Polyimide film for preparing super-thick graphite film, preparation method and application

By adopting a multi-layer composite film structure and specific processing steps, an ultra-thick graphite film was prepared, which solved the problems of insufficient thickness and easy defects in the existing graphite film, and achieved high thermal conductivity and high flexibility.

CN118895010APending Publication Date: 2024-11-05ANHUI GUOFENG PLASTIC +1
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411022437.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

The PI base graphite film on the existing market is thinner in thickness, which is difficult to meet the high heat dissipation needs. It is easy to cause bubbles inside the film when the thickness is increased, resulting in graphite film defects.

Method used

A polyimide film with a multi-layer composite membrane structure is used to prepare composite particles by mixing inorganic additives with polyamic acid resin, and a gel with an A-B-A structure is formed by stirring, heating, filtration, vacuum drying, grinding and other steps. The film was then subjected to longitudinal, transverse stretching and thermal imidation treatment, and finally carbonization and graphitization under vacuum and argon protection to prepare an ultra-thick graphite film.

Benefits of technology

The preparation of an ultra-thick graphite film is achieved, which avoids defects caused by bubbles in a single layer of film, improves the integrity and flexibility of sintering, and meets the needs of high thermal conductivity and high flexibility.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention belongs to the technical field of polyimide film materials, and particularly relates to a polyimide film for preparing an ultra-thick graphite film, a preparation method and application. The polyimide graphite film is a multi-layer composite film and is of an A-B-A type structure, and the polyimide graphite film is prepared from the following raw materials: a film A: 100 parts of polyamide acid resin a and 0.05-1 part of composite particles; the film B comprises the following components in parts by weight: 100 parts of polyamide acid resin b and 0.05-1 part of composite particles; the preparation method of the composite particles comprises the following steps: adding an inorganic auxiliary agent into polyimide powder, uniformly stirring, adding a tertiary amine compound catalyst, heating, stirring, filtering, washing, carrying out vacuum drying, and grinding to obtain the composite particles. The PI powder prepared from inorganic particles is used as the foaming aid, so that the compatibility of the polyamide acid resin and the inorganic aid is improved, the dispersion uniformity of the foaming aid in the resin is ensured, the coagulation phenomenon caused by high density of the inorganic aid is avoided, the foaming stability and uniformity in the film sintering process are improved, and the foaming performance of the film is improved. The graphite film has high flexibility and few crystal points.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of polyimide film materials, and in particular relates to a polyimide film for preparing an ultra-thick graphite film, a preparation method and an application thereof. Background Art

[0002] With the rapid development of 5G technology, electronic equipment such as smart phones, flat panel displays, and notebooks are becoming lighter, more compact, and more efficient. A large amount of heat will be generated and accumulated during their high-frequency and high-speed operation. If the heat cannot be discharged in time, it will seriously affect the working stability and service life of electronic components. As an important part of thermal solutions, the demand for heat dissipation materials is also increasing, especially heat dissipation materials with light weight and high thermal conductivity. Traditional metal heat dissipation materials have disadvantages such as high density, high thermal expansion coefficient, and low thermal conductivity, and it is difficult to meet the increasingly stringent heat dissipation requirements. Graphite has excellent properties such as light weight, high thermal conductivity, and easy processing and molding, making it the first choice for heat dissipation materials.

[0003] Graphite can be made by carbonizing polyimide (PI) under vacuum conditions at 1200-1300℃ and then subjecting it to high-temperature graphitization at 2800-3200℃. The product has a highly preferentially oriented graphite layer along the film surface similar to highly oriented pyrolytic graphite, and has high crystallinity. This method has a simpler preparation process than the pyrolysis method for preparing graphite, and is low in cost. It has greatly promoted the development of graphite as a heat dissipation material, and has also greatly promoted the further development of electronic and microelectronic devices towards miniaturization, integration, high capacity and ultra-thinness.

[0004] The thickness of PI-based graphite films on the market is relatively thin, mostly below 50μm. When used in components with large heat dissipation, graphite films are often laminated in multiple layers to achieve a specified thickness in order to obtain the desired heat dissipation effect. This method is time-consuming and labor-intensive, and the laminated graphite films have poor heat storage effects. Limited by current production equipment, most PI film manufacturers can only produce PI films with a thickness of less than 75μm for the preparation of graphite films. If the thickness is increased further, a large number of bubbles will be generated inside the film, causing defects in the graphite film. This has led to an increasing market demand for thick graphite films. Summary of the invention

[0005] In view of the deficiencies in the prior art, the present invention proposes a polyimide film for preparing an ultra-thick graphite film, a preparation method and an application thereof.

