Preparation method of high-purity 4N zinc oxide

The method of preparing high-purity zinc oxide in a mixture of argon and oxygen by electro-explosion solves the problem of insufficient purity in existing technologies, realizes the preparation of high-purity zinc oxide, and is suitable for the application of high-purity zinc oxide.

CN118894549AInactive Publication Date: 2024-11-05ANHUI JINHUA ZINC OXIDE CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411376771.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-30
Publication Date
2024-11-05
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing technologies are insufficient to produce high-purity zinc oxide at the 4N level, which fails to meet the high requirements of semiconductor manufacturing for target purity, performance control, and overall quality consistency.

Method used

The zinc wire is discharged in a mixture of argon and oxygen using an electro-explosion method to form high-purity zinc oxide nanoparticles, which are then collected onto glass fiber filter paper by a powder collector. Process parameters such as voltage, frequency, and wire feeding speed are controlled to ensure purity.

Benefits of technology

The preparation of high-purity zinc oxide with a purity of 4N grade has been achieved. The process is environmentally friendly and easy to control, making it suitable for the application of high-purity zinc oxide.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention belongs to the technical field of zinc oxide materials, and particularly relates to a preparation method of high-purity 4N zinc oxide, high-purity zinc oxide particles are synthesized in mixed gas of argon and oxygen through a zinc wire electric explosion method, after a zinc wire is vaporized, an electric breakdown phenomenon is formed in zinc steam and the mixed gas to induce electric explosion of the zinc wire at the moment, and the zinc oxide particles are obtained. After being overheated, the 4N zinc oxide is expanded in volume to form zinc steam and zinc liquid drops, the zinc steam and the zinc liquid drops interact with a mixed gas medium to form high-purity zinc oxide nanoparticles, and the high-purity 4N zinc oxide is deposited on glass fiber filter paper through a powder collector. The method has the advantages of high energy utilization efficiency, simple process control, no environmental pollution, good product activity and high purity, reaches the 4N level, and is suitable for the use requirements of high-purity zinc oxide.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of zinc oxide materials, in particular to a method for preparing high-purity 4N zinc oxide. Background Art

[0002] High-purity zinc oxide is widely used in the electronics industry, porcelain industry, magnetic materials, automobile tires, medicine, steel, agriculture, feed and other industries. Wang Jiale used high-purity zinc oxide film and applied it to aluminum electrode corrosion protection. With the upgrading of the information industry and the continuous advancement of semiconductor manufacturing technology, the demand for high-purity sputtering targets is increasing, and the requirements for target purity, performance control and overall target quality consistency are getting higher and higher. In order to achieve the desired film properties, factors such as the purity, relative density, grain size and grain orientation of the target must be accurately adjusted. The type and content of impurity elements should be strictly controlled during the preparation of the target. The purity of metal and metal oxide targets is generally required to reach 4N (99.99%) or more. Zhang Jianbin et al. used zinc-containing industrial solid waste to prepare high-purity zinc oxide. The particle size was 2 to 4 μm and the purity reached 99.47%. Cui Wenguang et al. used zinc ash direct method to produce high-purity zinc oxide with a purity of 99.7%. Wang Min used zinc slag as raw material, leached with sulfuric acid, precipitated basic zinc carbonate, and then calcined to produce high-purity zinc oxide. The total recovery rate of zinc is greater than 92%, and the purity can reach more than 99.5%. The existing methods in the past are still far from the 4N level. In order to solve the above problems, those skilled in the art are in urgent need of developing a preparation method of high-purity 4N zinc oxide to meet the existing market demand and performance requirements. Summary of the invention

[0003] In view of the above problems, the present invention aims to provide a method for preparing high-purity 4N zinc oxide.

[0004] A method for preparing high-purity 4N zinc oxide comprises the following steps: The first step is to place and fix the continuous zinc wire on the upper and lower electrodes in the explosion chamber of the electric explosion device; the second step is to seal the explosion chamber, use a vacuum pump to evacuate the explosion chamber to a vacuum of 0.5-0.8Pa, and then fill it with a mixed gas of argon and oxygen, the mixed gas pressure is 1.5-1.8MPa, and the volume flow rate of the mixed gas is 800-1000mL / min; the third step is to charge the energy storage device to the working voltage, start working, and the continuous zinc wire in the wire feeding explosion chamber is continuously and stably discharged; the fourth step is to discharge the gas in the explosion chamber, collect the powder collected by the powder collector on the glass fiber filter paper, and obtain high-purity 4N zinc oxide.

[0005] Furthermore, in the third step, the continuous zinc wire is continuously and stably discharged at an operating voltage of 30 to 35 kV, a charging frequency of 1 to 1.5 Hz, and a wire feeding speed of 5 to 6 cm / s.

