Method for preparing cyclohexanol by hydrating cyclohexene
By using sulfonic acid-modified ZSM-5 molecular sieve catalyst, the problems of slow reaction rate and low conversion rate in cyclohexene hydration reaction are solved, efficient production of cyclohexanol is achieved, production costs are reduced, and it is suitable for industrial promotion. .
Patent Information
- Application Number
- CN202410922316.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-10
- Publication Date
- 2024-11-05
AI Technical Summary
In the prior art, the molecular sieve catalyst has a slow reaction rate, low conversion rate, fast inactivation in the cyclohexene hydration reaction, and the ion exchange resin is easy to decompose at high temperatures, which limits its industrial promotion.
The sulfonic acid-modified ZSM-5 molecular sieve is used as a catalyst to increase the reaction rate and conversion rate through the hydration reaction, and reduce the amount of catalyst added to achieve industrial production.
It significantly improves the rate and conversion rate of cyclohexene hydration reaction, reduces production costs, and has good catalyst structure stability, making it suitable for industrial applications.
Smart Images

Figure CN118894760A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of cyclohexanol synthesis, and in particular to a method for preparing cyclohexanol by hydrating cyclohexene. Background Art
[0002] Cyclohexanol is an important chemical intermediate raw material, widely used in the production of chemical products such as resin paint, fragrance, pesticide, etc. It can also be used in the fields of disinfectants, leather softeners and wood preservatives. Cyclohexanol can be used as an intermediate of caprolactam and adipic acid, the raw materials for preparing nylon 6 and nylon 66, and has a large industrial demand. At the same time, due to its advantages such as low volatility and good solubility, cyclohexanol can also be used as a solvent to dissolve a variety of high molecular polymers, rubber, alkyd resins and acetate resins.
[0003] Compared with homogeneous catalysis using inorganic acids as catalysts, the method of generating cyclohexanol by hydration of cyclohexene using solid acids as catalysts has the advantages of good reaction performance, easy catalyst recovery and no corrosion to reaction equipment. It is the main development direction of cyclohexanol production at present.
[0004] At present, the solid acid catalyst commonly used in the cyclohexene hydration reaction is mainly a molecular sieve catalyst, such as ZSM-5, faujasite, mordenite, etc., wherein, ZSM-5 molecular sieve has become the catalyst of the main industrial application of the cyclohexene hydration process to prepare cyclohexanol due to its good stability and shape selectivity. However, in industrial production, this catalyst has the disadvantages of slow reaction rate, low conversion rate, and fast deactivation. In addition to molecular sieve catalysts, ion exchange resins have also been successfully applied to cyclohexene hydration to prepare cyclohexanol, but, due to the characteristic that ion exchange resins are easily decomposed at high temperatures, their industrial promotion is restricted. Therefore, it is necessary to provide a novel catalyst for catalyzing the cyclohexene hydration to prepare cyclohexanol, to improve reaction rate and conversion rate. Summary of the invention
[0005] In view of the problems of slow reaction rate, low conversion rate, and rapid deactivation when molecular sieve is used as a catalyst for preparing cyclohexanol by hydration of cyclohexene in the prior art, the present invention provides a method for preparing cyclohexanol by hydration of cyclohexene. The present invention adopts sulfonic acid group-modified molecular sieve as a catalyst for preparing cyclohexanol by hydration of cyclohexene, effectively improves the reaction rate and conversion rate, and can realize industrial production, with broad market prospects.
[0006] In order to solve the above technical problems, the technical solution provided by the present invention is:
[0007] A method for preparing cyclohexanol by hydrating cyclohexene comprises the following steps:
[0008] Cyclohexanol is obtained by hydration reaction with cyclohexene and water as raw materials and sulfonic acid group-modified ZSM-5 molecular sieve as catalyst.
[0009] Compared with the prior art, the method for preparing cyclohexanol by hydration of cyclohexene provided by the present invention uses sulfonic acid group-modified ZSM-5 as a catalyst, effectively improves the reaction rate and selectivity of cyclohexene hydration, and the conversion rate of cyclohexene can reach more than 18%. It can also effectively reduce the amount of catalyst added and reduce the production cost, thereby providing a new method for preparing cyclohexanol by hydration of cyclohexene. In addition, the method for preparing cyclohexanol provided by the present invention does not need to change the original production system, can realize industrial production, and has high practical value.
[0010] It should be noted that the above hydration reaction is carried out under an inert atmosphere.