[0006] The purpose of the present invention can be achieved through the following technical solutions:

[0007] A polyimide film for preparing an ultra-thick graphite film, wherein the polyimide graphite film is a multi-layer composite film with an ABA-type structure, and the raw materials for preparing the polyimide graphite film include the following components:

[0008] A film: 100 parts of polyamic acid resin a, 0.05-1 parts of composite particles;

[0009] B film: 100 parts of polyamic acid resin b, 0.05-1 parts of composite particles;

[0010] The composite particles are prepared as follows: adding an inorganic auxiliary agent to a polyamic acid resin, stirring evenly, then adding a tertiary amine compound catalyst, heating to 145-150° C., continuing stirring until a granular precipitate appears, filtering, washing, vacuum drying, and then treating at 250-300° C. for 2-4 hours, grinding, and obtaining the composite particles; the inorganic auxiliary agent is one or more of wollastonite, calcium carbonate, and barium carbonate; and the amount of the inorganic auxiliary agent added is 5-10% of the mass of the polyamic acid resin.

[0011] Furthermore, the polyamic acid resin a is obtained by polycondensation of diamine and dianhydride in a non-protonic strong polar solvent; the molar ratio of the diamine to the dianhydride is 1:(0.98-1.011); and the viscosity of the polyamic acid resin a is 50-150 Pa·s.

[0012] Furthermore, the diamine is one or two of p-phenylenediamine, m-phenylenediamine, 4,4'-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, and 4,4'-diaminodiphenyl sulfone; the dianhydride is one or two of pyromellitic acid dianhydride, 3,3',4,4'-biphenyltetracarboxylic acid dianhydride, and 3,3',4,4'-benzophenonetetracarboxylic acid dianhydride; and the aprotic strong polar solvent is one of N,N-dimethylformamide, N,N-dimethylacetamide, and N-methylpyrrolidone.

[0013] Furthermore, the polyamic acid resin b is obtained by polycondensation of diamine and dianhydride in a non-protonic strong polar solvent; the molar ratio of the diamine to the dianhydride is 1:(0.98-1.011); and the viscosity of the polyamic acid resin a is 50-150 Pa·s.

[0014] Furthermore, the diamine is one or two of p-phenylenediamine, 4,4'-diaminodiphenyl ether, and 2,2-bis[4-(4-aminophenoxy)phenyl]propane; the dianhydride is one or two of diphenyl ether tetracarboxylic dianhydride, 3,3',4,4'-dibenzophenone tetracarboxylic dianhydride, and 3,3',4,4'-biphenyltetracarboxylic dianhydride; and the aprotic strong polar solvent is one of N,N-dimethylformamide, N,N-dimethylacetamide, and N-methylpyrrolidone.

[0015] Furthermore, the average particle size of the inorganic auxiliary agent is 0.8-1.5 μm, the average particle size of the composite particles is 1.8-2.2 μm, and the tertiary amine compound is triethylamine or pyridine.

[0016] A method for preparing a polyimide film for preparing an ultra-thick graphite film, the method comprising the following steps:

[0017] S1, adding the composite particles into N,N-dimethylacetamide solvent, and stirring and dispersing the mixture to obtain a dispersion;

[0018] S2, adding the dispersion liquid to polyamic acid resin a, stirring and dispersing, to obtain polyamic acid resin a containing composite particles; adding the dispersion liquid to polyamic acid resin b, stirring and dispersing, to obtain polyamic acid resin b containing composite particles;

[0019] S3, firstly coating the polyamic acid resin a containing the composite particles on a steel belt to form a gel film a, then coating the polyamic acid resin b on the surface of the gel film a at intervals and casting it into a gel film b, and then coating the polyamic acid resin a on the surface of the gel film b at intervals to form a final aba type gel film;

[0020] S4, the aba type gel film is longitudinally stretched and transversely stretched, and then subjected to thermal imidization treatment to obtain an aba type polyimide film;

[0021] S5. Carbonize the aba type polyimide film and then graphitize it to obtain a polyimide graphite film.

[0022] Furthermore, in step S2, the stirring and dispersing time is 2 to 5 hours, and the stirring speed is 150 to 200 r / min; in step S3, the casting temperature is 150 to 200° C., the casting speed is 3 to 6 m / min, and the die head interval distance is 2 to 5 m; in step S4, the parameter conditions of thermal imidization are: 50° C. gradient temperature treatment from 100° C. to 450° C.; the longitudinal stretching ratio is 1.0 to 1.1, and the transverse stretching ratio is 1.0 to 1.2.

[0023] Furthermore, in step S5, the carbonization treatment is carried out under vacuum conditions, and the carbonization temperature is programmed to rise from 500°C to 1200-1300°C; the graphitization treatment is carried out under argon protection, and the graphitization temperature is programmed to rise from 1000°C to 2800-3200°C; the programmed heating rate in the carbonization and graphitization treatments is 1-3°C / min.

[0024] The above-mentioned polyimide film for preparing ultra-thick graphite film is used as a preparation material in electronic instruments and equipment.

