Acidification diverter and preparation method thereof, self-assembly diverter acid

Through the combination of polymer acidification steering agent and surfactant, self-assembled steering acid is formed, which solves the problems of low efficiency and great damage to the formation of existing acidification steering agents, achieves rapid viscosity increase and efficient sealing, and expands acidification Application scope and improve the utilization rate and acidification effect of acid solution.

CN118894960BActive Publication Date: 2024-12-03SOUTHWEST PETROLEUM UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411403409.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-10-09
Publication Date
2024-12-03
Estimated Expiration
2044-10-09

AI Technical Summary

Technical Problem

The existing acidification steering agents have low acidification steering efficiency, poor acidification effect, and narrow pH range, which can easily cause damage to the formation.

Method used

The free radicals are adopted by acrylamide, 3-[[2-(methacryloyloxy)ethyl]dimethylammonium]propane-1-sulfonate and 1-hexadecyl-3-vinylimidazole The polymeric acid-forming steering agent prepared by polymerization combines surfactant to form a self-assembled steering acid, achieving rapid viscosity increase and efficient sealing of the high-permeability layer.

Benefits of technology

It realizes rapid viscosity increase, improves acidification turnover efficiency under low acid rock reaction degree, expands the scope of acidification application, avoids damage to the formation by metal ion precipitation, has excellent high temperature resistance and shear resistance, and improves acid utilization rate and acidification effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118894960B_ABST
    Figure CN118894960B_ABST
Patent Text Reader

Abstract

The present application discloses an acidizing diverter and a preparation method thereof, and a self-assembling diverter acid, which belongs to the technical field of oil and gas well exploitation. The acidizing diverter is obtained by polymerization reaction of 4.2 to 4.6 parts of acrylamide, 4.8 to 5.4 parts of 3-[[2-(methacryloyloxy)ethyl]dimethylammonium]propane-1-sulfonate and 0.14 to 0.2 parts of 1-hexadecyl-3-vinyl imidazole, specifically a polymer. The present application also discloses a self-assembling diverter acid, which includes hydrochloric acid with a mass fraction of 20%, the aforementioned acidizing diverter and a surfactant, has a low initial viscosity, can achieve rapid viscosity increase at a lower acid-rock reaction degree, has the advantages of high efficiency plugging of high permeability layers, and can effectively achieve rapid diversion. And the introduced imidazole-based ion monomer has better aggregation behavior and temperature resistance, greatly improves the acidizing application effect, expands the scope of acidizing application, and promotes the exploitation of oil wells to be more efficient and high-yield.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of oil and gas well exploitation, and in particular relates to an acidizing diverter and a preparation method thereof, and a self-assembly diverter acid. Background Art

[0002] Acidizing is a measure of enhanced oil recovery (EOR) and an effective technical measure for increasing the production of oil and gas wells and injection wells. Its principle is to restore or improve the permeability of formation pores and fractures through the dissolution and corrosion of rock cements or blockages in formation pores and fractures by acid.

[0003] The carbonate reservoirs in my country are relatively old in geological age, with deep burial depth, high formation temperature, and heterogeneity. During the acidizing process, due to the heterogeneity of the formation, the acid tends to enter the high-permeability layer or low-pollution layer with less resistance first, while the low-permeability layer or high-pollution layer that needs to be transformed has less acid, resulting in uneven acid distribution, low acidizing efficiency, and large acid consumption. In order to improve the acidizing effect, acidizing diversion technology is often used.

[0004] In the prior art, acid diversion technology mainly includes foam diversion agents, polymer diversion agents and viscoelastic surfactant diversion agents. Each technology has its own advantages and disadvantages, but it is difficult for the prior art to simultaneously achieve the effects of high temperature resistance, low damage, and high efficiency. The working principle of polymer diversion agents is to cross-link with cross-linking agents under formation conditions to form a high-viscosity fluid to block the high permeability layer, allowing the acid to flow to the low permeability layer area. This type of diversion agent has problems such as a narrow applicable pH range and the easy precipitation of metal ions that cause great damage to the formation.

