Glass fiber-based composite material for rotary wheel dehumidification and preparation method of glass fiber-based composite material
Patent Information
- Application Number
- CN202411072065.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-08-06
AI Technical Summary
The existing glass fiber-based composite materials for dehumidification are insufficient in moisture absorption and mechanical properties, and the bonding strength are not high, resulting in a short service life and a health hazard caused by bacterial growth.
The composite filler and modified resin were used to prepare the glass fiber-based composite material for rotor dehumidification by impregnation. The composite filler was made of a metal organic framework as the matrix, and lithium chloride was added, and the cross-linking density and adhesiveness of the silicone were improved by the modified resin. Characteristics, combined with antibacterial properties of nanosilver.
It improves hygroscopic properties and mechanical properties, extends service life, and avoids health risks caused by bacterial growth, and enhances antibacterial ability.
Smart Images

Figure BDA0004981144680000131
Abstract
Description
Technical Field
[0001] The invention relates to the field of glass fiber-based composite materials, and in particular to a glass fiber-based composite material for a rotary dehumidification device and a preparation method thereof. Background Art
[0002] With the improvement of modern people's living standards and industrial-related requirements, the impact of air humidity on production and life is becoming more and more important. As a commonly used dehumidification device, the core component of the rotary dehumidifier is the dehumidification wheel, and most dehumidification wheels are made of a composite of activated silica gel and glass fiber.
[0003] As an adsorption material for dehumidification wheels, silica gel has the characteristics of stable properties and easy cleaning. However, silica gel as an adsorption material still has many shortcomings. For example, compared with lithium chloride, silica gel has a smaller moisture absorption capacity and lower dehumidification efficiency. On the other hand, the bonding strength between silica gel and the dehumidification wheel matrix is not high in a strong working environment or working pressure. In severe cases, the pores may collapse and the airflow may be blocked, which greatly reduces its dehumidification efficiency. At the same time, since the dehumidification wheel is in a humid environment for a long time, bacteria will inevitably breed. These bacteria are easily discharged with the dried air, posing certain health risks. Summary of the invention
[0004] The purpose of the present invention is to provide a glass fiber-based composite material for a rotary dehumidifier and a preparation method thereof, which solves the problems of the existing glass fiber-based composite materials for rotary dehumidifiers having insufficient hygroscopic properties and mechanical properties and low bonding strength with the rotary dehumidifier matrix resulting in a short service life, while also improving its antibacterial properties to avoid health hazards caused by bacterial growth.
[0005] The object of the present invention can be achieved by the following technical scheme: A method for preparing a glass fiber-based composite material for a rotary dehumidification device, comprising the following steps: Step S1: weighing the following raw materials in weight percentage: 30-35% of sodium water glass, 6-8% of modified resin, 3-5% of composite filler and 0.2-0.3% of glyoxal, with the balance being water, and mixing the sodium water glass, modified resin, composite filler, glyoxal and water to obtain a mixed solution;
[0006] Step S2: immersing the glass fiber base cloth in the mixed solution for 5-10 minutes, drying, and then immersing it in a sulfuric acid solution at a temperature of 50° C. for 4-5 hours, the pH value of the sulfuric acid solution is 6, washing, and drying to obtain a glass fiber-based composite material for a rotary dehumidification wheel;
[0007] The composite filler is prepared by the following steps:
[0008] Step A1: p-bromotoluene and ether are mixed, stirred at a stirring rate of 80-100 rpm and a temperature of 5°C, and n-butyl lithium is added, stirred for 2-3 hours, the temperature is raised to room temperature, trichlorosilane is added, and the reaction is carried out for 12 hours to obtain intermediate 1; intermediate 1, 3-vinylimidazole and tetrahydrofuran are mixed, stirred at a stirring rate of 120-150 rpm and a temperature of 90°C, and a Custer catalyst is added, and the reaction is carried out for 3-4 hours to obtain intermediate 2;
[0009] The dosage ratio of p-bromotoluene, n-butyl lithium and trichlorosilane is 0.02-0.022 mol: 8-10 mL: 0.005-0.006 mol, and the dosage ratio of intermediate 1, 3-vinylimidazole and Custer catalyst is 0.005-0.006 mol: 0.007-0.008 mol: 0.3-0.4 g;
[0010] During the reaction, under the action of n-butyl lithium as an initiator, trichlorosilane is first lithiated and then reacts with p-bromotoluene to form a carbon-silicon bond to obtain intermediate 1. Then, under the action of Custer's catalyst, the silicon-hydrogen bond in intermediate 1 reacts with the alkenyl group in 3-vinylimidazole to undergo a silylation reaction to obtain intermediate 2.