[0011] Furthermore, the preparation method of the sulfonic acid group-modified ZSM-5 molecular sieve comprises the following steps:
[0012] S1, adding ZSM-5 molecular sieve into toluene aqueous solution, dispersing evenly, then adding toluene solution of mercaptosilane coupling agent, reacting at 20°C to 60°C for 1h to 4h, to obtain mercaptosilane-modified ZSM-5 molecular sieve;
[0013] S2, adding the mercaptosilane-modified ZSM-5 molecular sieve into a hydrogen peroxide solution, reacting at 40° C. to 80° C. for 2 h to 8 h, separating the solid from the liquid, and drying to obtain a sulfonic acid group-modified ZSM-5 molecular sieve.
[0014] The invention uses ZSM-5 molecular sieve as a raw material, uses a mercaptosilane coupling agent to introduce hydrophobic groups and mercapto groups into the surface and pores of the ZSM-5 molecular sieve, and then oxidizes the ZSM-5 molecular sieve with hydrogen peroxide to obtain a sulfonic acid group-modified ZSM-5 molecular sieve. The synthesized oil-water amphiphilic catalyst is applied to the cyclohexene hydration reaction, which can effectively improve the reaction rate of the water reaction and the conversion rate of the cyclohexene.
[0015] It should be noted that the ZSM-5 molecular sieve used in the present invention is a commercially available ZSM-5 molecular sieve.
[0016] Furthermore, the mass ratio of the ZSM-5 molecular sieve to the mercaptosilane coupling agent is 0.1:2 to 1:2.
[0017] The invention can adjust the loading amount of sulfonic acid groups in the ZSM-5 molecular sieve by controlling the ratio of the ZSM-5 molecular sieve to the mercaptosilane coupling agent, thereby realizing the regulation of the catalytic activity of the ZSM-5 molecular sieve, and has simple operation and is convenient for large-scale production.
[0018] Furthermore, the mass ratio of water in the toluene aqueous solution to the mercaptosilane coupling agent is 1:0.9 to 1:1.1.
[0019] Furthermore, the ratio of the mercaptosilane coupling agent to toluene in the toluene solution of the mercaptosilane coupling agent is (0.1-1) g:20 mL.
[0020] Furthermore, the molar ratio of H2O2 to the mercaptosilane coupling agent in the hydrogen peroxide solution is 1:40 to 1:100.
[0021] Specifically, the mass percentage of the hydrogen peroxide solution is 30%.
[0022] Furthermore, the mercaptosilane coupling agent is 3-mercaptopropyltriethoxysilane.
[0023] Furthermore, in S1, after the reaction is completed, a post-treatment process is also included: solid-liquid separation of the reaction liquid, washing with anhydrous ethanol, and drying to obtain mercaptosilane-modified ZSM-5 molecular sieve.
[0024] Furthermore, the added amount of the catalyst is 5% to 10% of the mass of cyclohexene.
[0025] The sulfonic acid group-modified ZSM-5 molecular sieve provided by the present invention has excellent catalytic activity. Therefore, when applied to the cyclohexene hydration reaction, the addition ratio of the catalyst can be significantly reduced, thereby reducing the production cost of cyclohexanol.
[0026] Furthermore, the temperature of the hydration reaction is 100° C. to 130° C., the pressure is 0.3 MPa to 0.6 MPa, and the reaction time is 1 h to 3 h.
[0027] Furthermore, the mass ratio of cyclohexene to water is 0.3:1 to 0.5:1.
[0028] The present invention uses sulfonic acid group-modified ZSM-5 molecular sieve as a catalyst for cyclohexene hydration reaction. The sulfonic acid group-modified ZSM-5 molecular sieve has the advantages of high activity and high selectivity, thereby significantly improving the reaction rate and conversion rate of the hydration reaction. At the same time, the addition ratio of the catalyst is significantly reduced to about 1 / 4 of the amount of the traditional molecular sieve catalyst. The sulfonic acid group-modified ZSM-5 molecular sieve has good structural stability and can be reused, thereby facilitating the reduction of the production cost of cyclohexanol and having high promotion and application value. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 These are the X-ray diffraction patterns of catalysts A to D prepared in Examples to Example 4, and catalyst G prepared in Comparative Example 1. DETAILED DESCRIPTION
[0030] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0031] In order to better illustrate the present invention, further examples are given below.
[0032] Unless otherwise specified, the raw materials and reagents in the examples of this application are purchased from commercial sources. Among them, ZSM-5 molecular sieve is produced by the catalyst plant of Nankai University, and its silicon-aluminum ratio is 25.