[0005] Please refer to the invention patent entitled "A temperature-resistant acidification diverter and preparation method and carbonate reservoir acidification acid solution" and publication number CN117343233A. This patent discloses a polymer acidification diverter, which solves the problem of the existing technology that polymers need to be used in combination with metal ion cross-linking agents to cause great damage to the formation, but there are still certain problems: the diverter is applicable to a narrow pH range, the viscosity is slow, the plugging effect is late, and the acidification diverter efficiency is average. Therefore, the existing technology still has room for improvement. Summary of the invention

[0006] In view of this, the purpose of the embodiments of the present application is to provide an acid diverter to solve the problem that the acid diverter efficiency of the prior art acid diverter is general and the acid effect is poor. The acid diverter provided by the embodiments of the present application can achieve rapid viscosity increase at a lower acid-rock reaction degree and has the advantages of high efficiency plugging of high permeability layers, and can effectively achieve rapid diversion. The introduced imidazole ion monomer makes the diverting acid have better aggregation behavior and temperature resistance, greatly improves the acid application effect, expands the acid application range, and makes the exploitation of oil wells more efficient and high-yield.

[0007] The embodiment of the present application is implemented as follows:

[0008] The present application provides an acidification diverting agent, comprising a polymer having a structure shown in structural formula (1), wherein structural formula (1) is: ; Among them, the ratios of x, y, and z are (4.2~4.6):(4.8~5.4):(0.14~0.2).

[0009] Furthermore, the acid diverter is obtained by free radical polymerization of three monomers, and the amounts of the three monomers are embodied in molar ratio, specifically 4.2 to 4.6 parts of acrylamide, 4.8 to 5.4 parts of 3-[[2-(methacryloyloxy)ethyl]dimethylammonio]propane-1-sulfonate and 0.14 to 0.2 parts of 1-hexadecyl-3-vinyl imidazole. The presence of the imidazole group makes the acid diverter exhibit abundant self-aggregation behavior and can rapidly increase viscosity; and the rigid five-membered ring structure of imidazole makes the acid diverter have higher strength and excellent high temperature shear resistance.

[0010] The present application also provides a method for preparing the above-mentioned acidification diverter, comprising the following steps:

[0011] S1. dissolving three monomers, acrylamide, 3-[[2-(methacryloyloxy)ethyl]dimethylammonium]propane-1-sulfonate and 1-hexadecyl-3-vinylimidazole in deionized water in a nitrogen atmosphere to obtain a mixed solution;

[0012] S2. The mixed solution is heated to 40-60°C and the pH value of the solution is adjusted to 7;

[0013] S3. Adding an initiator to initiate the polymerization reaction for 5h to obtain a crude polymer;

[0014] S4. Wash and shred the crude polymer, and vacuum dry it to obtain an acidification diversion agent. Based on this method, the prepared acidification diversion agent has high purity, basically does not contain oligomers, and can exert a good acidification diversion effect.

[0015] Furthermore, in step S1, the sum of the masses of the three monomers accounts for 20-30% of the mass of the reaction system, that is, the monomer concentration is 20-30%.

[0016] Furthermore, in step S3, the initiator is 2,2-azobis(2-methylpropylimidazole) dihydrochloride.

[0017] Furthermore, the mass of the initiator in step S3 accounts for 0.6% of the mass of the reaction system.

[0018] Furthermore, in step S4, anhydrous ethanol is used to wash the crude polymer.

[0019] The present application also provides a self-assembling steering acid, which includes the acidification steering agent provided above or prepared by the above method; and also includes a hydrochloric acid solution with a mass fraction of 20% and a surfactant. Among them, the amount of the acidification steering agent is 1wt% of the amount of hydrochloric acid, and the amount of the surfactant is 0.1-0.5wt% of the amount of hydrochloric acid. The self-assembly mechanism is the electrostatic binding effect between the polymer acidification steering agent and the surfactant ion.

[0020] Furthermore, the surfactant is octadecyltrimethylammonium chloride.