[0011] Step A2: Mix intermediate 2, pyridine and deionized water, stir at a stirring rate of 80-120 rpm and a temperature of 80°C, add potassium permanganate, and react for 4-5 hours to obtain intermediate 3; mix intermediate 3, zirconium hydroxide, acetic acid and deionized water, stir at a stirring rate of 150-180 rpm and a temperature of 95°C, react for 12-14 hours, filter, and dry to obtain precursor 1;
[0012] The dosage ratio of intermediate 2, pyridine, deionized water and potassium permanganate is 0.009-0.01 mol: 110-130 mL: 40 mL: 25-28 g, and the dosage ratio of intermediate 3, zirconium hydroxide, acetic acid and deionized water is 0.009-0.01 mol: 2.8-3 g: 300 mL: 200 mL;
[0013] During the reaction, pyridine and deionized water are used as solvents and potassium permanganate is used as a catalyst to oxidize the methyl group in the benzyl group in the intermediate 2 to a carboxyl group to obtain the intermediate 3. Then, a precursor 1 having a metal organic framework structure is obtained by a solvothermal method with zirconium hydroxide as a zirconium source and the intermediate 3 as a ligand.
[0014] Step A3: Precursor 1, 1,4-butanesultone and acetone are mixed, and reacted for 24 hours at a stirring rate of 120-150 rpm and a temperature of 40° C. to obtain precursor 2, and precursor 2 is mixed with lithium chloride solution, and allowed to stand at room temperature for 12 hours, and dried to obtain a composite filler;
[0015] The amount ratio of precursor 1, 1,4-butane sultone and acetone is 3.5-3.8 g: 0.008-0.01 mol: 100-120 mL, the mass fraction of lithium chloride solution is 15%, and the amount ratio of precursor 2 and lithium chloride solution is 3.5-3.8 g: 10-12 mL;
[0016] During the reaction, in an acetone solvent, 1,4-butane sultone is ring-opened and reacts with the pyridine group in the precursor 1 to form a quaternary ammonium structure to obtain the precursor 2, and then lithium chloride is loaded in the precursor 2 by an impregnation method to obtain a composite filler;
[0017] The modified resin is prepared by the following steps:
[0018] Step B1: polyvinyl alcohol, p-toluenesulfonic acid and dimethyl sulfoxide are mixed, stirred at a stirring rate of 200-240 rpm and a temperature of 60° C., and vanillin is added, reacted for 2-3 hours, and then glycidyl methacrylate and 4-dimethylaminopyridine are added, and the reaction is continued for 6-8 hours to obtain modified polyvinyl alcohol;
[0019] The amount ratio of polyvinyl alcohol, p-toluenesulfonic acid, dimethyl sulfoxide, vanillin, glycidyl methacrylate and 4-dimethylaminopyridine is 3-3.4 g: 0.08-0.1 g: 30-35 mL: 0.018-0.02 mol: 0.018-0.02 mol: 0.08-0.1 g;
[0020] During the reaction, the aldehyde group in vanillin reacts with the hydroxyl group in polyvinyl alcohol to form an acetal reaction, thereby introducing a phenolic hydroxyl group. The phenolic hydroxyl group then reacts with the epoxy group in glycidyl methacrylate to introduce a double bond, thereby obtaining modified polyvinyl alcohol.
[0021] Step B2: β-cyclodextrin and deionized water are mixed, stirred at a stirring rate of 50-60 rpm and room temperature, and silver nitrate solution is added, stirred for 2-3 hours, and then sodium hydroxide solution is added to adjust the pH value to 10, and the reaction is carried out for 3-4 hours to obtain precursor a. Precursor a, 2-mercaptopropionic acid and deionized water are mixed, stirred at a rate of 120-150 rpm and a temperature of 40° C., and the reaction is carried out for 3-4 hours to obtain precursor b;
[0022] The molar concentration of the silver nitrate solution is 0.01 mol / L, the molar concentration of the sodium hydroxide solution is 1 mol / L, the dosage ratio of β-cyclodextrin to the silver nitrate solution is 11-12 g: 5-6 mL, and the dosage ratio of the precursor a to 2-mercaptopropionic acid is 0.3-0.4 g: 0.003-0.0035 mol;
[0023] During the reaction, β-cyclodextrin was used as a reducing agent and a stabilizer, and an in-situ reduction method was used under alkaline conditions to obtain a precursor a in which nanosilver was wrapped with β-cyclodextrin. Then, through the inclusion capacity of β-cyclodextrin in the precursor a, 2-mercaptopropionic acid was included in the inner cavity of β-cyclodextrin to obtain a precursor b.