[0033] 3-Mercaptopropyltriethoxysilane was produced by Sinopharm Chemical Co., Ltd.
[0034] The analysis method in the examples of this application is as follows:
[0035] The catalyst structure analysis was performed using a Bruker D8 X-ray diffractometer.
[0036] Micromeritics ASAP 3020 physical adsorption instrument was used to characterize the specific surface area and pore size distribution.
[0037] The product composition was analyzed using a Thermofisher Trace 1300 gas chromatograph (FID detector, TG-WAXMS capillary column).
[0038] Example 1
[0039] This embodiment provides a method for preparing cyclohexanol by hydrating cyclohexene, comprising the following steps:
[0040] S1, preparation of sulfonic acid group-modified ZSM-5 molecular sieve:
[0041] 0.1 g of water was added to 10 mL of toluene, and the mixture was stirred for 10 min. Then 2 g of commercial ZSM-5 molecular sieve was added and the mixture was stirred for 1 h to obtain a ZSM-5 dispersion.
[0042] 0.1 g of 3-mercaptopropyltriethoxysilane was added to 20 mL of toluene, stirred for 1 h, and then added dropwise to the above ZSM-5 dispersion, reacted at 20° C. for 4 h, and after the reaction was completed, filtered, washed with anhydrous ethanol, and dried to obtain a mercaptosilane-modified ZSM-5 molecular sieve;
[0043] Weigh 1 g of the above-mentioned mercaptosilane-modified ZSM-5 molecular sieve, add 30% hydrogen peroxide solution in a molar ratio of 3-mercaptopropyltriethoxysilane to H2O2 of 1:80, carry out oxidation reaction at 60°C for 4 hours, and dry at 120°C to obtain sulfonic acid-modified ZSM-5 molecular sieve, which is recorded as catalyst A.
[0044] S2, preparation of cyclohexanol:
[0045] Cyclohexene and water were mixed in a mass ratio of 0.4:1, and 5% of the mass of cyclohexene catalyst A was added and mixed evenly. The mixture was transferred to a closed reactor and replaced with nitrogen three times. The temperature of the reactor was increased to 120°C, the pressure was increased to 0.4 MPa, the stirring speed was 800 r / min, the reaction was carried out for 120 min, the temperature of the reactor was lowered to room temperature with cold water, the reactor was opened, the material was taken out, centrifuged, and the supernatant was taken for gas chromatography analysis.
[0046] Example 2
[0047] This embodiment provides a method for preparing cyclohexanol by hydrating cyclohexene, comprising the following steps:
[0048] S1, preparation of sulfonic acid group-modified ZSM-5 molecular sieve:
[0049] 0.2 g of water was added to 20 mL of toluene, and the mixture was stirred for 10 min. Then, 2 g of commercial ZSM-5 molecular sieve was added and the mixture was stirred for 1 h to obtain a ZSM-5 dispersion.
[0050] 0.2 g of 3-mercaptopropyltriethoxysilane was added to 20 mL of toluene, stirred for 1 h, then added dropwise to the above ZSM-5 dispersion, reacted at 40° C. for 2 h, filtered after the reaction, washed with anhydrous ethanol, and dried to obtain a mercaptosilane-modified ZSM-5 molecular sieve;
[0051] Weigh 1 g of the above-mentioned mercaptosilane-modified ZSM-5 molecular sieve, add 30% hydrogen peroxide solution in a molar ratio of 3-mercaptopropyltriethoxysilane to H2O2 of 1:80, carry out oxidation reaction at 80°C for 4 hours, and dry at 120°C to obtain sulfonic acid-modified ZSM-5 molecular sieve, which is recorded as catalyst B.
[0052] S2, preparation of cyclohexanol:
[0053] Cyclohexene and water were mixed in a mass ratio of 0.4:1, and catalyst B with a mass ratio of 10% of cyclohexene was added and mixed evenly. The mixture was transferred to a closed reactor and replaced with nitrogen three times. The temperature of the reactor was increased to 120°C, the pressure was increased to 0.4 MPa, the stirring speed was 800 r / min, the reaction was carried out for 120 min, the temperature of the reactor was lowered to room temperature with cold water, the reactor was opened, the material was taken out, centrifuged, and the supernatant was analyzed by gas chromatography.