[0021] Compared with the prior art, the beneficial effects of this application are:

[0022] 1. The polymer acidification diverter provided in the present application is a non-cross-linked diverter, which can achieve rapid viscosity increase and diverting effects without the need for metal ion cross-linking agents, thus avoiding the problem of adding metal ions in oil and gas wells and causing precipitation to cause secondary damage to the formation;

[0023] 2. The imidazole group in the acid diverter provided in the present application has the characteristics of low Krafft temperature, low critical micelle concentration, strong ability to reduce surface tension, etc. It shows excellent self-assembly ability in aqueous solution and can spontaneously form an ordered structure; the configured diverter acid can rapidly change viscosity as the acid-rock reaction proceeds, and the hydrogen ions in the acid liquid react with the calcium ions produced by the acid-rock reaction to achieve a self-viscosity-enhancing effect, rapid viscosity increase, and can efficiently block the high permeability layer. In the acidizing operation, the rapid viscosity increase of the diverter acid represents a higher acid utilization rate, avoiding low diverter efficiency and acid waste caused by excessive acid entering the high permeability layer;

[0024] 3. After the acid diversion agent provided by the present application blocks the high permeability layer and realizes the acid diversion effect, the self-assembled diversion acid still has a high hydrogen ion concentration, and can continue to react with the acid rock and carry out subsequent acidification treatment. This technology can greatly improve the acidification effect, expand the scope of acidification application, and solve the bottleneck problem of acidification diversion technology in the prior art;

[0025] 4. The self-assembled steering acid provided in this application can be heated to 160°C for 170s after the viscosity increases rapidly. -1 Under the shear rate, the apparent viscosity of 70mPa·s is still maintained, the shear resistance is strong, and the polymer network is not easily destroyed; compared with the existing diverting acid, which has the problems of easy destruction of structure under shear force, easy loss of diverting performance, inability to achieve uniform acid distribution, and poor acidification effect, the self-assembled diverting acid provided in the present application still maintains good strength during subsequent operations, and the stability of the diverting acid will not be destroyed due to high-intensity operations, and repeated acid injection and other problems will not occur;

[0026] 5. After the self-assembled diverting acid provided in the present application achieves the purpose of acidification diversion with high efficiency, the decrease in its viscosity is conducive to the subsequent gel breaking and return treatment of the residual acid. The subsequent gel breaking and return treatment is simpler, consumes less resources, and has higher economic benefits. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0028] Figure 1 This is a graph showing the relationship between the residual acid viscosity value of the self-assembled steering acid prepared in Example 4 of the present application and the amount of water added;

[0029] Figure 2 This is the infrared spectrum characterization diagram of the acidification diverting agent prepared in Example 4 of the present application;

[0030] Figure 3 This is a test chart of the high temperature resistance and shear resistance of the self-assembled steering acid prepared in Example 4 of the present application. DETAILED DESCRIPTION

[0031] In order to make the purpose, technical scheme and advantages of the present application more clearly understood, the present application is further described in detail below in conjunction with the embodiments. The illustrative implementation methods and descriptions of the present application are only used to explain the present application and are not intended to limit the present application. Any product identical or similar to the present application that is obtained by anyone under the inspiration of the present application or by combining the features of the present application with other prior arts shall fall within the protection scope of the present application.

[0032] The specific experimental steps or conditions not indicated in the embodiment can be carried out according to the operation or conditions of the conventional experimental steps described in the prior art in this area. The reagents used and other instruments that do not indicate the manufacturer are all conventional reagent products that can be obtained commercially. In addition, the accompanying drawings are only schematic diagrams of the embodiments of the present application and are not necessarily drawn to scale. The same reference numerals in the figure represent the same or similar parts, and thus their repeated description will be omitted. Some block diagrams shown in the accompanying drawings are functional entities and do not necessarily correspond to physically or logically independent entities.

[0033] The present application provides an acidification diversion agent, which includes a polymer as shown in structural formula (1). Structural formula (1) is: ; Among them, the ratios of x, y, and z are (4.2~4.6):(4.8~5.4):(0.14~0.2).

[0034] Furthermore, the polymer is obtained by free radical polymerization of three monomers, which are acrylamide (hereinafter referred to as AM), 3-[[2-(methacryloyloxy)ethyl]dimethylammonio]propane-1-sulfonate (hereinafter referred to as SPE) and 1-hexadecyl-3-vinylimidazole (hereinafter referred to as NV-16). The molar ratio of AM, SPE and NV-16 is (4.2-4.6): (4.8-5.4): (0.14-0.2).