[0024] Step B3: Mix the modified polyvinyl alcohol, precursor b and deionized water, under nitrogen protection, ultraviolet irradiation, stirring rate of 120-150rpm, at room temperature, stir and add 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone, react for 10-15min to obtain composite polyvinyl alcohol, mix the composite polyvinyl alcohol, 3-glycidyloxypropyltrimethoxysilane and N,N-dimethylformamide, under nitrogen protection, stirring rate of 120-150rpm, temperature of 90°C, react for 4-5h to obtain a modified resin;
[0025] The amount ratio of modified polyvinyl alcohol, precursor b and 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone is 3.2-3.5g: 0.08-0.1g: 0.03g, and the amount ratio of composite polyvinyl alcohol and 3-glycidyloxypropyltrimethoxysilane is 3.2-3.5g: 0.8-1g;
[0026] During the reaction, under the action of the initiator 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone, the double bonds in the modified polyvinyl alcohol and the thiol groups in the precursor b undergo a click reaction, and the precursor b is connected to the modified polyvinyl alcohol to obtain a composite polyvinyl alcohol. The hydroxyl groups in the composite polyvinyl alcohol then react with the epoxy groups in 3-glycidyloxypropyltrimethoxysilane to obtain a modified resin.
[0027] Beneficial effects of the invention: The invention discloses a glass fiber-based composite material for a rotary dehumidifier and a preparation method thereof. The invention solves the problems of insufficient hygroscopic performance and mechanical performance of the existing glass fiber-based composite material for a rotary dehumidifier and a short service life due to low bonding strength with the rotary dehumidifier matrix by adding a composite filler and a modified resin into the silica gel preparation raw material. The invention also improves its antibacterial performance to avoid health hazards caused by bacterial growth. Since the composite filler is based on a metal organic skeleton and is impregnated with lithium chloride by an impregnation method, and since the metal organic skeleton itself is a special porous structure, and its metal element is zirconium and pyridine and sulfonic acid groups are introduced at the same time, the metal organic skeleton itself has good water adsorption performance, and the lithium chloride impregnated in the metal organic skeleton has a large water absorption capacity. The combination of the composite filler has excellent water absorption performance. At the same time, the special structure of the metal organic skeleton avoids the health hazards of the rotary dehumidifier. The overflow of lithium chloride during the wet regeneration process, and the modified resin is based on polyvinyl alcohol and connected with precursor b and 3-glycidyloxypropyltrimethoxysilane. In the gel process of sodium water glass, the methoxy group in 3-glycidyloxypropyltrimethoxysilane will also be hydrolyzed, so that the modified resin can participate in the formation of silica gel on the glass fiber base cloth. Since polyvinyl alcohol has certain adhesive properties after hydroformylation, the bonding ability between silica gel and glass fiber base cloth is improved to a certain extent. At the same time, due to the introduction of glyoxal as a cross-linking agent, glyoxal can react with the active hydroxyl groups in the modified resin to increase the cross-linking density of silica gel, thereby improving the mechanical properties of silica gel itself. Since precursor b is based on nanosilver as the core and the surface is β-cyclodextrin, and the special external hydrophilic and internal hydrophobic structure of cyclodextrin avoids its influence on the water absorption performance of silica gel itself, and also enables nanosilver and quaternary ammonium groups to synergistically exert good antibacterial ability. DETAILED DESCRIPTION
[0028] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0029] Embodiment 1 A method for preparing a glass fiber-based composite material for a rotary dehumidification device comprises the following steps: Step S1: weigh the following raw materials in weight percentage: 30% of commercially available Narmei sodium water glass, 6% of modified resin, 3% of composite filler and 0.3% of glyoxal, and the balance is water, and mix the sodium water glass, modified resin, composite filler, glyoxal and water to obtain a mixed solution;
[0030] Step S2: immersing the commercially available Haozheng glass fiber base cloth in the mixed solution for 5 minutes, drying, and then immersing it in a sulfuric acid solution at a temperature of 50°C for 5 hours, the pH of the sulfuric acid solution is 6, washing, and drying to obtain a glass fiber-based composite material for rotary dehumidification;
[0031] The composite filler is prepared by the following steps:
[0032] Step A1: p-bromotoluene and ether are mixed, stirred at a stirring rate of 80 rpm and a temperature of 5°C, and n-butyl lithium is added, stirred for 2 hours, the temperature is raised to room temperature, trichlorosilane is added, and the reaction is carried out for 12 hours to obtain intermediate 1; intermediate 1, 3-vinylimidazole and tetrahydrofuran are mixed, stirred at a stirring rate of 120 rpm and a temperature of 90°C, and Custer catalyst is added, and the reaction is carried out for 3 hours to obtain intermediate 2;
[0033] The ratio of p-bromotoluene, n-butyl lithium and trichlorosilane is 0.02 mol: 8 mL: 0.005 mol, and the ratio of intermediate 1, 3-vinylimidazole and Custer catalyst is 0.005 mol: 0.007 mol: 0.3 g;
[0034] Step A2: Mix intermediate 2, pyridine and deionized water, stir at a stirring rate of 80 rpm and a temperature of 80°C, add potassium permanganate, and react for 4 hours to obtain intermediate 3; mix intermediate 3, zirconium hydroxide, acetic acid and deionized water, stir at a stirring rate of 150 rpm and a temperature of 95°C, react for 12 hours, filter, and dry to obtain precursor 1;
[0035] The usage ratio of intermediate 2, pyridine, deionized water and potassium permanganate is 0.009 mol: 110 mL: 40 mL: 25 g, and the usage ratio of intermediate 3, zirconium hydroxide, acetic acid and deionized water is 0.009 mol: 2.8 g: 300 mL: 200 mL;
[0036] Step A3: Precursor 1, 1,4-butanesultone and acetone were mixed, and the mixture was reacted for 24 hours at a stirring rate of 120 rpm and a temperature of 40° C. to obtain precursor 2. Precursor 2 was mixed with lithium chloride solution, and the mixture was allowed to stand at room temperature for 12 hours, and then dried to obtain a composite filler.
