Method for preparing foamed ceramic filter by using waste chrome corundum
By mixing waste chromium corundum with oxide and calcining, and combining special solvents and stirring methods to prepare foam ceramic filters, the problem of poor use of waste chromium corundum in foam ceramics is solved, and high-efficiency filtration and long-life foam ceramics are achieved Filter.
Patent Information
- Application Number
- CN202411140949.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-08-20
AI Technical Summary
Waste chromium corundum contains Cr2O3 and cannot be used directly to prepare foam ceramics, resulting in poor filtration effect and short service life, so it cannot be effectively used.
The waste chromium corundum is grinded and graded, mixed with cerium oxide, lanthanum oxide, zirconia, and alumina respectively, and calcined multiple times to form a stable complex oxide. Combining glycerin and solvent oil as solvents, the slurry is prepared by a special stirring method. The material is sintered to prepare a foam ceramic filter using soft polyurethane foam as a carrier.
It has achieved a foam ceramic filter with good filtration effect and long service life under high doping, which solved the problems of chromium pollution and short service life, and improved the filtration effect and service life.
Smart Images

Figure BDA0005000769320000091 
Figure BDA0005000769320000101
Abstract
Description
Technical Field
[0001] The present application relates to the field of solid waste utilization, and in particular to a method for preparing a foam ceramic filter using waste chromium corundum. Background Art
[0002] Waste chrome corundum is widely found in many waste refractory materials. The main mineral composition of its raw material chrome corundum is α-Al2O3-Cr2O3 solid solution. Fully recycling the alumina in it is of great significance for digesting solid waste and reducing costs.
[0003] The main raw material of foam ceramics is alumina, so recycling waste chromium corundum to prepare foam ceramics is one of the ways to reuse it as a resource.
[0004] However, waste chromium corundum cannot be directly used to prepare foam ceramics because it contains Cr2O3. In order to avoid the introduction of chromium impurity elements and ensure the filtering effect, only a small amount can be added, which can easily lead to problems such as poor filtering effect and short service life.
[0005] In view of this, it is necessary to study a method to solve the above problems and realize the effective utilization of waste chrome corundum. Summary of the invention
[0006] The purpose of the present application is to provide a method for preparing a foam ceramic filter using waste chromium corundum to solve the above problems.
[0007] To achieve the above objectives, this application adopts the following technical solutions:
[0008] A method for preparing a foam ceramic filter using waste chromium corundum, comprising:
[0009] Grinding the waste chrome corundum and sieving to obtain fine particles less than 0.15 mm, medium particles of 0.15-0.3 mm, and coarse particles greater than 0.3 mm and less than or equal to 1 mm;
[0010] The fine particles are mixed with cerium oxide and lanthanum oxide of the same particle size range to obtain a first mixture, the medium particles are mixed with zirconium oxide of the same particle size range to obtain a second mixture, and the coarse particles are mixed with aluminum oxide of the same particle size range to obtain a third mixture;
[0011] The first mixture, the second mixture, and the third mixture are calcined at 1000-1300° C. for 2-4 times respectively, and then ground and mixed to obtain a fourth mixture;
[0012] The fourth mixture is mixed with glycerin and solvent oil, and stirred with a double planetary stirrer to obtain a slurry, and soft polyurethane foam is used as a carrier to impregnate the slurry, and then extruded and dried to obtain a blank;
[0013] The blank is sintered and cooled to obtain a foam ceramic filter.
[0014] Fine particles, medium particles and coarse particles have different requirements for chromium solidification. Fine particles are more likely to dissipate chromium into the filtered metal solution during the subsequent preparation process, followed by medium particles and the lowest for coarse particles. Therefore, fine particles are mixed with cerium oxide and lanthanum oxide for calcination, medium particles are calcined with zirconium oxide, and coarse particles are calcined with aluminum oxide. Lanthanum oxide and cerium oxide are the most stable for the solidification of chromium by the complex oxides formed between chromium and chromium oxide, followed by zirconium oxide. Alumina is the most common filter raw material and is combined with coarse particles. The purpose of multiple calcinations is to further strengthen the above effects.
