Preparation method of Bi6Fe2Ti3O18 material with three-dimensional ordered macroporous structure

The preparation of Bi6Fe2Ti3O18 material with three-dimensional ordered macroporous structures through the template method solves the problem of traditional materials lacking macroporous structures, achieves the performance improvement of the materials in the fields of catalysis and other fields, and expands its application potential.

CN118894555APending Publication Date: 2024-11-05NINGBO ORIENTAL UNIV OF TECH (TEMPORARY NAME)
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411036889.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

Traditional Bi6Fe2Ti3O18 materials lack macroporous structures, which limits their application potential in the fields of catalysis, adsorption, etc.

Method used

Using the template method, polystyrene microspheres as templates, Bi6Fe2Ti3O18 material with three-dimensional ordered macroporous structures was prepared through multi-step impregnation and high-temperature sintering processes. Specific steps include preparation of styrene emulsion, impregnation of precursor solution and high-temperature sintering treatment, controlling temperature and time to form a stable three-dimensional macropore structure.

Benefits of technology

The three-dimensional ordered macroporous structure Bi6Fe2Ti3O18 material with good mass transfer performance, photocatalytic performance and mechanical stability was successfully prepared, which expanded its application prospects in catalysis and other fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118894555A_ABST
    Figure CN118894555A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of a Bi6Fe2Ti3O18 material with a three-dimensional ordered macroporous structure, and the preparation method specifically comprises the following steps: preparing a template, preparing a precursor solution, dipping the template into the precursor solution to obtain a semi-finished product material, and finally carrying out high-temperature sintering treatment on the semi-finished product material to obtain the Bi6Fe2Ti3O18 material with the three-dimensional ordered macroporous structure. According to the preparation method disclosed by the invention, the Bi6Fe2Ti3O18 material with the three-dimensional ordered macroporous structure is successfully prepared by adopting a template method and utilizing polystyrene microspheres as a template through a multi-step impregnation and high-temperature sintering process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of dielectric materials, and in particular to a three-dimensional ordered macroporous structure of Bi6Fe2Ti3O 18 Material preparation method. Background Art

[0002] Bi6Fe2Ti3O 18 It is an Aurivillius layered perovskite oxide material with excellent dielectric, magnetic and optical properties, and is widely used in various functional materials. Three-dimensionally ordered macroporous structure (3DOM) materials have the following advantages over other structures: Good mass transfer performance: The large pores of the 3DOM structure provide good mass transfer channels, which are conducive to the rapid transmission of reactants and products. This reduces the mass transfer restrictions during the reaction and improves the reaction efficiency. Light scattering and light capture ability: The ordered macroporous structure of the 3DOM material can improve the material's light scattering and capture ability, increase the light absorption efficiency in the photocatalytic reaction, and thus improve the photocatalytic performance. Mechanical stability: The 3DOM structure generally has high mechanical strength and stability, can maintain structural integrity under harsh conditions, and extend the service life of the material. Adjustability: The pore size and pore structure of the 3DOM material can be adjusted through the synthesis method, so that the material performance can be optimized according to the specific application requirements. These advantages make the three-dimensional ordered macroporous structure material show great potential and application prospects in fields such as photocatalysis. However, the traditional Bi6Fe2Ti3O 18 Materials usually lack macroporous structures, which limits their applications in catalysis, adsorption, etc. Therefore, there is an urgent need for a Bi6Fe2Ti3O 18 Material. Summary of the Invention

[0003] The technical problem to be solved by the present invention is to overcome the problem of Bi6Fe2Ti3O 18 The material lacks a macroporous structure. In order to overcome the above defects of the prior art, the present invention provides a Bi6Fe2Ti3O 18 Material preparation method.

[0004] The present invention provides a Bi6Fe2Ti3O 18 The preparation method of the material specifically comprises the following steps:

[0005] S1. Template preparation: Styrene is added to deionized water, and the mixture is heated to the reaction temperature while stirring. An initiator is then added, and the mixture is stirred to obtain an emulsion. The emulsion is then subjected to rotary evaporation to obtain monodisperse polystyrene beads. The polystyrene beads are added to deionized water, and ultrasonic treatment and drying are performed in sequence to obtain a polystyrene colloidal opal template.