[0054] Example 3
[0055] This embodiment provides a method for preparing cyclohexanol by hydrating cyclohexene, comprising the following steps:
[0056] S1, preparation of sulfonic acid group-modified ZSM-5 molecular sieve:
[0057] 0.3 g of water was added to 30 mL of toluene and stirred for 10 min, then 2 g of commercial ZSM-5 molecular sieve was added and stirred for 1 h to obtain a ZSM-5 dispersion;
[0058] 0.3 g of 3-mercaptopropyltriethoxysilane was added to 20 mL of toluene, stirred for 1 h, then added dropwise to the above ZSM-5 dispersion, reacted at 60° C. for 1 h, filtered after the reaction, washed with anhydrous ethanol, and dried to obtain a mercaptosilane-modified ZSM-5 molecular sieve;
[0059] Weigh 1 g of the above-mentioned mercaptosilane-modified ZSM-5 molecular sieve, add 30% hydrogen peroxide solution in a molar ratio of 3-mercaptopropyltriethoxysilane to H2O2 of 1:60, carry out oxidation reaction at 40°C for 8 hours, and dry at 120°C to obtain sulfonic acid-modified ZSM-5 molecular sieve, which is recorded as catalyst C.
[0060] S2, preparation of cyclohexanol:
[0061] Cyclohexene and water were mixed in a mass ratio of 0.4:1, and 8% of the mass of cyclohexene catalyst C was added and mixed evenly. The mixture was transferred to a closed reactor and replaced with nitrogen three times. The temperature of the reactor was increased to 130°C, the pressure was increased to 0.6MPa, the stirring speed was 800r / min, the reaction was carried out for 60min, the temperature of the reactor was lowered to room temperature with cold water, the reactor was opened, the material was taken out, centrifuged, and the supernatant was taken for gas chromatography analysis.
[0062] Example 4
[0063] This embodiment provides a method for preparing cyclohexanol by hydrating cyclohexene, comprising the following steps:
[0064] S1, preparation of sulfonic acid group-modified ZSM-5 molecular sieve:
[0065] 0.5 g of water was added to 50 mL of toluene and stirred for 10 min, then 2 g of commercial ZSM-5 molecular sieve was added and stirred for 1 h to obtain a ZSM-5 dispersion;
[0066] 0.5 g of 3-mercaptopropyltriethoxysilane was added to 20 mL of toluene, stirred for 1 h, then added dropwise to the above ZSM-5 dispersion, reacted at 50° C. for 1 h, filtered after the reaction, washed with anhydrous ethanol, and dried to obtain a mercaptosilane-modified ZSM-5 molecular sieve;
[0067] Weigh 1 g of the above-mentioned mercaptosilane-modified ZSM-5 molecular sieve, add 30% hydrogen peroxide solution in a molar ratio of 3-mercaptopropyltriethoxysilane to H2O2 of 1:60, carry out oxidation reaction at 80°C for 6 hours, and dry at 120°C to obtain sulfonic acid-modified ZSM-5 molecular sieve, which is recorded as catalyst D.
[0068] S2, preparation of cyclohexanol:
[0069] Cyclohexene and water were mixed in a mass ratio of 0.4:1, and 7% of the mass of cyclohexene catalyst D was added and mixed evenly. The mixture was transferred to a closed reactor and replaced with nitrogen three times. The temperature of the reactor was increased to 110°C, the pressure was increased to 0.5 MPa, the stirring speed was 800 r / min, the reaction was carried out for 140 min, the temperature of the reactor was lowered to room temperature with cold water, the reactor was opened, the material was taken out, centrifuged, and the supernatant was taken for gas chromatography analysis.
[0070] Example 5
[0071] This embodiment provides a method for preparing cyclohexanol by hydrating cyclohexene, comprising the following steps:
[0072] S1, preparation of sulfonic acid group-modified ZSM-5 molecular sieve:
[0073] Add 1 g of water to 100 mL of toluene and stir for 10 min, then add 2 g of commercial ZSM-5 molecular sieve and stir for 1 h to obtain a ZSM-5 dispersion;
[0074] 1 g of 3-mercaptopropyltriethoxysilane was added to 20 mL of toluene, stirred for 1 h, then added dropwise to the above ZSM-5 dispersion, reacted at 30° C. for 3 h, filtered after the reaction, washed with anhydrous ethanol, and dried to obtain a mercaptosilane-modified ZSM-5 molecular sieve;
[0075] Weigh 1 g of the above-mentioned mercaptosilane-modified ZSM-5 molecular sieve, add 30% hydrogen peroxide solution in a molar ratio of 3-mercaptopropyltriethoxysilane to H2O2 of 1:40, carry out oxidation reaction at 100°C for 2h, and dry at 120°C to obtain sulfonic acid-modified ZSM-5 molecular sieve, which is recorded as catalyst E.