[0037] The amount ratio of precursor 1, 1,4-butane sultone and acetone is 3.5g:0.008-0.01mol:100mL, the mass fraction of lithium chloride solution is 15%, and the amount ratio of precursor 2 and lithium chloride solution is 3.5g:10mL;
[0038] The modified resin is prepared by the following steps:
[0039] Step B1: commercially available Newbridge 2500 polyvinyl alcohol, p-toluenesulfonic acid and dimethyl sulfoxide were mixed, stirred at a stirring rate of 200 rpm and a temperature of 60°C, and vanillin was added, reacted for 2 hours, and then glycidyl methacrylate and 4-dimethylaminopyridine were added, and the reaction was continued for 6 hours to obtain modified polyvinyl alcohol;
[0040] The amount ratio of polyvinyl alcohol, p-toluenesulfonic acid, dimethyl sulfoxide, vanillin, glycidyl methacrylate and 4-dimethylaminopyridine is 3g:0.08g:30mL:0.018mol:0.018mol:0.08g;
[0041] Step B2: β-cyclodextrin and deionized water were mixed, stirred at a stirring rate of 50 rpm and room temperature, and silver nitrate solution was added, stirred for 2-3 hours, and then sodium hydroxide solution was added to adjust the pH value to 10, and the reaction was carried out for 3 hours to obtain precursor a. Precursor a, 2-mercaptopropionic acid and deionized water were mixed, stirred at a stirring rate of 120 rpm and a temperature of 40°C, and the reaction was carried out for 3 hours to obtain precursor b;
[0042] The molar concentration of the silver nitrate solution is 0.01 mol / L, the molar concentration of the sodium hydroxide solution is 1 mol / L, the dosage ratio of β-cyclodextrin to the silver nitrate solution is 11 g:5 mL, and the dosage ratio of the precursor a to 2-mercaptopropionic acid is 0.3 g:0.003 mol;
[0043] Step B3: Mix the modified polyvinyl alcohol, precursor b and deionized water, stir and add 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone under nitrogen protection, ultraviolet irradiation, stirring rate of 120 rpm, room temperature, and react for 10 minutes to obtain composite polyvinyl alcohol, mix the composite polyvinyl alcohol, 3-glycidyloxypropyltrimethoxysilane and N,N-dimethylformamide, and react for 4 hours under nitrogen protection, stirring rate of 120 rpm, and temperature of 90°C to obtain a modified resin;
[0044] The amount ratio of modified polyvinyl alcohol, precursor b and 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone is 3.2g:0.08g:0.03g, and the amount ratio of composite polyvinyl alcohol and 3-glycidyloxypropyltrimethoxysilane is 3.2g:0.8g.