[0006] S2. Preparation of precursor solution: Dissolve Bi(CH3COO3)3, (CH3COO3)3 and Ti(OC4H9)4 in a mixed solvent and stir to obtain a precursor solution;

[0007] S3, template impregnation: immersing the polystyrene colloidal opal template obtained in step S1 in the precursor solution obtained in step S2, taking it out after sufficient adsorption and drying it to obtain a semi-finished material;

[0008] S4, the semi-finished material obtained in step S3 is subjected to high temperature sintering to obtain Bi6Fe2Ti3O 18 Material.

[0009] Compared with the existing technology, the present invention successfully prepared Bi6Fe2Ti3O3 with three-dimensional ordered macroporous structure by adopting the template method and using polystyrene microspheres as templates through multi-step impregnation and high-temperature sintering processes. 18 Material.

[0010] In some embodiments, in step S1, the reaction temperature is 60-80° C., the initiator is potassium persulfate, and the mass ratio of styrene to initiator is 1:(0.005-0.01).

[0011] Compared with the prior art, the present invention adopts the method of heating while mixing and stirring, wherein stirring helps to maintain the homogeneity of the reaction mixture, and heating accelerates the polymerization reaction. The initiator is added at a reaction temperature of 60-80°C, and the initiator decomposes under heating conditions to generate free radicals, thereby initiating the polymerization reaction of styrene, that is, styrene molecules are connected to each other under the action of free radicals to form polystyrene chains.

[0012] In some embodiments, the styrene monomer is washed multiple times with a 2M NaOH solution before use to remove the polymerization inhibitor.

[0013] In some embodiments, in step S1, the stirring reaction time is 7-14 hours, and the stirring reaction is carried out under a nitrogen atmosphere.

[0014] Compared with the existing technology, the entire stirring reaction process is carried out under a nitrogen atmosphere. Nitrogen can eliminate oxygen in the air, prevent oxygen from inhibiting the polymerization reaction, and ensure the smooth progress of the polymerization reaction. The stirring reaction lasts for 7-14 hours, which can ensure that the polymerization reaction is fully carried out and a stable emulsion is formed.

[0015] In some embodiments, in step S1, the parameters of the rotary evaporation treatment are as follows: temperature is 55° C., and time is 2 h.

[0016] Compared with the prior art, the present invention subjects the emulsion to rotary evaporation, ie, heating and evaporating under reduced pressure, which can help remove unreacted styrene monomers and concentrate and collect the polystyrene ball emulsion.

[0017] In some embodiments, in step S1, the ultrasonic treatment time is 0.5 h, and the parameters of the drying treatment are as follows: temperature is 40° C., and time is 7 days.

[0018] Compared to existing technologies, the present invention disperses the rotary-evaporated polystyrene bead emulsion in deionized water (to a polystyrene bead mass fraction greater than 60%) in a proportional manner, then ultrasonically treats the particles for 0.5 hours to further disperse and clean them. The particles are then dried at 40°C for 7 days to completely remove moisture, resulting in a dry, stable polystyrene colloidal opal template.

[0019] In some embodiments, in step S2, the molar ratio of Bi(CH3COO3)3, Fe(CH3COO3)2 and Ti(OC4H9)4 is 6:2:3.

[0020] In the present invention, Bi(CH3COO3)3 is used in an excess amount of 10% to compensate for the volatilization of Bi at high temperature.

[0021] In some embodiments, in step S2, the mixed solvent consists of propionic acid and monoethanolamine, and the volume ratio of propionic acid to monoethanolamine is 12:1.

[0022] Compared with the prior art, the present invention adopts a mixed solvent with the above-mentioned volume ratio, wherein propionic acid is an organic acid that can effectively dissolve metal organic compounds, and monoethanolamine can be used as a stabilizer to help form a more stable precursor solution. In the preparation process of the precursor solution, the complete dissolution of the raw materials is crucial, which directly affects the quality of the precursor solution and further affects the purity and structure of the final product. Therefore, the present invention adopts a mixed solvent with the above-mentioned composition.