[0035] The applicant creatively discovered that in the process of synthesizing the acidification diverter, the free electrons on the imidazole ring in NV-16 and the hydrogen bonds between the imidazole rings exhibited abundant self-aggregation behaviors, and the hydrophobic long chain structure provided by the hexadecyl group in NV-16 acted together to realize the abundant associative entanglement behaviors of the molecular structure of the diverter acid, and the polymerization and adhesion were faster; compared with the traditional quaternary ammonium salt monomers with the same hydrophobic chain length, the imidazole hydrophobic monomers have lower Kraft temperature, smaller critical micelle concentration, higher ability to reduce surface tension, and stronger self-assembly ability in aqueous solution, which can effectively ensure the rapid formation of aggregates in the acid solution, making the acid solution thickening fast and efficient. The imidazole groups and hydrophobic long chains in the acid solution exhibited associative entanglement effects, and the acid solution spontaneously and rapidly thickened under the influence of changes in the concentration of hydrogen ions in the acid solution and the concentration of calcium ions in the acid-rock reaction. Moreover, the imidazole groups introduced by NV-16 have a five-membered rigid ring structure, which is more stable and can greatly enhance the temperature resistance and shear resistance of the polymer. Based on this, the acidification diverter provided in the present application can effectively achieve rapid diversion and thus achieve the purpose of uniform acid distribution.

[0036] The specific preparation steps of the acidification diverter are:

[0037] S1. Under nitrogen atmosphere, place an appropriate amount of NV-16 in a reaction container, add an appropriate amount of deionized water and stir to dissolve, then add an appropriate amount of AM and SPE and stir to dissolve and mix evenly to prepare a mixed solution with a concentration of 20-30%. That is, the sum of the mass of the three monomers AM, SPE and NV-16 and the mass ratio of the reaction system (AM, SPE, NV-16 and deionized water) is 20-30%.

[0038] Passing nitrogen into the reaction vessel can remove residual oxygen and other gases in the container, avoiding interference of oxygen and other gases on the polymerization reaction of the monomer; continue to pass nitrogen until the reaction vessel is sealed to ensure that no new oxygen and other gases are mixed into the reaction process. Specifically, continue to pass nitrogen into the reaction vessel until the initiator is added (see step S3). After the initiator is added, the reaction container is sealed and the nitrogen can be stopped. Whether nitrogen remains in the reaction vessel has no effect on the reaction. Helium, argon or other inert gases can also be introduced to drive out oxygen, which is not limited in this application.

[0039] S2. The reaction system is heated to 40-60° C. and maintained at a constant temperature. Then, an appropriate amount of alkaline solution is added and stirred to adjust the pH value of the reaction system to 7. The alkaline solution added is preferably sodium hydroxide solution.

[0040] S3. Add an appropriate amount of initiator 2,2-azobis(2-methylpropylimidazole) dihydrochloride (hereinafter referred to as V50) to the constant temperature reaction system to initiate polymerization. The mass of V50 is 0.6% of the sum of the masses of the three monomers (AM, SPE and NV-16). After adding the initiator, the polymerization reaction is carried out for 5 hours to obtain a crude polymer.

[0041] S4, the crude polymer appears as a gel-like solid. At this time, it has a certain viscosity because it contains a certain amount of water, unreacted monomers and oligomers. Taking advantage of the fact that unreacted monomers and oligomers are soluble in water and ethanol, and crude polymers are insoluble in ethanol, anhydrous ethanol is used to rinse and shred the crude product to remove moisture, unreacted monomers and oligomer impurities in the crude product, and obtain a brittle, non-sticky polymer. The polymer has a high purity, and the oligomer component is very small, which can play an excellent self-adhesive effect in the subsequent acidification and diversion process. The polymer is placed in a vacuum oven and dried at 45-50°C to obtain a pure polymer acidification and diversion agent.