[0015] Optionally, the calcination temperature may be 1000°C, 1100°C, 1200°C, 1300°C or any value between 1000-1300°C, and the calcination times may be any value among 2, 3 or 4 times.
[0016] Preferably, the mass ratio of the fine particles, the cerium oxide and the lanthanum oxide is 1:(0.01-0.05):(0.01-0.05), the mass ratio of the medium particles to the zirconium oxide is 1:(0.1-0.5), and the mass ratio of the coarse particles to the aluminum oxide is 1:(0.1-0.5).
[0017] Optionally, the mass ratio of the fine particles, the cerium oxide and the lanthanum oxide can be 1:0.01:0.01, 1:0.01:0.03, 1:0.01:0.05, 1:0.03:0.01, 1:0.03:0.03, 1:0.03:0.05, 1:0.05:0.01, 1:0.05:0.03, 1:0.05:0.05 or 1:(0.01-0.05):(0 .01-0.05), the mass ratio of the medium particles to the zirconium oxide can be 1:0.1, 1:0.2, 1:0.3, 1:0.4, 1:0.5 or any value between 1:(0.1-0.5), and the mass ratio of the coarse particles to the aluminum oxide can be 1:0.1, 1:0.2, 1:0.3, 1:0.4, 1:0.5 or any value between 1:(0.1-0.5).
[0018] Preferably, the mass ratio of the first mixture, the second mixture and the third mixture is 1:(1-3):(1-3).
[0019] Optionally, the mass ratio of the first mixture, the second mixture, and the third mixture can be 1:1:1, 1:2:1, 1:3:1, 1:2:1, 1:2:2, 1:2:3, 1:3:1, 1:3:2, 1:3:3 or any value between 1:(1-3):(1-3).
[0020] Preferably, the calcination time is independently 1-5 h.
[0021] Optionally, the calcination time can be independently 1 h, 2 h, 3 h, 4 h, 5 h or any value between 1 and 5 h.
[0022] Preferably, the particle size of the fourth mixture is less than 200 mesh.
[0023] Preferably, the volume ratio of the glycerol to the solvent oil is 1:(1-5).
[0024] Glycerin and mineral spirits are combined to form a solvent system having a viscosity suitable for mixing the three calcined particles in the fourth mixture.
[0025] Optionally, the volume ratio of the glycerol to the solvent oil can be 1:1, 1:2, 1:3, 1:4, 1:5 or any value between 1:(1-5).
[0026] Preferably, the solid content of the slurry is 20-40%.
[0027] Optionally, the solid content of the slurry may be 20%, 25%, 30%, 35%, 40% or any value between 20-40%.
[0028] Preferably, the stirring comprises:
[0029] Stir at an orbital speed of 500-1000 rpm and an autorotation speed of 1500-2000 rpm for 1-2 hours, then let it stand for 12-24 hours, and then stir at an orbital speed of 100-300 rpm and an autorotation speed of 500-1000 rpm for 12-24 hours.
[0030] First, mix them evenly with high-speed stirring and then let them stand. In the presence of glycerin and solvent oil, the particles will not be separated into layers when left standing like in water, but the uneven parts will be separated from the uniform parts. Then, stir them for a long time at a lower speed to form a uniform slurry, avoiding local defects during the subsequent impregnation and sintering processes.
[0031] Optionally, the stirring first performed, the revolution speed can be 500 rpm, 600 rpm, 700 rpm, 800 rpm, 900 rpm, 1000 rpm or any value between 500-1000 rpm, the rotation speed can be 1500 rpm, 1600 rpm, 1700 rpm, 1800 rpm, 1900 rpm, 2000 rpm or any value between 1500-2000 rpm, the time can be 1h, 1.5h, 2h or any value between 1-2h; The standing time can be 12h, 18h, 24h or any value between 12-24h; the stirring is then carried out, the revolution speed can be 100 rpm, 200 rpm, 300 rpm or any value between 100-300 rpm, the rotation speed can be 500 rpm, 600 rpm, 700 rpm, 800 rpm, 900 rpm, 1000 rpm or any value between 500-1000 rpm, and the time can be 12h, 18h, 24h or any value between 12-24h.