[0023] In some embodiments, in step S2, the stirring time is 6 hours.

[0024] Compared to the prior art, to ensure that the raw materials are fully dissolved and evenly distributed, the solution needs to be stirred for 6 hours under specific conditions. This stirring time helps to fully contact the raw material molecules with the solvent molecules, accelerates the dissolution process, and also helps to eliminate any precipitation and ensure the uniformity of the solution. Throughout step S2, it is necessary to precisely control the raw material ratio, solvent type, and stirring time to ensure the quality of the precursor solution, thereby improving the synthesis efficiency and performance of the final material.

[0025] In some embodiments, in step S3, the immersion time is 5 hours, and the drying parameters are as follows: temperature is 40° C., time is 2 hours; and the immersion and drying are repeated 3 times.

[0026] Compared with the prior art, the present invention immerses the previously prepared polystyrene colloidal opal template into a precursor solution, wherein the precursor solution contains components such as Bi(CH3COO3)3, Fe(CH3COO3)2 and Ti(OC4H9)4, which will be deposited in the pores of the template to provide the necessary metal ion source for subsequent heat treatment. The immersion time of 5 hours is used to ensure that the precursor molecules have enough time to penetrate into all the pores of the template and achieve sufficient adsorption. The template adsorbed with the precursor is then taken out and placed at 40°C for drying for 2 hours to remove excess solvent on the template and fix the position of the precursor molecules in the pores of the template to prepare for subsequent heat treatment. The present invention adopts a cyclic treatment of repeated immersion and drying, which can gradually accumulate more precursor substances in the pores of the template, which is very critical for forming a final material with a three-dimensional ordered macroporous structure. By controlling the number of cycles, the thickness and porosity of the final material can be adjusted, thereby affecting its physical and chemical properties.

[0027] In some embodiments, in step S4, the high-temperature sintering process specifically includes the following steps:

[0028] S41, control the heating rate to 2°C / min, raise the temperature to 300°C, and keep it warm for 2h;

[0029] S42, control the heating rate to 2°C / min, continue heating to 400°C, and keep warm for 2h;

[0030] S43. Control the heating rate to 2°C / min, continue heating to 550-750°C, and keep warm for 2h.

[0031] High temperature sintering treatment is the preparation of three-dimensional ordered macroporous Bi6Fe2Ti3O 18The final and crucial step in the material process is to control temperature and time to transform the precursor into the target oxide structure and form a stable three-dimensional macroporous structure. Compared with the existing technology, the present invention adopts a three-stage high-temperature sintering process. The role of each stage is to:

[0032] The first stage: The main purpose is to preheat the material and remove any residual organic components, such as incompletely reacted organic solvents or templates. Slow heating helps reduce stress inside the material and prevent crack formation.

[0033] The second stage: further promotes the decomposition of organic matter and begins to activate the metal ions in the precursor, laying the foundation for the subsequent formation of oxides.

[0034] Stage 3: This is the core of the sintering process. At high temperatures, the metal ions undergo an oxidation reaction, forming the target oxide structure. Simultaneously, the high temperature promotes crystal growth, resulting in a stable macroporous structure. The holding time ensures the reaction proceeds fully, resulting in a more uniform and dense material structure.

[0035] Given this, the present invention employs the aforementioned three stages and further defines their parameters. This is because the heating rate, maximum sintering temperature, and holding time are critical parameters throughout the sintering process, directly impacting the structure, porosity, and properties of the final material. For example, an excessively rapid heating rate can lead to internal stress concentrations and structural defects, while insufficient temperatures or short holding times can result in incomplete oxidation reactions, compromising the material's purity and structural integrity. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 This is a scanning electron microscope image of the polystyrene colloidal opal template prepared in Example 1 of the present invention;

[0037] Figure 2 The polystyrene colloidal opal template prepared in Example 2 of the present invention;

[0038] Figure 3 The polystyrene colloidal opal template prepared in Example 3 of the present invention;