[0006] Furthermore, in the first step, the distance between the upper and lower electrodes is 7 to 8 cm.

[0007] Furthermore, the volume ratio of oxygen to argon in the second step mixed gas is 15-20:80-85.

[0008] Furthermore, the purity of oxygen in the second step is ≥99.999%.

[0009] Furthermore, the purity of the argon gas in the second step is ≥99.999%.

[0010] Furthermore, the continuous zinc wire has a diameter of 0.2 to 0.35 mm, and the Zn content of the zinc wire is ≥99.995%, the total impurities are ≤0.005%, Pb≤0.003%, Fe≤0.001%, Cd≤0.002%, Sn≤0.001%, Tin≤0.001%, and Al≤0.001%.

[0011] Beneficial effects of the present invention: The preparation method of high-purity 4N zinc oxide disclosed in the present invention adopts a zinc wire electric explosion method to synthesize high-purity zinc oxide particles in a mixed gas of argon and oxygen, and the zinc wire is vaporized to form an electric breakdown phenomenon in the zinc vapor and the mixed gas to induce the electric explosion zinc wire to produce an electric explosion in an instant, and the volume expands after overheating to form zinc vapor and zinc droplets, which interact with the mixed gas medium to form high-purity zinc oxide nanoparticles, and the high-purity 4N zinc oxide is deposited on glass fiber filter paper through a powder collector. It has high energy utilization efficiency, simple process control, no environmental pollution, good product activity, high purity, reaching 4N level, and is suitable for the use requirements of high-purity zinc oxide. DETAILED DESCRIPTION

[0012] The present invention is described below with specific examples, but is not intended to be limiting of the present invention. Example 1

[0013] Raw materials and equipment: SNB-Ⅳ type electric explosion device; Jinhai nonferrous metal zinc wire with a diameter of 0.25mm, the zinc wire has a Zn content of ≥99.995%, a total impurity content of ≤0.005%, Pb≤0.003%, Fe≤0.001%, Cd≤0.002%, Sn≤0.001%, Tin≤0.001%, Al≤0.001%. Yunfeilong special gas oxygen purity ≥99.999%; Yunfeilong special gas argon purity ≥99.999%.

[0014] A method for preparing high-purity 4N zinc oxide comprises the following steps: The first step is to place and fix the continuous zinc wire on the upper and lower electrodes in the explosion chamber of the electric explosion device, with a distance of 7.5 cm between the upper and lower electrodes; the second step is to seal the explosion chamber, use a vacuum pump to evacuate the explosion chamber to a vacuum of 0.6 Pa, and then fill it with a mixed gas of argon and oxygen, the volume ratio of oxygen and argon in the mixed gas is 18:82, the mixed gas pressure is 1.6 MPa, and the volume flow rate of the mixed gas is 9000 mL / min; the third step is to charge the energy storage device to the working voltage, start working, and feed the continuous zinc wire in the explosion chamber to discharge continuously and stably, the continuous zinc wire discharges continuously and stably, the working voltage is 32 kV, the charging frequency is 1.2 Hz, and the wire feeding speed is 5.5 cm / s; the fourth step is to discharge the gas in the explosion chamber, and collect the powder collected on the glass fiber filter paper by the powder collector to obtain high-purity 4N zinc oxide.

[0015] Products: Zinc oxide purity (on a dry basis) ≥99.99%, metal content (on a Zn basis), w / % ≤ none; hydrochloric acid insoluble matter, w / % ≤0.0005; ignition loss, w / % ≤0.0015; sieve residue (45μm test sieve), w / % ≤0.10; water-soluble matter, w / % ≤0.005; volatile matter at 105℃, w / % ≤0.005; lead (Pb) content, w / % ≤0.0001; copper (Cu) content, w / % ≤0.0002; manganese (Mn) content, w / % ≤0.0001; cadmium (cd) content, w / % ≤0.0002; iron (Fe) content, w / % ≤0.0005; specific surface area 62㎡ / g; oil absorption 13g / 100g. Example 2

[0016] Raw materials and equipment: SNB-Ⅳ type electric explosion device; zinc wire with a diameter of 0.2mm from Hebei Xinxing Metallurgy, the zinc wire has a Zn content of ≥99.995%, a total impurity content of ≤0.005%, Pb≤0.003%, Fe≤0.001%, Cd≤0.002%, Sn≤0.001%, Tin≤0.001%, Al≤0.001%. Yunfeilong special gas oxygen purity ≥99.999%; Yunfeilong special gas argon purity ≥99.999%.