[0032] Preferably, the maximum sintering temperature is 1200-1400° C. and the sintering time is 6-8 hours.
[0033] Preferably, the flexible polyurethane foam has a pore size of 10-30 PPI.
[0034] Compared with the prior art, the beneficial effects of this application include:
[0035] The present application provides a method for preparing a foam ceramic filter using waste chrome corundum, which comprises first grinding the waste chrome corundum and then grading it, and then mixing it with cerium oxide, lanthanum oxide, zirconium oxide and aluminum oxide according to different particle sizes, and then calcining each of them multiple times, so as to solve the problem of uneven distribution of complex oxides caused by uneven mixing with various oxides during the use of the waste chrome corundum, and further solve the problem of chromium pollution during the use of the foam ceramic filter; change the traditional method of using water as a solvent to prepare the slurry, use glycerol and solvent oil as solvents, and further solve the many defects caused by uneven mixing of the slurry due to different densities of various materials in the fourth mixture through a special stirring method, so as to achieve a foam ceramic filter with good filtering effect and long service life even with a high doping amount of the waste chrome corundum. DETAILED DESCRIPTION
[0036] The embodiments of the present application will be described in detail below in conjunction with specific examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. If specific conditions are not specified in the examples, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0037] Example 1
[0038] This embodiment provides a method for preparing a foam ceramic filter using waste chromium corundum, which specifically includes the following steps:
[0039] The waste chrome corundum is ground and sieved to obtain fine particles less than 0.15 mm, medium particles of 0.15-0.3 mm, and coarse particles greater than 0.3 mm and less than or equal to 1 mm;
[0040] The fine particles are mixed with cerium oxide and lanthanum oxide of the same particle size range to obtain a first mixture, the medium particles are mixed with zirconium oxide of the same particle size range to obtain a second mixture, and the coarse particles are mixed with aluminum oxide of the same particle size range to obtain a third mixture; the mass ratio of the fine particles, cerium oxide and lanthanum oxide is 1:0.01:0.02, the mass ratio of the medium particles to zirconium oxide is 1:0.1, and the mass ratio of the coarse particles to aluminum oxide is 1:0.1;
[0041] The first mixture, the second mixture and the third mixture were calcined at 1000°C for 4 times, each calcination time was 4 hours; after each calcination, they were naturally cooled to room temperature; then ground and mixed to obtain a fourth mixture with a particle size of less than 200 mesh; the mass ratio of the first mixture, the second mixture and the third mixture was 1:1:1;
[0042] The fourth mixture is mixed with glycerin and No. 70 solvent oil, and stirred with a double planetary stirrer to obtain a slurry with a solid content of 20%; the stirring comprises: stirring at a revolution speed of 500 rpm and a rotation speed of 1500 rpm for 2 hours, then standing for 24 hours, and then stirring at a revolution speed of 100 rpm and a rotation speed of 500 rpm for 24 hours;
[0043] The slurry is impregnated into a soft polyurethane foam as a carrier, and then the excess slurry is squeezed out and dried at 120° C. to obtain a blank; the soft polyurethane foam has a pore size of 10 PPI;
[0044] The blank is sintered and cooled to obtain a foam ceramic filter; the sintering is performed with a uniform temperature increase, the highest sintering temperature is 1200° C., and the sintering time is 8 hours.