[0039] Figure 4 The three-dimensional ordered macroporous structure of Bi6Fe2Ti3O prepared in Example 8 of the present invention 18 X-ray diffraction pattern of the material;

[0040] Figure 5 The three-dimensional ordered macroporous structure of Bi6Fe2Ti3O prepared in Example 8 of the present invention 18 Scanning electron microscope images of the materials;

[0041] Figure 6 The three-dimensional ordered macroporous structure of Bi6Fe2Ti3O prepared in Example 8 of the present invention 18 Transmission electron microscope image and electron diffraction pattern of the material. DETAILED DESCRIPTION

[0042] To make the above-mentioned objects, features, and advantages of the present invention more clearly understood, specific embodiments of the present invention are described in detail below. It should be noted that the following embodiments are only intended to illustrate the implementation methods and typical parameters of the present invention, and are not intended to limit the parameter ranges described in the present invention. Reasonable variations derived therefrom are still within the scope of protection of the claims of the present invention.

[0043] It should be noted that the endpoints of the ranges and any values ​​disclosed herein are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoints of each range, the endpoints of each range and individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, and these numerical ranges should be considered to be specifically disclosed herein.

[0044] Unless otherwise defined, all terms, symbols and other scientific terms used herein are intended to have the same meaning as commonly understood by those skilled in the art to which the present invention belongs. In some cases, terms with conventional meanings are defined herein for the purpose of clarification or ease of reference, and such definitions herein should not be construed as indicating significant differences from conventional understandings in the art. The technical methods described or cited herein are generally well understood by those skilled in the art and are adopted by conventional methods. Unless otherwise stated, the use of commercially available kits, reagents and instruments was carried out in accordance with the protocols and parameters given by the manufacturers.

[0045] The technical effects of the present invention are described below with reference to specific embodiments.

[0046] Example 1

[0047] The present embodiment provides a polystyrene colloidal crystal opal template, which is prepared by the following preparation method: 20 mL of styrene and 400 mL of deionized water are added to a 500 mL three-necked flask, mixed and stirred until the temperature rises to 60° C., 0.3 g of potassium persulfate initiator is quickly added, and the reaction is stirred for 7 hours. The entire reaction is carried out under a nitrogen atmosphere. The white emulsion obtained after the reaction is subjected to rotary evaporation (55° C., 2 hours) to remove unreacted styrene monomer to obtain monodisperse polystyrene beads. The monodisperse polystyrene beads are poured into a 1 L beaker, and deionized water is added to a volume of 500 mL. After ultrasonic treatment for 0.5 hours, the mixture is allowed to stand in a 40° C. oven for 7 days to obtain a polystyrene colloidal crystal opal template.

[0048] Example 2

[0049] This embodiment provides a polystyrene colloidal opal template. The only difference from Example 1 is that the amount of styrene added in this embodiment is 30 mL. The rest is the same as Example 1 and will not be repeated here.

[0050] Example 3

[0051] This embodiment provides a polystyrene colloidal opal template. The only difference from Example 1 is that the amount of styrene added in this embodiment is 40 mL. The rest is the same as Example 1 and will not be repeated here.

[0052] Example 5

[0053] This embodiment provides a polystyrene colloidal opal template, which is prepared by the following preparation method: 20 mL of styrene and 400 mL of deionized water are added to a 500 mL three-necked flask, mixed and stirred until the temperature rises to 65°C, 0.3 g of potassium persulfate initiator is quickly added, and the reaction is stirred for 8 hours. The entire reaction is carried out under a nitrogen atmosphere. The white emulsion obtained after the reaction is rotary evaporated (55°C, 2 hours) to remove unreacted styrene monomer to obtain monodisperse polystyrene beads. The monodisperse polystyrene beads are poured into a 1 L beaker, and deionized water is added to the volume of 500 mL. After ultrasonic treatment for 0.5 hours, the mixture is allowed to stand in a 40°C oven for 7 days to obtain a polystyrene colloidal opal template.