[0076] S2, preparation of cyclohexanol:
[0077] Cyclohexene and water were mixed in a mass ratio of 0.4:1, and catalyst E was added at 10% of the mass of cyclohexene. The mixture was evenly mixed and transferred to a closed reactor. The mixture was replaced with nitrogen three times. The temperature of the reactor was increased to 100°C, the pressure was increased to 0.6 MPa, the stirring speed was 800 r / min, the reaction was carried out for 150 min, the temperature of the reactor was lowered to room temperature with cold water, the reactor was opened, the material was taken out, centrifuged, and the supernatant was analyzed by gas chromatography.
[0078] Example 6
[0079] This embodiment provides a method for preparing cyclohexanol by hydrating cyclohexene, comprising the following steps:
[0080] S1, preparation of sulfonic acid group-modified ZSM-5 molecular sieve:
[0081] 0.7 g of water was added to 70 mL of toluene, and the mixture was stirred for 10 min. Then, 2 g of commercial ZSM-5 molecular sieve was added and the mixture was stirred for 1 h to obtain a ZSM-5 dispersion.
[0082] 0.7 g of 3-mercaptopropyltriethoxysilane was added to 20 mL of toluene, stirred for 1 h, then added dropwise to the above ZSM-5 dispersion, reacted at 40° C. for 3 h, filtered after the reaction, washed with anhydrous ethanol, and dried to obtain a mercaptosilane-modified ZSM-5 molecular sieve;
[0083] Weigh 1 g of the above-mentioned mercaptosilane-modified ZSM-5 molecular sieve, add 30% hydrogen peroxide solution in a molar ratio of 3-mercaptopropyltriethoxysilane to H2O2 of 1:100, carry out oxidation reaction at 60°C for 3 h, and dry at 120°C to obtain sulfonic acid-modified ZSM-5 molecular sieve, which is recorded as catalyst F.
[0084] S2, preparation of cyclohexanol:
[0085] Cyclohexene and water were mixed in a mass ratio of 0.4:1, and catalyst F with a mass percentage of 9% of cyclohexene was added and mixed evenly. The mixture was transferred to a closed reactor and replaced with nitrogen three times. The temperature of the reactor was increased to 130°C, the pressure was increased to 0.3 MPa, the stirring speed was 800 r / min, the reaction was carried out for 180 min, the temperature of the reactor was lowered to room temperature with cold water, the reactor was opened, the material was taken out, centrifuged, and the supernatant was taken for gas chromatography analysis.
[0086] Comparative Example 1
[0087] The ZSM-5 molecular sieve was calcined at 550°C for 240 min and cooled to room temperature, which was recorded as Catalyst G.
[0088] Comparative Example 2
[0089] 0.2 g of water was added to 20 mL of toluene, and the mixture was stirred for 10 min. Then, 2 g of commercial ZSM-5 molecular sieve was added and the mixture was stirred for 1 h to obtain a ZSM-5 dispersion.
[0090] 0.2 g of 3-mercaptopropyltriethoxysilane was added to 20 mL of toluene and stirred for 1 h. Then, it was added dropwise to the above ZSM-5 dispersion and reacted at 40° C. for 2 h. After the reaction, it was filtered with suction, washed with anhydrous ethanol, and dried to obtain a mercaptosilane-modified ZSM-5 molecular sieve, which was recorded as catalyst H.
[0091] Catalyst surface area, pore volume and pore size distribution test
[0092] Nitrogen physical adsorption-desorption and pore structure analysis were performed on catalysts A to E prepared in Examples 1 to 5 and catalyst G prepared in Comparative Example 1, and the specific surface area, pore volume and pore diameter were calculated based on the obtained nitrogen physical adsorption-desorption curves. The results are shown in Table 1.
[0093] Table 1 Specific surface area, pore volume and pore diameter of catalysts
[0094]
[0095] X-ray diffraction test of catalyst
[0096] Catalysts A to D prepared in Examples 1 to 4 and Catalyst G prepared in Comparative Example 1 were subjected to X-ray diffraction tests. The results are as follows: Figure 1 shown.