[0045] Embodiment 2 A method for preparing a glass fiber-based composite material for a rotary dehumidification device comprises the following steps: Step S1: Weigh the following raw materials in weight percentage: 35% of commercially available Narmei sodium water glass, 6% of modified resin, 5% of composite filler and 0.2% of glyoxal, and the balance is water, and mix the sodium water glass, modified resin, composite filler, glyoxal and water to obtain a mixed solution;
[0046] Step S2: immersing the commercially available Haozheng glass fiber base cloth in the mixed solution for 5 minutes, drying, and then immersing it in a sulfuric acid solution at a temperature of 50°C for 4 hours, the pH of the sulfuric acid solution is 6, washing, and drying to obtain a glass fiber-based composite material for rotary dehumidification;
[0047] The composite filler is prepared by the following steps:
[0048] Step A1: p-bromotoluene and ether are mixed, stirred at a stirring rate of 100 rpm and a temperature of 5°C, and n-butyl lithium is added, stirred for 2 hours, the temperature is raised to room temperature, trichlorosilane is added, and the reaction is carried out for 12 hours to obtain intermediate 1; intermediate 1, 3-vinylimidazole and tetrahydrofuran are mixed, stirred at a stirring rate of 150 rpm and a temperature of 90°C, and a Custer catalyst is added, and the reaction is carried out for 3 hours to obtain intermediate 2;
[0049] The ratio of p-bromotoluene, n-butyl lithium and trichlorosilane is 0.02 mol: 10 mL: 0.006 mol, and the ratio of intermediate 1, 3-vinylimidazole and Custer catalyst is 0.006 mol: 0.007 mol: 0.3 g;
[0050] Step A2: Mix intermediate 2, pyridine and deionized water, stir at a stirring rate of 120 rpm and a temperature of 80°C, add potassium permanganate, and react for 4 hours to obtain intermediate 3; mix intermediate 3, zirconium hydroxide, acetic acid and deionized water, stir at a stirring rate of 180 rpm and a temperature of 95°C, react for 12 hours, filter, and dry to obtain precursor 1;
[0051] The usage ratio of intermediate 2, pyridine, deionized water and potassium permanganate is 0.01 mol: 110 mL: 40 mL: 28 g, and the usage ratio of intermediate 3, zirconium hydroxide, acetic acid and deionized water is 0.01 mol: 2.8 g: 300 mL: 200 mL;
[0052] Step A3: Precursor 1, 1,4-butanesultone and acetone were mixed, and the mixture was reacted for 24 hours at a stirring rate of 120 rpm and a temperature of 40° C. to obtain precursor 2. Precursor 2 was mixed with lithium chloride solution, and the mixture was allowed to stand at room temperature for 12 hours, and then dried to obtain a composite filler.
[0053] The amount ratio of precursor 1, 1,4-butane sultone and acetone is 3.8g:0.008mol:120mL, the mass fraction of lithium chloride solution is 15%, and the amount ratio of precursor 2 and lithium chloride solution is 3.5g:12mL;
[0054] The modified resin is prepared by the following steps:
[0055] Step B1: commercially available Newbridge 2500 polyvinyl alcohol, p-toluenesulfonic acid and dimethyl sulfoxide were mixed, stirred at a stirring rate of 240 rpm and a temperature of 60°C, and vanillin was added, reacted for 2 hours, and then glycidyl methacrylate and 4-dimethylaminopyridine were added, and the reaction was continued for 8 hours to obtain modified polyvinyl alcohol;
[0056] The amount ratio of polyvinyl alcohol, p-toluenesulfonic acid, dimethyl sulfoxide, vanillin, glycidyl methacrylate and 4-dimethylaminopyridine is 3.4 g: 0.08 g: 30 mL: 0.02 mol: 0.018 mol: 0.1 g;
[0057] Step B2: β-cyclodextrin and deionized water were mixed, stirred at a stirring rate of 50 rpm and room temperature, and silver nitrate solution was added, stirred for 3 hours, and then sodium hydroxide solution was added to adjust the pH value to 10, and the reaction was carried out for 4 hours to obtain precursor a. Precursor a, 2-mercaptopropionic acid and deionized water were mixed, stirred at a stirring rate of 150 rpm and a temperature of 40° C., and the reaction was carried out for 3 hours to obtain precursor b;
[0058] The molar concentration of the silver nitrate solution is 0.01 mol / L, the molar concentration of the sodium hydroxide solution is 1 mol / L, the dosage ratio of β-cyclodextrin to the silver nitrate solution is 12 g:5 mL, and the dosage ratio of the precursor a to 2-mercaptopropionic acid is 0.4 g:0.003 mol;
[0059] Step B3: Mix the modified polyvinyl alcohol, precursor b and deionized water, stir and add 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone under nitrogen protection, ultraviolet irradiation, stirring rate of 150 rpm, room temperature, and react for 10 minutes to obtain composite polyvinyl alcohol; mix the composite polyvinyl alcohol, 3-glycidyloxypropyltrimethoxysilane and N,N-dimethylformamide, and react for 4 hours under nitrogen protection, stirring rate of 150 rpm, and temperature of 90°C to obtain a modified resin;
[0060] The amount ratio of modified polyvinyl alcohol, precursor b and 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone is 3.5g:0.08g:0.03g, and the amount ratio of composite polyvinyl alcohol and 3-glycidyloxypropyltrimethoxysilane is 3.5g:0.8g;