[0054] Example 6

[0055] This embodiment provides a polystyrene colloidal opal template, which is prepared by the following preparation method: 20 mL of styrene and 400 mL of deionized water are added to a 500 mL three-necked flask, mixed and stirred until the temperature rises to 75°C, 0.3 g of potassium persulfate initiator is quickly added, and the reaction is stirred for 12 hours. The entire reaction is carried out under a nitrogen atmosphere. The white emulsion obtained after the reaction is rotary evaporated (55°C, 2 hours) to remove unreacted styrene monomer to obtain monodisperse polystyrene beads. The monodisperse polystyrene beads are poured into a 1 L beaker, and deionized water is added to the volume to 500 mL. After ultrasonic treatment for 0.5 hours, the mixture is allowed to stand in a 40°C oven for 7 days to obtain a polystyrene colloidal opal template.

[0056] Example 7

[0057] This embodiment provides a polystyrene colloidal opal template, which is prepared by the following preparation method: 20 mL of styrene and 400 mL of deionized water are added to a 500 mL three-necked flask, mixed and stirred until the temperature rises to 80°C, 0.3 g of potassium persulfate initiator is quickly added, and the reaction is stirred for 14 hours. The entire reaction is carried out under a nitrogen atmosphere. The white emulsion obtained after the reaction is rotary evaporated (55°C, 2 hours) to remove unreacted styrene monomer to obtain monodisperse polystyrene beads. The monodisperse polystyrene beads are poured into a 1 L beaker, and deionized water is added to the volume of 500 mL. After ultrasonic treatment for 0.5 hours, the mixture is allowed to stand in a 40°C oven for 7 days to obtain a polystyrene colloidal opal template.

[0058] Example 8

[0059] This embodiment provides a three-dimensional ordered macroporous structure of Bi6Fe2Ti3O 18 The material was prepared by the following preparation method:

[0060] S1. Preparation of precursor solution: Calculate the required Bi(CH3COO3)3, (CH3COO3)3 and Ti(OC4H9)4 for 10 mL of 0.1 M precursor according to the stoichiometric ratio and dissolve them in a mixed solution of propionic acid and monoethanolamine (mixing volume ratio: 12:1). Bi(CH3COO3)3 needs to be in excess of 10% to compensate for the volatilization of Bi at high temperature. Stir continuously for 6 h to obtain a uniform precursor solution.

[0061] S2. Template impregnation: The polystyrene colloidal opal template prepared in Example 1 was impregnated in the precursor solution. After sufficient adsorption, it was taken out and dried. The impregnation (5 h) and drying (40° C., 2 h) were repeated three times to ensure that the precursor solution fully filled the pores of the template.

[0062] S3. High temperature sintering: The impregnated template is sintered at high temperature in air atmosphere. During the sintering process, the template decomposes, leaving behind a three-dimensional ordered macroporous structure of Bi6Fe2Ti3O 18 Materials, high temperature sintering treatment specifically includes the following steps:

[0063] S31, control the heating rate to 2°C / min, raise the temperature to 300°C, and keep it warm for 2h;

[0064] S32, control the heating rate to 2°C / min, continue heating to 400°C, and keep warm for 2h;

[0065] S33. Control the heating rate to 2°C / min, continue heating to 550-750°C, and keep warm for 2h.

[0066] Example 9

[0067] This embodiment provides a three-dimensional ordered macroporous structure of Bi6Fe2Ti3O 18 The material is different from that of Example 8 only in that the polystyrene colloidal opal template prepared in Example 2 is used in this example. The rest is the same as that of Example 8 and will not be repeated here.

[0068] Example 10

[0069] This embodiment provides a three-dimensional ordered macroporous structure of Bi6Fe2Ti3O 18 The material is different from that of Example 8 only in that the polystyrene colloidal opal template prepared in Example 3 is used in this example. The rest is the same as that of Example 8 and will not be described again here.

[0070] Comparative Example 1

[0071] This comparative example provides a three-dimensional ordered macroporous structure of Bi6Fe2Ti3O 18 The material is different from Example 8 only in that the high-temperature sintering step in step S3 of this comparative example is only: controlling the heating rate to 2°C / min, heating to 550-750°C, and keeping warm for 2h. The rest is the same as Example 8 and will not be repeated here.