[0045] Example 2
[0046] This embodiment provides a method for preparing a foam ceramic filter using waste chromium corundum, which specifically includes the following steps:
[0047] The waste chrome corundum is ground and sieved to obtain fine particles less than 0.15 mm, medium particles of 0.15-0.3 mm, and coarse particles greater than 0.3 mm and less than or equal to 1 mm;
[0048] The fine particles are mixed with cerium oxide and lanthanum oxide of the same particle size range to obtain a first mixture, the medium particles are mixed with zirconium oxide of the same particle size range to obtain a second mixture, and the coarse particles are mixed with aluminum oxide of the same particle size range to obtain a third mixture; the mass ratio of the fine particles, cerium oxide and lanthanum oxide is 1:0.05:0.01, the mass ratio of the medium particles to zirconium oxide is 1:0.5, and the mass ratio of the coarse particles to aluminum oxide is 1:0.3;
[0049] The first mixture, the second mixture and the third mixture are calcined twice at 1300°C for 1 hour each; the mixtures are naturally cooled to room temperature after each calcination; and then ground and mixed to obtain a fourth mixture with a particle size of less than 200 mesh; the mass ratio of the first mixture, the second mixture and the third mixture is 1:2:3;
[0050] The fourth mixture is mixed with glycerin and No. 70 solvent oil, and stirred with a double planetary stirrer to obtain a slurry with a solid content of 30%; the stirring includes: stirring at a revolution speed of 1000 rpm and a rotation speed of 2000 rpm for 1 hour, then standing for 12 hours, and then stirring at a revolution speed of 300 rpm and a rotation speed of 1000 rpm for 12 hours; the volume ratio of glycerin to solvent oil is 1:5;
[0051] The slurry is impregnated into a soft polyurethane foam as a carrier, and then the excess slurry is squeezed out and dried at 120° C. to obtain a blank; the soft polyurethane foam has a pore size of 20 PPI;
[0052] The blank is sintered and cooled to obtain a foam ceramic filter; the sintering is performed with a uniform temperature increase, the highest sintering temperature is 1400° C., and the sintering time is 6 hours.
[0053] Example 3
[0054] This embodiment provides a method for preparing a foam ceramic filter using waste chromium corundum, which specifically includes the following steps:
[0055] The waste chrome corundum is ground and sieved to obtain fine particles less than 0.15 mm, medium particles of 0.15-0.3 mm, and coarse particles greater than 0.3 mm and less than or equal to 1 mm;
[0056] The fine particles are mixed with cerium oxide and lanthanum oxide of the same particle size range to obtain a first mixture, the medium particles are mixed with zirconium oxide of the same particle size range to obtain a second mixture, and the coarse particles are mixed with aluminum oxide of the same particle size range to obtain a third mixture; the mass ratio of the fine particles, cerium oxide and lanthanum oxide is 1:(0.03):0.05, the mass ratio of the medium particles to zirconium oxide is 1:0.4, and the mass ratio of the coarse particles to aluminum oxide is 1:0.5;
[0057] The first mixture, the second mixture and the third mixture were calcined at 1200°C for 3 times, and the calcination time was 2 hours respectively; after each calcination, they were naturally cooled to room temperature; then ground and mixed to obtain a fourth mixture with a particle size of less than 200 mesh; the mass ratio of the first mixture, the second mixture and the third mixture was 1:3:2;
[0058] The fourth mixture is mixed with glycerin and No. 70 solvent oil, and stirred with a double planetary stirrer to obtain a slurry with a solid content of 40%; the stirring comprises: stirring at a revolution speed of 800 rpm and a rotation speed of 1600 rpm for 2 hours, then standing for 15 hours, and then stirring at a revolution speed of 200 rpm and a rotation speed of 700 rpm for 20 hours;
[0059] The slurry is impregnated into a soft polyurethane foam as a carrier, and then the excess slurry is squeezed out and dried at 120° C. to obtain a blank; the volume ratio of glycerol to solvent oil is 1:3; and the soft polyurethane foam has a pore size of 30 PPI;
[0060] The blank is sintered and cooled to obtain a foam ceramic filter; the sintering is performed with a uniform temperature increase, the highest sintering temperature is 1300° C., and the sintering time is 7 hours.