[0017] A method for preparing high-purity 4N zinc oxide comprises the following steps: The first step is to place and fix the continuous zinc wire on the upper and lower electrodes in the explosion chamber of the electric explosion device, with the distance between the upper and lower electrodes being 7 cm; the second step is to seal the explosion chamber, use a vacuum pump to evacuate the explosion chamber to a vacuum of 0.8 Pa, and then fill it with a mixed gas of argon and oxygen, the volume ratio of oxygen and argon in the mixed gas is 20:80, the mixed gas pressure is 1.5 MPa, and the volume flow rate of the mixed gas is 800 mL / min; the third step is to charge the energy storage device to the working voltage, start working, and feed the continuous zinc wire in the explosion chamber to discharge continuously and stably, the continuous zinc wire discharges continuously and stably, the working voltage is 30 kV, the charging frequency is 1 Hz, and the wire feeding speed is 5 cm / s; the fourth step is to discharge the gas in the explosion chamber, and collect the powder collected on the glass fiber filter paper by the powder collector to obtain high-purity 4N zinc oxide.

[0018] Products: Zinc oxide purity (on a dry basis) ≥99.99%, metal content (on a Zn basis), w / % ≤ none; hydrochloric acid insoluble matter, w / % ≤0.0005; ignition loss, w / % ≤0.0015; sieve residue (45μm test sieve), w / % ≤0.10; water-soluble matter, w / % ≤0.005; volatile matter at 105℃, w / % ≤0.005; lead (Pb) content, w / % ≤0.0001; copper (Cu) content, w / % ≤0.0002; manganese (Mn) content, w / % ≤0.0001; cadmium (cd) content, w / % ≤0.0002; iron (Fe) content, w / % ≤0.0005; specific surface area 65㎡ / g; oil absorption 14g / 100g. Example 3

[0019] Raw materials and equipment: SNB-Ⅳ type electric explosion device; zinc wire with a diameter of 0.35mm from Changxing Star Tower, the zinc wire has a Zn content of ≥99.995%, a total impurity content of ≤0.005%, Pb≤0.003%, Fe≤0.001%, Cd≤0.002%, Sn≤0.001%, Tin≤0.001%, Al≤0.001%. Yunfeilong special gas oxygen purity ≥99.999%; Yunfeilong special gas argon purity ≥99.999%.

[0020] A method for preparing high-purity 4N zinc oxide comprises the following steps: The first step is to place and fix the continuous zinc wire on the upper and lower electrodes in the explosion chamber of the electric explosion device, with the distance between the upper and lower electrodes being 8 cm; the second step is to seal the explosion chamber, use a vacuum pump to evacuate the explosion chamber to a vacuum of 0.5 Pa, and then fill it with a mixed gas of argon and oxygen, the volume ratio of oxygen and argon in the mixed gas is 15:85, the mixed gas pressure is 1.8 MPa, and the volume flow rate of the mixed gas is 1000 mL / min; the third step is to charge the energy storage device to the working voltage, start working, and feed the continuous zinc wire in the explosion chamber to discharge continuously and stably, the continuous zinc wire discharges continuously and stably, the working voltage is 35 kV, the charging frequency is 1.5 Hz, and the wire feeding speed is 5 cm / s; the fourth step is to discharge the gas in the explosion chamber, and collect the powder collected on the glass fiber filter paper by the powder collector to obtain high-purity 4N zinc oxide.

[0021] Products: Zinc oxide purity (on a dry basis) ≥99.995%, metal content (on a Zn basis), w / % ≤ none; hydrochloric acid insoluble matter, w / % ≤0.0005; ignition loss, w / % ≤0.0015; sieve residue (45μm test sieve), w / % ≤0.10; water-soluble matter, w / % ≤0.005; volatile matter at 105℃, w / % ≤0.005; lead (Pb) content, w / % ≤0.0001; copper (Cu) content, w / % ≤0.0002; manganese (Mn) content, w / % ≤0.0001; cadmium (cd) content, w / % ≤0.0002; iron (Fe) content, w / % ≤0.0005; specific surface area 68㎡ / g; oil absorption 12g / 100g.