[0061] Embodiment 3 A method for preparing a glass fiber-based composite material for a rotary dehumidification device comprises the following steps: Step S1: Weigh the following raw materials in weight percentage: 35% of commercially available Narmei sodium water glass, 8% of modified resin, 5% of composite filler and 0.3% of glyoxal, and the balance is water, and mix the sodium water glass, modified resin, composite filler, glyoxal and water to obtain a mixed solution;
[0062] Step S2: immersing the commercially available Haozheng glass fiber base cloth in the mixed solution for 10 minutes, drying, and then immersing it in a sulfuric acid solution at a temperature of 50° C. for 5 hours, the pH of the sulfuric acid solution is 6, washing, and drying to obtain a glass fiber-based composite material for rotary dehumidification;
[0063] The composite filler is prepared by the following steps:
[0064] Step A1: p-bromotoluene and ether are mixed, stirred at a stirring rate of 100 rpm and a temperature of 5°C, and n-butyl lithium is added, stirred for 3 hours, the temperature is raised to room temperature, trichlorosilane is added, and the reaction is carried out for 12 hours to obtain intermediate 1; intermediate 1, 3-vinylimidazole and tetrahydrofuran are mixed, stirred at a stirring rate of 150 rpm and a temperature of 90°C, and a Custer catalyst is added, and the reaction is carried out for 4 hours to obtain intermediate 2;
[0065] The ratio of p-bromotoluene, n-butyl lithium and trichlorosilane is 0.022 mol: 10 mL: 0.006 mol, and the ratio of intermediate 1, 3-vinylimidazole and Custer catalyst is 0.006 mol: 0.008 mol: 0.4 g;
[0066] Step A2: Mix intermediate 2, pyridine and deionized water, stir at a stirring rate of 120 rpm and a temperature of 80°C, add potassium permanganate, and react for 5 hours to obtain intermediate 3; mix intermediate 3, zirconium hydroxide, acetic acid and deionized water, stir at a stirring rate of 180 rpm and a temperature of 95°C, react for 14 hours, filter, and dry to obtain precursor 1;
[0067] The usage ratio of intermediate 2, pyridine, deionized water and potassium permanganate is 0.01 mol: 130 mL: 40 mL: 28 g, and the usage ratio of intermediate 3, zirconium hydroxide, acetic acid and deionized water is 0.01 mol: 3 g: 300 mL: 200 mL;
[0068] Step A3: Precursor 1, 1,4-butanesultone and acetone were mixed, and the mixture was reacted for 24 hours at a stirring rate of 150 rpm and a temperature of 40° C. to obtain precursor 2. Precursor 2 was mixed with lithium chloride solution, and the mixture was allowed to stand at room temperature for 12 hours, and then dried to obtain a composite filler.
[0069] The amount ratio of precursor 1, 1,4-butanesultone and acetone is 3.8g:0.01mol:120mL, the mass fraction of lithium chloride solution is 15%, and the amount ratio of precursor 2 and lithium chloride solution is 3.8g:12mL;
[0070] The modified resin is prepared by the following steps:
[0071] Step B1: commercially available Newbridge 2500 polyvinyl alcohol, p-toluenesulfonic acid and dimethyl sulfoxide were mixed, stirred at a stirring rate of 240 rpm and a temperature of 60°C, and vanillin was added, reacted for 3 hours, and then glycidyl methacrylate and 4-dimethylaminopyridine were added, and the reaction was continued for 8 hours to obtain modified polyvinyl alcohol;
[0072] The amount ratio of polyvinyl alcohol, p-toluenesulfonic acid, dimethyl sulfoxide, vanillin, glycidyl methacrylate and 4-dimethylaminopyridine is 3.4 g: 0.1 g: 35 mL: 0.02 mol: 0.02 mol: 0.1 g;
[0073] Step B2: β-cyclodextrin and deionized water were mixed, stirred at a stirring rate of 60 rpm and room temperature, and silver nitrate solution was added, stirred for 3 hours, and then sodium hydroxide solution was added to adjust the pH value to 10, and the reaction was carried out for 4 hours to obtain precursor a. Precursor a, 2-mercaptopropionic acid and deionized water were mixed, stirred at a rate of 120-150 rpm and a temperature of 40° C., and the reaction was carried out for 4 hours to obtain precursor b;
[0074] The molar concentration of the silver nitrate solution is 0.01 mol / L, the molar concentration of the sodium hydroxide solution is 1 mol / L, the dosage ratio of β-cyclodextrin to the silver nitrate solution is 12 g: 6 mL, and the dosage ratio of the precursor a to 2-mercaptopropionic acid is 0.4 g: 0.0035 mol;
[0075] Step B3: Mix the modified polyvinyl alcohol, precursor b and deionized water, stir and add 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone under nitrogen protection, ultraviolet irradiation, stirring rate of 150 rpm, room temperature, and react for 15 minutes to obtain composite polyvinyl alcohol; mix the composite polyvinyl alcohol, 3-glycidyloxypropyltrimethoxysilane and N,N-dimethylformamide, and react for 5 hours under nitrogen protection, stirring rate of 150 rpm, and temperature of 90°C to obtain a modified resin;
[0076] The amount ratio of modified polyvinyl alcohol, precursor b and 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone is 3.5g:0.1g:0.03g, and the amount ratio of composite polyvinyl alcohol and 3-glycidyloxypropyltrimethoxysilane is 3.5g:1g.