[0042] The present application also discloses a self-assembling steering acid, which includes the polymer acidification steering agent provided in the present application. The self-assembly mechanism is the electrostatic binding effect between the polymer acidification steering agent and the surfactant ion. The specific preparation steps of the self-assembling steering acid are:

[0043] Take an appropriate amount of 20% hydrochloric acid solution, add 1wt% of pure polymer acidification steering agent and 0.1-0.5wt% of cationic surfactant, stir evenly, and self-assembly steering acid can be obtained. The cationic surfactant is preferably one or more of tetradecyltrimethylammonium chloride, hexadecyltrimethylammonium chloride and octadecyltrimethylammonium chloride, more preferably octadecyltrimethylammonium chloride.

[0044] The self-assembling steering acid provided in this application introduces imidazole ion monomers, which makes the steering acid have lower critical micelle concentration and surface tension, stronger self-assembly ability, better surface activity and richer aggregation behavior in acid solution; and the imidazole group, as a five-membered rigid ring structure, has better stability, making the steering acid have better high temperature resistance and shear resistance. The experimental results show that the acid solution at the maximum viscosity is at 160℃ and 170s -1 At a shear rate of , the acid solution still has an apparent viscosity of 70 mPa·s. Under lower acid-rock reaction conditions (when the acid solution still has a high hydrogen ion concentration), the viscosity reaches 336 mPa·s. Compared with the prior art in which the maximum viscosity is reached at the end of the acid-rock reaction, the imidazole-based self-assembled steering acid provided in this application can continue to acidify until the acidification operation is completed, and has a more efficient reservoir acidification treatment effect. In addition, the preparation method of the self-assembled steering acid is simple and energy-saving. In actual use, a small amount can achieve an acidification steering effect, and the practical application value is high.

[0045] In order to enable those skilled in the art to more clearly understand the present invention, the acidification diverting agent and the self-assembling diverting acid described in the present application will be described in detail below through examples and test examples.

[0046] Embodiment 1:

[0047] Take the raw materials according to the molar ratio, place 0.14 parts of NV-16 in a reaction container, add an appropriate amount of deionized water under a nitrogen atmosphere and stir to dissolve, then add 4.6 parts of AM and 5.2 parts of SPE and stir to dissolve, mix evenly, and obtain a mixed solution with a mass fraction of 20%. Heat the reaction system to 40°C and keep the temperature constant, add sodium hydroxide solution and adjust the pH value of the reaction system to 7, add 0.6% of V50 initiator and react for 5h to obtain a crude product. Wash the crude product with anhydrous ethanol and cut it into pieces, send it into a vacuum oven and dry it thoroughly to obtain an acidification steering agent, recorded as ASN1.

[0048] A 20% by mass hydrochloric acid solution was measured, and 1 wt % of ASN1 and 0.1 wt % of a surfactant, octadecyltrimethylammonium chloride, were added thereto to obtain a self-assembled steering acid, which was recorded as steering acid 1.

[0049] Embodiment 2:

[0050] Take the raw materials according to the molar ratio, place 0.2 parts of NV-16 in the reaction container, add an appropriate amount of deionized water under nitrogen atmosphere and stir to dissolve, then add 4.2 parts of AM and 5.2 parts of SPE and stir to dissolve, mix evenly, and obtain a mixed solution with a mass fraction of 25%. Heat the reaction system to 50°C and keep the temperature constant, add sodium hydroxide solution and adjust the pH value of the reaction system to 7, add 0.6% of V50 initiator and react for 5h to obtain a crude product. Wash the crude product with anhydrous ethanol and cut it into pieces, send it into a vacuum oven and dry it thoroughly to obtain an acidification steering agent, recorded as ASN2.

[0051] A 20% by mass hydrochloric acid solution was measured, and 1 wt % of ASN2 and 0.2 wt % of a surfactant octadecyltrimethylammonium chloride were added thereto to obtain a self-assembled steering acid, which was recorded as steering acid 2.

[0052] Embodiment 3:

[0053] Take the raw materials according to the molar ratio, place 0.16 parts of NV-16 in a reaction container, add an appropriate amount of deionized water under a nitrogen atmosphere and stir to dissolve, then add 4.6 parts of AM and 5.4 parts of SPE and stir to dissolve, mix evenly, and obtain a mixed solution with a mass fraction of 30%. Heat the reaction system to 60°C and keep the temperature constant, add sodium hydroxide solution and adjust the pH value of the reaction system to 7, add 0.6% of V50 initiator and react for 5h to obtain a crude product. Wash the crude product with anhydrous ethanol and cut it into pieces, send it into a vacuum oven and dry it thoroughly to obtain an acidification steering agent, recorded as ASN3.