[0097] Catalytic performance of catalysts
[0098] Table 2 Cyclohexene conversion and cyclohexanol selectivity
[0099]
[0100]
[0101] Catalyst stability test
[0102] The catalyst B used in Example 2 was washed twice with ethanol, dried at 80°C, and stored for later use. The reactor was replaced with nitrogen twice, cyclohexene and water were mixed at a mass ratio of 0.4:1, and 10% of the mass of cyclohexene in the regenerated catalyst B was added, the reactor was heated to 120°C, the pressure was raised to 0.4MPa, the stirring speed was 800r / min, the reaction was carried out for 120min, the reactor temperature was lowered to room temperature with cold water, the reactor was opened to take out the material, centrifuged, and the supernatant was analyzed by gas chromatography, which was repeated 7 times. The cyclohexene conversion rate and cyclohexanol selectivity are shown in Table 3.
[0103] Table 3 Catalyst stability test
[0104] Experiment No. Cyclohexene conversion rate % Cyclohexanol selectivity % 1 18.8 99.8 2 18.7 99.8 3 18.6 99.6 4 18.2 99.6 5 17.8 99.6 6 17.4 99.5 7 17.4 99.4
[0105] It can be seen from the above table that the sulfonic acid group-modified ZSM-5 molecular sieve prepared in the embodiment of the present invention shows higher stability in the reaction of preparing cyclohexanol by hydration of cyclohexene.
[0106] In summary, the lipophilicity of ZSM-5 zeolite can be increased by silanization loading, but the conversion rate is not significantly improved; after oxidation, the cyclohexene hydration reaction rate is greatly increased, the reaction selectivity is also significantly improved, and the catalyst is easy to separate after the reaction and has a good cycle life, which provides a new method for the preparation of cyclohexanol by hydration of cyclohexene and has broad application prospects.
[0107] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modification, equivalent substitution or improvement made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing cyclohexanol by hydrating cyclohexene, characterized in that: The steps include: Cyclohexanol is obtained by hydration reaction with cyclohexene and water as raw materials and sulfonic acid group-modified ZSM-5 molecular sieve as catalyst.
2. The method for preparing cyclohexanol by hydrating cyclohexene as claimed in claim 1, characterized in that: The preparation method of the sulfonic acid group-modified ZSM-5 molecular sieve comprises the following steps: Add ZSM-5 molecular sieve into toluene aqueous solution and disperse it evenly, then add toluene solution of mercaptosilane coupling agent and react at 20°C to 60°C for 1h to 4h to obtain mercaptosilane-modified ZSM-5 molecular sieve; The mercaptosilane-modified ZSM-5 molecular sieve is added into a hydrogen peroxide solution, reacted at 40° C. to 80° C. for 2 h to 8 h, solid-liquid separation is performed, and the mixture is dried to obtain the sulfonic acid group-modified ZSM-5 molecular sieve.
3. The method for preparing cyclohexanol by hydrating cyclohexene as claimed in claim 2, characterized in that: The mass ratio of the ZSM-5 molecular sieve to the mercaptosilane coupling agent is 0.1:2 to 1:
2.
4. The method for preparing cyclohexanol by hydrating cyclohexene as claimed in claim 2, characterized in that: The mass ratio of water in the toluene aqueous solution to the mercaptosilane coupling agent is 1:0.9 to 1:1.
1.
5. The method for preparing cyclohexanol by hydrating cyclohexene as claimed in claim 2, characterized in that: The ratio of the mercaptosilane coupling agent to toluene in the toluene solution of the mercaptosilane coupling agent is (0.1-1) g:20 mL.
6. The method for preparing cyclohexanol by hydrating cyclohexene as claimed in claim 2, characterized in that: The molar ratio of H2O2 to the mercaptosilane coupling agent in the hydrogen peroxide solution is 1:40 to 1:
100.
7. The method for preparing cyclohexanol by hydrating cyclohexene as claimed in claim 2, characterized in that: The mercaptosilane coupling agent is 3-mercaptopropyltriethoxysilane.
8. The method for preparing cyclohexanol by hydrating cyclohexene according to any one of claims 1 to 7, characterized in that: The added amount of the catalyst is 5% to 10% of the mass of cyclohexene.
9. The method for preparing cyclohexanol by hydrating cyclohexene as claimed in claim 1, characterized in that: The temperature of the hydration reaction is 100° C. to 130° C., the pressure is 0.3 MPa to 0.6 MPa, and the reaction time is 1 h to 3 h.
10. The method for preparing cyclohexanol by hydrating cyclohexene as claimed in claim 1, characterized in that: The mass ratio of the cyclohexene to water is 0.3:1 to 0.5:1.
Citation Information
Cited By
Preparation method and application of hydration catalyst
CN120827915A