[0077] Comparative Example 1 Compared with Example 3, this comparative example is to remove 1,4-butanesultone in the preparation process of the composite filler in Example 3, and the other steps are the same.
[0078] Comparative Example 2 Compared with Example 3, this comparative example is to remove the lithium chloride solution in the process of preparing the composite filler in Example 3, and the other steps are the same.
[0079] Comparative Example 3 Compared with Example 3, this comparative example is characterized in that the precursor b in the modified resin preparation process of Example 3 is replaced by nanosilver, and the other steps are the same.
[0080] Comparative Example 4 This comparative example is compared with Example 3, except that 3-glycidyloxypropyltrimethoxysilane in the preparation process of the modified resin in Example 3 is replaced by isopropyl glycidyl ether, and the other steps are the same.
[0081] Take the glass fiber-based composite materials for rotary dehumidification prepared in Example 1, Example 2, Example 3, Comparative Example 1, Comparative Example 2, Comparative Example 3 and Comparative Example 4, cut them into samples of the same size, and test their adsorption capacity under the conditions of room temperature, humidity of 90%, and adsorption time of 1h. Then, under the conditions of temperature of 100°C and desorption time of 2h, calculate the desorption rate. Under the conditions of room temperature, humidity of 90%, adsorption time of 4h, temperature of 100°C, and desorption time of 2h, the samples were subjected to cyclic adsorption and desorption experiments for 28 cycles, and then the adsorption performance retention rate and desorption performance retention rate were calculated to evaluate their service life. The antibacterial performance was tested by oscillation method. The test results are shown in Table 1 below:
[0082] Table 1 Test results
[0083]
[0084] It can be seen from the test results in the table shown that Example 1, Example 2 and Example 3 are compared with Comparative Example 1, Comparative Example 2, Comparative Example 3 and Comparative Example 4. Comparative Example 1 removes 1,4-butanesulfonic acid lactone during the preparation of the composite filler in Example 3. Due to the lack of sulfonic acid groups and quaternary ammonium groups, its water absorption capacity and antibacterial ability decrease to a certain extent. Comparative Example 2 removes the lithium chloride solution during the preparation of the composite filler in Example 3. Due to the lack of lithium chloride impregnation, its water absorption capacity decreases significantly. Comparative Example 3 replaces the precursor b with nanosilver during the preparation of the modified resin in Example 3. Due to the lack of cyclodextrin encapsulation, its antibacterial performance decreases significantly. Comparative Example 4 replaces 3-glycidyloxypropyltrimethoxysilane with isopropyl glycidyl ether during the preparation of the modified resin in Example 3. Due to the lack of silicon methoxy groups, its binding ability and mechanical properties decrease to a certain extent, thereby affecting its service life.
[0085] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0086] The above contents are merely examples and explanations of the concept of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the concept of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.
Claims
1. A method for preparing a glass fiber-based composite material for a rotary dehumidification machine. Features: The method comprises the following steps: Step S1: weighing the following raw materials in weight percentage: 30-35% of sodium water glass, 6-8% of modified resin, 3-5% of composite filler and 0.2-0.3% of glyoxal, with the balance being water, and mixing the sodium water glass, modified resin, composite filler, glyoxal and water to prepare a mixed solution; Step S2: immerse the glass fiber base cloth in the mixed solution for 5-10 minutes, dry it, and then immerse it in a sulfuric acid solution at a temperature of 50°C for 4-5 hours, the pH value of the sulfuric acid solution is 6, wash it, and dry it to obtain a glass fiber-based composite material for rotary dehumidification.
2. A method for preparing a glass fiber-based composite material for a rotary dehumidification according to claim 1, Features: The composite filler is prepared by the following steps: Step A1: p-bromotoluene and ether are mixed, stirred at a stirring rate of 80-100 rpm and a temperature of 5°C, and n-butyl lithium is added, stirred for 2-3 hours, the temperature is raised to room temperature, trichlorosilane is added, and the reaction is carried out for 12 hours to obtain intermediate 1; intermediate 1, 3-vinylimidazole and tetrahydrofuran are mixed, stirred at a stirring rate of 120-150 rpm and a temperature of 90°C, and a Custer catalyst is added, and the reaction is carried out for 3-4 hours to obtain intermediate 2; Step A2: Mix intermediate 2, pyridine and deionized water, stir at a stirring rate of 80-120 rpm and a temperature of 80°C, add potassium permanganate, and react for 4-5 hours to obtain intermediate 3; mix intermediate 3, zirconium hydroxide, acetic acid and deionized water, stir at a stirring rate of 150-180 rpm and a temperature of 95°C, react for 12-14 hours, filter, and dry to obtain precursor 1; Step A3: Precursor 1, 1,4-butanesulfonate and acetone are mixed, and reacted for 24 hours at a stirring rate of 120-150 rpm and a temperature of 40°C to obtain precursor 2. Precursor 2 is mixed with lithium chloride solution, and allowed to stand at room temperature for 12 hours, and then dried to obtain a composite filler.