[0061] Example 4
[0062] This embodiment provides a method for preparing a foam ceramic filter using waste chromium corundum, which specifically includes the following steps:
[0063] The waste chrome corundum is ground and sieved to obtain fine particles less than 0.15 mm, medium particles of 0.15-0.3 mm, and coarse particles greater than 0.3 mm and less than or equal to 1 mm;
[0064] The fine particles are mixed with cerium oxide and lanthanum oxide of the same particle size range to obtain a first mixture, the medium particles are mixed with zirconium oxide of the same particle size range to obtain a second mixture, and the coarse particles are mixed with aluminum oxide of the same particle size range to obtain a third mixture; the mass ratio of the fine particles, cerium oxide and lanthanum oxide is 1:0.03:0.03, the mass ratio of the medium particles to zirconium oxide is 1:0.35, and the mass ratio of the coarse particles to aluminum oxide is 1:0.25;
[0065] The first mixture, the second mixture and the third mixture were calcined 4 times at 1200°C, and the calcination time was 3 hours respectively; after each calcination, they were naturally cooled to room temperature; then ground and mixed to obtain a fourth mixture with a particle size of less than 200 mesh; the mass ratio of the first mixture, the second mixture and the third mixture was 1:2:2;
[0066] The fourth mixture is mixed with glycerin and No. 70 solvent oil, and stirred with a double planetary stirrer to obtain a slurry with a solid content of 40%; the stirring comprises: stirring at a revolution speed of 800 rpm and a rotation speed of 1800 rpm for 2 hours, then standing for 24 hours, and then stirring at a revolution speed of 200 rpm and a rotation speed of 800 rpm for 24 hours;
[0067] The slurry is impregnated into a soft polyurethane foam as a carrier, and then the excess slurry is squeezed out and dried at 120° C. to obtain a blank; the volume ratio of glycerol to solvent oil is 1:3; and the soft polyurethane foam has a pore size of 20 PPI;
[0068] The blank is sintered and cooled to obtain a foam ceramic filter; the sintering is performed with a uniform temperature increase, the highest sintering temperature is 1300° C., and the sintering time is 6 hours.
[0069] Comparative Example 1
[0070] Different from Example 4, the waste chromium corundum is not classified after grinding, but is directly mixed with cerium oxide, lanthanum oxide, zirconium oxide and aluminum oxide, and calcined four times at 1200° C., with each calcination time being 3 hours.
[0071] Comparative Example 2
[0072] Different from Example 4, the waste chromium corundum is not classified after grinding, but is mixed with cerium oxide, lanthanum oxide, zirconium oxide and aluminum oxide in the same mass ratio as in Example 4 to obtain a first mixture, a second mixture and a third mixture.
[0073] Comparative Example 3
[0074] The difference from Example 4 is that calcination is performed only once.
[0075] Comparative Example 4
[0076] The difference from Example 4 is that equal amounts of water are used to replace glycerol and mineral spirits.
[0077] Comparative Example 5
[0078] Different from Example 4, a conventional stirring method was adopted, with stirring at 1600 rpm for 26 h.
[0079] Comparative Example 6
[0080] The difference from Example 4 is that cerium oxide, lanthanum oxide and zirconium oxide are not used, but are replaced by an equal amount of aluminum oxide.
[0081] The foam ceramic filters obtained in the embodiment and the comparative example were prepared into a size of 30*30*20mm, and were tested using aluminum water at a temperature of 700-750°C, with each piece filtering 20kg of aluminum water each time. The aluminum water after one filtration was tested for the detection of chromium elements, the maximum number of uses (without considering the filtration effect, only observing whether cracks appeared; the data is the average value of multiple tests, rounded off), and the percentage increase in the tensile strength and elongation of the aluminum water after one filtration. The test results are as follows:
[0082] Table 1 Test results
[0083]
[0084]
[0085] As shown in Table 1 above, the ground waste chrome corundum is graded and then mixed with the corresponding cerium oxide, lanthanum oxide, zirconium oxide and aluminum oxide respectively, which plays an important role in effectively improving the filtering effect, inhibiting the pollution of chromium element to aluminum liquid during use, and improving the service life. Multiple calcinations can improve the service life and filtering effect of the filter to a certain extent; glycerol and solvent oil are combined to form a solvent system with a viscosity suitable for the mixture of the three calcined particles in the fourth mixture, which helps to improve the filtering effect and has a certain effect on the service life of the filter. The special stirring method can avoid local defects in the subsequent impregnation and sintering process, and can greatly improve the service life. The use of cerium oxide, lanthanum oxide and zirconium oxide is one of the basic factors for obtaining the filtering effect, inhibiting the pollution of chromium element to aluminum liquid during use, and improving the service life.
[0086] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit it. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present application.