[0072] Comparative Example 2

[0073] This comparative example provides a three-dimensional ordered macroporous structure of Bi6Fe2Ti3O 18 The only difference between the materials and Example 8 is that the high-temperature sintering process in step S3 of this comparative example is:

[0074] S31, control the heating rate to 2°C / min, raise the temperature to 300°C, and keep it warm for 2h;

[0075] S32, control the heating rate to 2°C / min, continue heating to 550-750°C, and keep warm for 2h; the rest is the same as in Example 8 and will not be repeated here.

[0076] Comparative Example 3

[0077] This comparative example provides a three-dimensional ordered macroporous structure of Bi6Fe2Ti3O 18 The only difference between the materials and Example 8 is that the high-temperature sintering process in step S3 of this comparative example is:

[0078] S31, control the heating rate to 2°C / min, raise the temperature to 400°C, and keep it warm for 2h;

[0079] S32, control the heating rate to 2°C / min, continue heating to 550-750°C, and keep warm for 2h; the rest is the same as in Example 8 and will not be repeated here.

[0080] Comparative Example 4

[0081] This comparative example provides a three-dimensional ordered macroporous structure of Bi6Fe2Ti3O 18 The only difference between the materials and Example 8 is that the high-temperature sintering process in step S3 of this comparative example is:

[0082] S31, control the heating rate to 5-10°C / min, heat to 550-750°C, and keep warm for 2h; other steps are the same as those in Example 8 and will not be repeated here.

[0083] The inventors tested the performance of the products prepared in Examples 1-3 and Example 8, and the test results are as follows: Figures 1-6 As shown, Figure 1 This is a scanning electron microscope image of the polystyrene colloidal opal template prepared in Example 1 of the present invention. Figure 2 This is a scanning electron microscope image of the polystyrene colloidal opal template prepared in Example 2 of the present invention; Figure 3 This is a scanning electron microscope image of the polystyrene colloidal opal template prepared in Example 3 of the present invention; Figure 4 The three-dimensional ordered macroporous structure of Bi6Fe2Ti3O prepared in Example 8 of the present invention 18 X-ray diffraction pattern of the material; Figure 5 The three-dimensional ordered macroporous structure of Bi6Fe2Ti3O prepared in Example 8 of the present invention 18 Scanning electron microscope images of the materials; Figure 6 The three-dimensional ordered macroporous structure of Bi6Fe2Ti3O prepared in Example 8 of the present invention 18 Transmission electron microscope image and electron diffraction pattern of the material.

[0084] from Figure 1-Figure 3 It can be seen that different styrene dosages can adjust the size of the polystyrene beads in the template. The more styrene dosage is used, the larger the size of the polystyrene beads obtained. Figure 4 The obtained three-dimensional ordered macroporous structure Bi6Fe2Ti3O 18 The material has good crystallinity, and the peak position is consistent with that of the standard card. Figure 5 It shows that the prepared Bi6Fe2Ti3O 18 The material has a good hierarchical pore structure. Figure 6 It shows that the prepared Bi6Fe2Ti3O 18 The material has a good hierarchical pore structure and a single crystal structure with a good degree of crystallization.

[0085] Furthermore, the invention observed the materials obtained in Comparative Examples 1 to 4. In Comparative Example 1, due to the lack of preheating and organic matter removal procedures, the sintering process of the material was accompanied by the template removal process, so the obtained Bi6Fe2Ti3O18 The material will have cracks and structural collapse. In Comparative Example 2, due to the lack of organic matter removal process, the sintering process of the material is accompanied by the template removal process, so the obtained Bi6Fe2Ti3O 18 The material will experience structural collapse and cannot obtain a three-dimensional ordered macroporous structure. In Comparative Example 3, due to the lack of preheating procedure, the obtained Bi6Fe2Ti3O 18 The material will have cracks and other phenomena, and it is impossible to obtain a good three-dimensional ordered macroporous structure. The Bi6Fe2Ti3O 18 The material will not be able to obtain a three-dimensional ordered macroporous structure

[0086] Although the present disclosure is disclosed as above, the protection scope of the present disclosure is not limited thereto. Those skilled in the art can make various changes and modifications without departing from the spirit and scope of the present disclosure, and these changes and modifications will fall within the protection scope of the present invention.