[0054] A 20% by mass hydrochloric acid solution was measured, and 1 wt % of ASN1 and 0.5 wt % of a surfactant, octadecyltrimethylammonium chloride, were added thereto to obtain a self-assembled steering acid, which was recorded as steering acid 3.

[0055] Embodiment 4:

[0056] Take the raw materials according to the molar ratio, place 0.16 parts of NV-16 in a reaction container, add an appropriate amount of deionized water under a nitrogen atmosphere and stir to dissolve, then add 4.6 parts of AM and 5.2 parts of SPE and stir to dissolve, mix evenly, and obtain a mixed solution with a mass fraction of 25%. Heat the reaction system to 50°C and keep the temperature constant, add sodium hydroxide solution and adjust the pH value of the reaction system to 7, add 0.6% of V50 initiator and react for 5h to obtain a crude product. Wash the crude product with anhydrous ethanol and cut it into pieces, send it into a vacuum oven and dry it thoroughly to obtain an acidification steering agent, recorded as ASN4.

[0057] A 20% by mass hydrochloric acid solution was measured, and 1 wt % of ASN1 and 0.2 wt % of a surfactant, octadecyltrimethylammonium chloride, were added thereto to obtain a self-assembled steering acid, which was recorded as steering acid 4.

[0058] Embodiment 5:

[0059] Take the raw materials according to the molar ratio, place 0.16 parts of NV-16 in the reaction container, add an appropriate amount of deionized water under nitrogen atmosphere and stir to dissolve, then add 4.6 parts of AM and 4.8 parts of SPE and stir to dissolve, mix evenly, and obtain a mixed solution with a mass fraction of 25%. Heat the reaction system to 50°C and keep the temperature constant, add sodium hydroxide solution and adjust the pH value of the reaction system to 7, add 0.6% of V50 initiator and react for 5h to obtain a crude product. Wash the crude product with anhydrous ethanol and cut it into pieces, send it into a vacuum oven and dry it thoroughly to obtain an acidification steering agent, recorded as ASN5.

[0060] A 20% by mass hydrochloric acid solution was measured, and 1 wt % of ASN1 and 0.2 wt % of a surfactant octadecyltrimethylammonium chloride were added thereto to obtain a self-assembled steering acid, which was recorded as steering acid 5.

[0061] Test Example 1:

[0062] The self-assembled steering acid obtained in Example 1 to Example 5 was evaluated. Specifically, five beakers containing equal amounts of steering acid were placed in a constant temperature water bath at 90°C. The reaction of calcium carbonate and hydrochloric acid will consume hydrochloric acid. A certain amount of calcium carbonate powder was added in sequence according to the stoichiometric relationship between calcium carbonate and hydrochloric acid. The beakers were sealed with plastic wrap to prevent the volatilization of hydrochloric acid, and reaction solutions with hydrochloric acid concentrations of 20%, 15%, 10%, 5% and 0 were obtained in sequence. After being fully stirred and defoamed in a constant temperature water bath, the steering acids with different reaction degrees were placed in the sample cup of a six-speed rotary viscometer and heated for 170s. -1 The apparent viscosity was tested at a shear rate of , and the results are shown in the following table.