[0022] Note: The sieve residue shall be measured in accordance with the provisions of GB / T5211.18-2015, and the sample shall be 10g. The ignition loss, metal content, and hydrochloric acid insoluble matter shall refer to GB / T 3185-2016; the water-soluble matter shall be measured in accordance with the provisions of GB / T5211.2-2003, and the sample shall be 10g. The volatile matter at 105℃ shall be measured in accordance with the provisions of GB / T5211.3, and the sample shall be 5g. The content of lead (Pb) shall be measured in accordance with the provisions of GB / T9723-2007. The content of copper (Cu) shall be measured in accordance with the provisions of GB / T9723-2007. The content of manganese (Mn) shall be measured in accordance with the provisions of GB / T9723-2007. The content of cadmium (Cd) shall be measured in accordance with the provisions of GB / T9723-2007. The oil absorption is carried out according to the provisions of GB / T5211.15-2014, and the sample is 10g; the determination principle of zinc oxide content (in dry product) is to dissolve the sample in hydrochloric acid, and after neutralization, use EDTA standard titration solution to titrate the zinc oxide content. Reagents and materials-hydrochloric acid solution: high-grade pure, diluted 1+1;-ammonia water: high-grade pure;-ammonia water solution: high-grade pure, diluted 1+1;-ammonium chloride: high-grade pure;-buffer solution (pH=10): weigh 54g ammonium chloride and dissolve it in 200mL water, add 350mL ammonia water and continue to dilute with water to 1000mL;-chrome black T indicator: 5g / L;-ethylenediaminetetraacetic acid disodium (EDTA) standard titration solution: c(EDTA)=0.05mol / L. Instruments and equipment balance: accuracy 0.1mg; conical flask: 500mL; oven: can maintain a temperature of 105℃; electric furnace. Analysis steps: Weigh 0.15g of the sample that has been dried at 105℃ for 1h, accurate to 0.1mg. Place the sample in a 500mL conical flask, add a small amount of water to moisten it, add 3mL of hydrochloric acid solution and heat to dissolve, add water to 200mL, neutralize with ammonia solution to pH about 7-8 (zinc hydroxide precipitation is generated), add 10mL of buffer solution and 5 drops of chrome black T indicator, and titrate with EDTA standard titration solution until the solution changes from grape purple to the end point. The result represents the content of high-purity zinc oxide, calculated according to the formula: w=c×V×0.081408 / m×100%. In the formula: C--the concentration of EDTA standard titration solution, in moles per liter (mol / L); V--the volume of EDTA standard titration solution consumed in titration, in milliliters (mL); m--the mass of the sample, in grams (g); 0.081408--the mass of zinc oxide in grams equivalent to 1.00mL EDTA standard titration solution [c(EDTA)=1.000mol / L].

Claims

1. A method for preparing high-purity 4N zinc oxide, characterized in that: The following steps are involved: The first step is to place and fix the continuous zinc wire on the upper and lower electrodes in the explosion chamber of the electric explosion device; The second step is to seal the explosion chamber, use a vacuum pump to evacuate the explosion chamber to a vacuum of 0.5-0.8Pa, and then fill it with a mixed gas of argon and oxygen. The mixed gas pressure is 1.5-1.8MPa, and the volume flow rate of the mixed gas is 800-1000mL / min; the third step is to charge the energy storage device to the working voltage and start working. The continuous zinc wire in the wire feeding explosion chamber is continuously discharged; the fourth step is to discharge the gas in the explosion chamber, and collect the powder collected by the powder collector on the glass fiber filter paper to obtain high-purity 4N zinc oxide.

2. The method for preparing high-purity 4N zinc oxide according to claim 1, characterized in that: In the third step, the continuous zinc wire is continuously and stably discharged at an operating voltage of 30 to 35 kV, a charging frequency of 1 to 1.5 Hz, and a wire feeding speed of 5 to 6 cm / s.

3. The method for preparing high-purity 4N zinc oxide according to claim 1, characterized in that: In the first step, the distance between the upper and lower electrodes is 7 to 8 cm.

4. The method for preparing high-purity 4N zinc oxide according to claim 1, characterized in that: The volume ratio of oxygen to argon in the second step mixed gas is 15-20:80-85.

5. The method for preparing high-purity 4N zinc oxide according to claim 1, characterized in that: The purity of oxygen in the second step is ≥99.999%.

6. The method for preparing high-purity 4N zinc oxide according to claim 1, characterized in that: The purity of the argon gas in the second step is ≥99.999%.

7. The method for preparing high-purity 4N zinc oxide according to claim 1, characterized in that: The first step is a continuous zinc wire with a diameter of 0.2 to 0.35 mm, wherein the zinc content of the zinc wire is ≥99.995%, the total impurities are ≤0.005%, Pb ≤0.003%, Fe ≤0.001%, Cd ≤0.002%, Sn ≤0.001%, Tin ≤0.001%, and Al ≤0.001%.

Citation Information

Patent Citations

  • Preparation method of nanoscale aluminum powder

    CN112809012A

  • Method of producing nanosized zinc oxide

    RU2696460C1

  • Metal oxide nano powder and manufacturing method of the same

    US20080193760A1

  • Apparatus and method for manufacturing particles

    US20150047467A1