[0087] In addition, those skilled in the art will appreciate that, although some embodiments herein include certain features included in other embodiments but not other features, the combination of features of different embodiments is meant to be within the scope of the present application and form different embodiments. For example, in the above claims, any one of the claimed embodiments may be used in any combination. The information disclosed in this background technology section is intended only to deepen the understanding of the overall background technology of the present application and should not be regarded as an admission or in any form of implication that the information constitutes prior art known to those skilled in the art.
Claims
1. A method for preparing a foam ceramic filter using waste chromium corundum, It is characterized in that include: Grinding the waste chrome corundum and sieving to obtain fine particles less than 0.15 mm, medium particles of 0.15-0.3 mm, and coarse particles greater than 0.3 mm and less than or equal to 1 mm; The fine particles are mixed with cerium oxide and lanthanum oxide of the same particle size range to obtain a first mixture, the medium particles are mixed with zirconium oxide of the same particle size range to obtain a second mixture, and the coarse particles are mixed with aluminum oxide of the same particle size range to obtain a third mixture; The first mixture, the second mixture, and the third mixture are calcined at 1000-1300° C. for 2-4 times respectively, and then ground and mixed to obtain a fourth mixture; The fourth mixture is mixed with glycerin and solvent oil, and stirred with a double planetary stirrer to obtain a slurry, and soft polyurethane foam is used as a carrier to impregnate the slurry, and then extruded and dried to obtain a blank; The blank is sintered and cooled to obtain a foam ceramic filter.
2. The method for preparing a foam ceramic filter using waste chromium corundum according to claim 1, It is characterized in that The mass ratio of the fine particles, the cerium oxide and the lanthanum oxide is 1:(0.01-0.05):(0.01-0.05), the mass ratio of the medium particles to the zirconium oxide is 1:(0.1-0.5), and the mass ratio of the coarse particles to the aluminum oxide is 1:(0.1-0.5).
3. The method for preparing a foam ceramic filter using waste chromium corundum according to claim 2, It is characterized in that The mass ratio of the first mixture, the second mixture and the third mixture is 1:(1-3):(1-3).
4. The method for preparing a foam ceramic filter using waste chromium corundum according to claim 1, It is characterized in that The calcination time is independently 1-5 h.
5. The method for preparing a foam ceramic filter using waste chromium corundum according to claim 1, It is characterized in that The particle size of the fourth mixture is less than 200 mesh.
6. The method for preparing a foam ceramic filter using waste chromium corundum according to claim 1, It is characterized in that The volume ratio of the glycerol to the solvent oil is 1:(1-5).
7. The method for preparing a foam ceramic filter using waste chromium corundum according to claim 6, It is characterized in that The solid content of the slurry is 20-40%.
8. The method for preparing a foam ceramic filter using waste chromium corundum according to claim 1, It is characterized in that The stirring comprises: Stir at an orbital speed of 500-1000 rpm and an autorotation speed of 1500-2000 rpm for 1-2 hours, then let it stand for 12-24 hours, and then stir at an orbital speed of 100-300 rpm and an autorotation speed of 500-1000 rpm for 12-24 hours.
9. The method for preparing a foam ceramic filter using waste chromium corundum according to claim 1, It is characterized in that The maximum sintering temperature is 1200-1400° C. and the sintering time is 6-8 hours.
10. The method for preparing a foam ceramic filter using waste chromium corundum according to any one of claims 1 to 9, It is characterized in that The flexible polyurethane foam has a pore size of 10-30 PPI.
Citation Information
Patent Citations
Honeycomb ceramic heat accumulator with high heat conduction performance, high specific gravity and good slag resistance
CN102603346A
Method for utilizing solid waste for preparing light-weight heat-insulating wall material
CN106542843A
Zirconium-chromium-corundum refractory material for incinerator used for pyrolysis and gasification of organic solid waste and preparation method of zirconium-chromium-corundum refractory material
CN113788690A
High-chromium-slag-amount sintering formula and synergistic foaming ceramic production process
CN114394845A
High-wear-resistance zirconium-chromium-based corundum refractory plastic material and preparation method thereof
CN115626831A
Cited By
Corundum foamed ceramic filter preparation equipment and method
CN121372560A