[0063] Table 1: Apparent viscosity of the diverting acid at different hydrochloric acid concentrations

[0064] As can be seen from the above table, the diverting acid obtained in Examples 1-5 has a regular viscosity performance, that is, the viscosity is lowest when the hydrochloric acid concentration is 20%, and the viscosity is highest when the hydrochloric acid concentration is 10%. Since the initial diverting hydrochloric acid concentration is 20%, that is, when calcium carbonate powder is not added, that is, when the hydrogen ions in the diverting acid do not react with calcium carbonate, the viscosity of the diverting acid is the lowest, which is conducive to the injection of the diverting acid into the formation. As the acid-rock reaction proceeds, the hydrogen ions in the diverting acid are consumed, and the hydrochloric acid concentration gradually decreases; it can be seen from the table that the viscosity of the diverting acid increases rapidly, and the viscosity of the diverting acid reaches the highest point when the hydrochloric acid concentration is 10%. It can be proved that in practical applications, the diverting acid provided in this application quickly forms a high-viscosity fluid, and the high-viscosity fluid can block the high-permeability layer with low resistance, so that the acid solution flows to the low-permeability layer area. At this time, there are still more hydrogen ions in the acid solution, and the acidity is still maintained at a certain level, and the subsequent acidification treatment work can continue.

[0065] As hydrogen ions are consumed, the viscosity of the self-assembled steering acid provided in the present application gradually decreases. The reason is that the hydrogen ion concentration in the acid solution will affect the viscosity of the steering acid. Specifically, the viscosity increases rapidly with the acid-rock reaction. After reaching the peak, the aggregation ability of the acidifying steering agent molecules gradually decreases, the aggregate structure is gradually destroyed, resulting in a reduction in its size, and the interaction between molecules is weakened, thereby resulting in a decrease in the apparent viscosity of the system.

[0066] During the acidizing process of oil and gas wells, the diverting acid plays a temporary plugging role, thereby enabling the acid to flow to the low-permeability layer or high-pollution layer with high resistance; in actual production, high-viscosity acid is not allowed to remain in the formation all the time, which will cause serious damage to the reservoir. After the acid is diverted, the diverting acid stuck in the formation needs to be debonded and returned. After the self-assembled diverting acid system provided in the present application plays its temporary plugging and diverting role, its apparent viscosity is reduced, which is conducive to the debonding and return of the acid; debonding can be done by direct water injection or by using hydrocarbon substances in the formation (generally referring to the residual oil in the formation during the oil production process after acidizing treatment).

[0067] A gel breaking experiment was conducted on the residual acid of the diverting acid 4 after the hydrochloric acid hydrogen ions were consumed. Tap water was added to the residual acid of the diverting acid 4 with an apparent viscosity of 174mPa·s. The amount of water added was calculated based on the residual acid volume to simulate the introduction of water into the formation to achieve gel breaking. The residual acid was then placed in the sample cup of a six-speed rotary viscometer and heated at 90°C, 170s -1 The apparent viscosity test results are as follows: Figure 1 As shown in the figure, it can be seen that after the volume ratio of water to residual acid is greater than 1.6, the residual acid viscosity value tends to be stable. At this time, the viscosity value is less than 10mPa·s and there is no precipitate, which proves that the residual steering acid can be degelled using a small amount of water, the treatment cost is very low, and the residual acid can be effectively discharged.

[0068] Test Example 2:

[0069] The acidification diversion agent prepared in Example 4 was tested for its structural composition by infrared spectrometer. The test results are as follows: Figure 2 As shown. Among them, the acidification diverter is at 3445cm -1 The peak at 3029cm is the OH stretching vibration peak of water absorbed in the air. -1 and 2945cm -1 The stretching vibration peak of saturated hydrocarbon CH2 appears at 1184cm -1 The stretching vibration peak of imidazole ring tertiary amine CN appeared at 1484cm -1 The peaks at 3197cm are the stretching vibration of C=N on the imidazole ring and the vibration peak of the aromatic skeleton. -1 The stretching vibration peak of NH in AM appears at 1733cm -1 and 1671cm -1 The stretching vibration peaks of C=O in AM and SPE appeared at 1034 cm -1 and 733cm -1 The SO stretching vibration peak of SPE is at 604cm -1 The position is the CS stretching vibration peak on SPE. According to the above analysis, it can be seen that the polymer acidification diverting agent prepared in Example 4 contains the initially designed groups, indicating that the diverting agent structure is consistent with the target product.

