collector and water in a mass ratio of 1:2:97, the first frother is tributyl phosphate, and the first collector is a mixture of one or both of linoleic acid and sodium dodecyl sulfate; the first flotation reagent accounts for 0.5% to 5% of the mass of the phosphogypsum.

3. The method for preparing activated calcium carbonate using phosphogypsum according to claim 2, characterized in that: The first collector is composed of linoleic acid and sodium dodecyl sulfate in a mass ratio of 3:

1.

4. The method for preparing activated calcium carbonate using phosphogypsum according to claim 1, characterized in that: In step S2, the acid is sulfuric acid, hydrochloric acid or a mixture of the two.

5. The method for preparing activated calcium carbonate using phosphogypsum according to claim 4, characterized in that: The acid is composed of sulfuric acid and hydrochloric acid in a mass ratio of 3:

1.

6. The method for preparing activated calcium carbonate using phosphogypsum according to claim 1, characterized in that: In step S2, the mass concentration of the acid is 10% to 60%, the solid-liquid mass ratio of the first product to the acid is 1:1 to 10; the reaction temperature is 60 to 120° C., and the reaction time is 0.5 to 8 hours.

7. The method for preparing activated calcium carbonate using phosphogypsum according to claim 1, characterized in that: In step S3, the first flotation reagent accounts for 0.5% to 5% of the mass of the second product.

8. The method for preparing activated calcium carbonate using phosphogypsum according to claim 1, characterized in that: In step S4, the molar ratio of the third product to the ammonium bicarbonate and the ammonia water is 1:1-10:1-10, the mass fraction of the ammonia water is 5%-30%, and the solid-liquid ratio of the third product to water is 1:1-10; the reaction temperature of the third product, the ammonium bicarbonate and the ammonia water is 10-70°C, and the reaction time is 0.5-8h.

9. The method for preparing activated calcium carbonate using phosphogypsum according to claim 1, characterized in that: In step S5, the second flotation reagent is composed of a second collector and water in a mass ratio of 4:96, the collector is at least one of dodecylamine and oleic acid, and the second flotation reagent accounts for 0.5% to 10% of the mass of the fourth product.

10. The method for preparing activated calcium carbonate using phosphogypsum according to claim 9, characterized in that: The second collector is composed of dodecylamine and oleic acid in a mass ratio of 3:1.

Citation Information

Patent Citations

  • Method for preparing high-purity calcium carbonate from ardealite

    CN116654969A