3. A method for preparing a glass fiber-based composite material for a rotary dehumidification according to claim 2, Features: In step A1, the ratio of p-bromotoluene, n-butyl lithium and trichlorosilane is 0.02-0.022 mol: 8-10 mL: 0.005-0.006 mol, and the ratio of intermediate 1, 3-vinylimidazole and Custer catalyst is 0.005-0.006 mol: 0.007-0.008 mol: 0.3-0.4 g.
4. The method for preparing a glass fiber-based composite material for a rotary dehumidification according to claim 2, Features: In step A2: the usage ratio of intermediate 2, pyridine, deionized water and potassium permanganate is 0.009-0.01 mol: 110-130 mL: 40 mL: 25-28 g, and the usage ratio of intermediate 3, zirconium hydroxide, acetic acid and deionized water is 0.009-0.01 mol: 2.8-3 g: 300 mL: 200 mL.
5. The method for preparing a glass fiber-based composite material for a rotary dehumidification wheel according to claim 2, Features: In step A3: the amount ratio of precursor 1, 1,4-butanesultone and acetone is 3.5-3.8 g: 0.008-0.01 mol: 100-120 mL, the mass fraction of lithium chloride solution is 15%, and the amount ratio of precursor 2 and lithium chloride solution is 3.5-3.8 g: 10-12 mL.
6. The method for preparing a glass fiber-based composite material for a rotary dehumidification wheel according to claim 1, Features: The modified resin is prepared by the following steps: Step B1: polyvinyl alcohol, p-toluenesulfonic acid and dimethyl sulfoxide are mixed, stirred at a stirring rate of 200-240 rpm and a temperature of 60° C., and vanillin is added, reacted for 2-3 hours, and then glycidyl methacrylate and 4-dimethylaminopyridine are added, and the reaction is continued for 6-8 hours to obtain modified polyvinyl alcohol; Step B2: β-cyclodextrin and deionized water are mixed, stirred at a stirring rate of 50-60 rpm and room temperature, and silver nitrate solution is added, stirred for 2-3 hours, and then sodium hydroxide solution is added to adjust the pH value to 10, and the reaction is carried out for 3-4 hours to obtain precursor a. Precursor a, 2-mercaptopropionic acid and deionized water are mixed, stirred at a rate of 120-150 rpm and a temperature of 40° C., and the reaction is carried out for 3-4 hours to obtain precursor b; Step B3: Mix the modified polyvinyl alcohol, precursor b and deionized water, stir and add 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone under nitrogen protection, ultraviolet irradiation, stirring rate of 120-150rpm, room temperature, and react for 10-15min to obtain composite polyvinyl alcohol; mix the composite polyvinyl alcohol, 3-glycidyloxypropyltrimethoxysilane and N,N-dimethylformamide, under nitrogen protection, stirring rate of 120-150rpm, temperature of 90°C, and react for 4-5h to obtain a modified resin.
7. The method for preparing a glass fiber-based composite material for a rotary dehumidification wheel according to claim 6, Features: In step B1, the amount ratio of polyvinyl alcohol, p-toluenesulfonic acid, dimethyl sulfoxide, vanillin, glycidyl methacrylate and 4-dimethylaminopyridine is 3-3.4 g: 0.08-0.1 g: 30-35 mL: 0.018-0.02 mol: 0.018-0.02 mol: 0.08-0.1 g.
8. The method for preparing a glass fiber-based composite material for a rotary dehumidification wheel according to claim 6, Features: In step B2: the molar concentration of the silver nitrate solution is 0.01 mol / L, the molar concentration of the sodium hydroxide solution is 1 mol / L, the dosage ratio of β-cyclodextrin and the silver nitrate solution is 11-12 g: 5-6 mL, and the dosage ratio of the precursor a and 2-mercaptopropionic acid is 0.3-0.4 g: 0.003-0.0035 mol.
9. The method for preparing a glass fiber-based composite material for a rotary dehumidification wheel according to claim 6, Features: In step B3: the ratio of modified polyvinyl alcohol, precursor b and 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone is 3.2-3.5g:0.08-0.1g:0.03g, and the ratio of composite polyvinyl alcohol and 3-glycidyloxypropyltrimethoxysilane is 3.2-3.5g:0.8-1g.
10. A glass fiber-based composite material for a rotary dehumidification device, Features: Prepared according to any one of claims 1 to 9.
Citation Information
Patent Citations
Antibacterial wear-resistant polyamide fiber and preparation method thereof
CN118422369A
Sustained-release antibacterial film and preparation method thereof
US20240199826A1