[0070] Test Example 3:

[0071] The self-assembled steering acid prepared in Example 4 was subjected to a high temperature shear test using a HAAKE MARS 60 rheometer. The steering acid 4 was first thickened to a maximum value and then heated to 160°C and 170 s. -1 Under high temperature shear conditions, the self-assembled steering acid performance of steering acid 4 after high temperature shearing for 1 hour was tested and evaluated. Please refer to Figure 3 The blue line is the shift to acid 4 with a fixed shear rate for 170 s. -1 The continuous shear line shows an almost straight line because the rate remains unchanged no matter how long the time lasts. The red line is the temperature change curve of the steering acid 4, which is heated from room temperature to 160°C, so it first increases and then stabilizes over time. The black curve shows the apparent viscosity of the steering acid 4 changing with time due to the influence of temperature and shear.

[0072] As can be seen from the figure, from about 17 to 30 minutes, the temperature of steering acid 4 was raised from 75℃ to 120℃. Due to the thermal motion of the molecules, the long chains in steering acid 4 were further entangled, resulting in an increase in macroscopic viscosity. However, as the temperature continued to rise and the shear time continued to increase, in the range of 120-160℃, steering acid 4 maintained a viscosity of 170s.-1 The rate has been sheared for 30 to 45 minutes, and the network structure of the self-assembled molecules in the polymer is destroyed, resulting in a rapid decrease in viscosity. The results show that when the acidified steering agent is added at 1wt% and the surfactant octadecyltrimethylammonium chloride is added at 0.2wt% to prepare the steering acid, the apparent viscosity remains at 70mPa·s at high temperature shearing for more than 1 hour at 160℃, proving that the self-assembled steering acid has excellent high temperature resistance and shear resistance.

[0073] The above are only preferred embodiments of the present invention. It should be noted that the above preferred embodiments should not be regarded as limiting the present invention, and the protection scope of the present invention should be based on the scope defined by the claims. For ordinary technicians in this technical field, several improvements and modifications can be made without departing from the spirit and scope of the present invention, and these improvements and modifications should also be regarded as the protection scope of the present invention.

Claims

1. An acidification diverter, characterized in that: A polymer having a structure represented by structural formula (1) is: ; Among them, the ratios of x, y, and z are (4.2~4.6):(4.8~5.4):(0.14~0.2).

2. The acidification diverter according to claim 1, characterized in that The invention is obtained by polymerization reaction of 4.2-4.6 parts of acrylamide, 4.8-5.4 parts of 3-[[2-(methacryloyloxy)ethyl]dimethylammonio]propane-1-sulfonate and 0.14-0.2 parts of 1-hexadecyl-3-vinylimidazole in molar ratio.

3. A method for preparing an acidification diverting agent, characterized in that: The following steps are involved: S1. dissolving three monomers, acrylamide, 3-[[2-(methacryloyloxy)ethyl]dimethylammonium]propane-1-sulfonate and 1-hexadecyl-3-vinylimidazole in deionized water in a nitrogen atmosphere to obtain a mixed solution; S2. The mixed solution is heated to 40-60°C and the pH value of the solution is adjusted to 7; S3. Adding an initiator to initiate the polymerization reaction for 5h to obtain a crude polymer; S4. Wash and chop the crude polymer, and vacuum dry it to obtain an acidification diverting agent.

4. The method for preparing the acidification diverting agent according to claim 3, characterized in that: The sum of the masses of the three monomers in step S1 accounts for 20-30% of the mass of the reaction system.

5. The method for preparing the acidification diverting agent according to claim 3, characterized in that: The initiator in step S3 is 2,2-azobis(2-methylpropylimidazole) dihydrochloride.

6. The method for preparing the acidification diverting agent according to claim 3, characterized in that: The mass of the initiator in step S3 accounts for 0.6% of the mass of the reaction system.

7. The method for preparing the acidification diverting agent according to claim 3, characterized in that: In step S4, anhydrous ethanol is used for washing.

8. A self-assembling steering acid, characterized in that The invention comprises 20% hydrochloric acid by mass, 1% by mass of an acidification diversion agent and 0.1-0.5% by mass of a surfactant, wherein the acidification diversion agent is the acidification diversion agent according to any one of claims 1 to 2 or the acidification diversion agent prepared by the preparation method according to any one of claims 3 to 7.

9. The self-assembling steering acid according to claim 8, characterized in that The surfactant is octadecyltrimethylammonium chloride.