Claims

1. A three-dimensional ordered macroporous structure of Bi6Fe2Ti3O 18 The method for preparing the material is characterized in that: The preparation method specifically comprises the following steps: S1. Template preparation: adding styrene to deionized water, heating to the reaction temperature while mixing and stirring, adding an initiator, and obtaining an emulsion after stirring and reacting, and then subjecting the emulsion to rotary evaporation to obtain monodisperse polystyrene beads, adding the polystyrene beads to deionized water, and sequentially subjecting the mixture to ultrasonic treatment and drying to obtain a polystyrene colloidal opal template; S2. Preparation of precursor solution: Dissolve Bi(CH3COO3)3, Fe(CH3COO3)2 and Ti(OC4H9)4 in a mixed solvent, and obtain a precursor solution after stirring; S3, template impregnation: the polystyrene colloidal opal template prepared in step S1 is impregnated in the precursor solution prepared in step S2, and after sufficient adsorption, it is taken out and dried to obtain a semi-finished material; S4, the semi-finished material obtained in step S3 is subjected to high temperature sintering to obtain Bi6Fe2Ti3O 18 Material.

2. The three-dimensional ordered macroporous Bi6Fe2Ti3O 18 The method for preparing the material is characterized in that: In the step S1, the reaction temperature is 60-80° C., the initiator is potassium persulfate, and the mass ratio of styrene to the initiator is 1:(0.005-0.01).

3. The three-dimensional ordered macroporous Bi6Fe2Ti3O 18 The method for preparing the material is characterized in that: In the step S1, the stirring reaction time is 7-14 hours, and the stirring reaction is carried out under a nitrogen atmosphere.

4. The three-dimensional ordered macroporous Bi6Fe2Ti3O according to claim 1 18 The method for preparing the material is characterized in that: In step S1, the parameters of the rotary evaporation treatment are as follows: temperature is 55° C., and time is 2 h.

5. The three-dimensional ordered macroporous Bi6Fe2Ti3O according to claim 1 18 The method for preparing the material is characterized in that: In step S1, the ultrasonic treatment time is 0.5 h, and the parameters of the drying treatment are as follows: temperature is 40° C., and time is 7 days.

6. The three-dimensional ordered macroporous Bi6Fe2Ti3O3 according to claim 1 18 The method for preparing the material is characterized in that: In step S2, the molar ratio of Bi(CH3COO3)3, Fe(CH3COO3)2 and Ti(OC4H9)4 is 6:2:

3.

7. The three-dimensional ordered macroporous Bi6Fe2Ti3O3 according to claim 1 18 The method for preparing the material is characterized in that: In step S2, the mixed solvent consists of propionic acid and monoethanolamine, and the volume ratio of propionic acid to monoethanolamine is 12:

1.

8. The three-dimensional ordered macroporous Bi6Fe2Ti3O according to claim 1 18 The method for preparing the material is characterized in that: In step S2, the stirring time is 6 hours.

9. The three-dimensional ordered macroporous Bi6Fe2Ti3O according to claim 1 18 The method for preparing the material is characterized in that: In step S3, the immersion time is 5 hours, and the drying parameters are as follows: temperature is 40° C., time is 2 hours; the immersion and drying are repeated 3 times.

10. The three-dimensional ordered macroporous Bi6Fe2Ti3O according to claim 1 18 The method for preparing the material is characterized in that: In step S4, the high temperature sintering process specifically includes the following steps: S41, control the heating rate to 2°C / min, raise the temperature to 300°C, and keep it warm for 2h; S42, control the heating rate to 2°C / min, continue heating to 400°C, and keep warm for 2h; S43. Control the heating rate to 2°C / min, continue heating to 550-750°C, and keep warm for 2h.