[0025] The beneficial effects of the present invention are as follows: the present invention uses inorganic particles to prepare PI powder as a foaming aid, thereby improving the compatibility of polyamic acid resin and the inorganic additive, thereby ensuring the uniformity of the dispersion of the foaming aid in the resin, and will not cause coagulation due to the high density of the inorganic additive, thereby improving the stability and uniformity of foaming during the film sintering process, and the graphite film has higher flexibility and fewer crystal points; the ABA form is used to prepare the ultra-thick PI original film, avoiding the preparation of a single-layer thick film, and the bubbles on the film surface are easy to exist, resulting in defects on the graphite film surface after sintering, and the B-layer PI film is a thermoplastic film, which can fit tightly with the A-layer PI film, ensuring the integrity of the sintering, and the thickness is thicker. DETAILED DESCRIPTION

[0026] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0027] Example 1

[0028] A method for preparing a polyimide film for preparing an ultra-thick graphite film, the method comprising the following steps:

[0029] S1. Add 2 parts of composite particles into N,N-dimethylacetamide solvent, stir and disperse, and obtain 2 parts of dispersion liquid; the composite particles are prepared as follows: add inorganic auxiliary agent barium carbonate with an average particle size of 1.5 μm to polyamic acid resin, stir evenly, then add catalyst triethylamine, heat to 150°C, continue stirring until granular precipitate appears, filter out the granular precipitate and wash it with acetone 2-3 times to remove residual solvent; put the obtained solid particles into a vacuum oven at 120°C for 8 hours, and then put it into a high-temperature oven at 250°C for 2 hours, and finally further grind the obtained solid particles to obtain the desired PI composite particles with an average particle size of 2 μm.

[0030] S2, adding 1 part of the dispersion to 100 parts of polyamic acid resin a, stirring at a speed of 200 r / min for 4 hours, to obtain polyamic acid resin a containing composite particles; adding 1 part of the dispersion to 100 parts of polyamic acid resin b, stirring at a speed of 200 r / min for 4 hours, to obtain polyamic acid resin b containing composite particles; the polyamic acid resin a is prepared by polycondensation of p-phenylenediamine and pyromellitic anhydride in N,N-dimethylformamide solvent The obtained product has a molar ratio of p-phenylenediamine to pyromellitic acid dianhydride of 1:0.98; the viscosity of the polyamic acid resin a is 100 Pa·s; the polyamic acid resin b is obtained by polycondensation of 4,4'-diaminodiphenyl ether and diphenyl ether tetracarboxylic dianhydride in N,N-dimethylformamide solvent; the molar ratio of 4,4'-diaminodiphenyl ether to diphenyl ether tetracarboxylic dianhydride is 1:1.011; the viscosity of the polyamic acid resin b is 90 Pa·s.

[0031] S3, firstly coating the polyamic acid resin a containing the composite particles on a steel belt at a casting temperature of 190° C. and a casting speed of 5 m / min to form a gel film a, then coating the polyamic acid resin b on the surface of the gel film a at an interval of 5 m under the same conditions and casting it into a gel film b, and then coating the polyamic acid resin a on the surface of the gel film b at an interval of 5 m under the same conditions to form a final aba type gel film;

[0032] S4, the aba type gel film is first longitudinally stretched, and the longitudinal stretching ratio is 1.05; then thermal imidization is performed under the condition of gradient heating of 100-450°C (starting from 100°C in the first oven, each imidization oven increases by 50°C, 100°C, 150°C, 200°C, 250°C..., until it reaches 450°C), and transverse stretching is performed, and the transverse stretching ratio is 1.1, so as to obtain an aba type polyimide film, and the thickness is controlled to be 175±3μm;

[0033] S5. The aba type polyimide film is first subjected to a carbonization treatment at a temperature of 600°C, programmed to 1300°C, and vacuum conditions, and then subjected to a graphitization treatment at a temperature of 1000°C, programmed to 2900°C, and argon protection to obtain a polyimide graphite film.

[0034] Example 2

[0035] A method for preparing a polyimide film for preparing an ultra-thick graphite film, the method comprising the following steps:

[0036] S1. Add 2 parts of composite particles into N,N-dimethylacetamide solvent, stir and disperse, and obtain 2 parts of dispersion liquid; the composite particles are prepared as follows: add inorganic auxiliary agent barium carbonate with an average particle size of 1.5 μm to polyamic acid resin, stir evenly, then add catalyst triethylamine, heat to 150°C, continue stirring until granular precipitate appears, filter out the granular precipitate and wash it with acetone 2-3 times to remove residual solvent; put the obtained solid particles into a vacuum oven at 120°C for 8 hours, and then put it into a high-temperature oven at 250°C for 2 hours, and finally further grind the obtained solid particles to obtain the desired PI composite particles with an average particle size of 2 μm.

[0037] S2, adding 1 part of the dispersion to 100 parts of polyamic acid resin a, stirring at a speed of 200 r / min for 4 hours, to obtain polyamic acid resin a containing composite particles; adding 1 part of the dispersion to 100 parts of polyamic acid resin b, stirring at a speed of 200 r / min for 4 hours, to obtain polyamic acid resin b containing composite particles; the polyamic acid resin a is prepared by polycondensation of p-phenylenediamine and pyromellitic anhydride in N,N-dimethylformamide solvent The obtained product has a molar ratio of p-phenylenediamine to pyromellitic acid dianhydride of 1:0.98; the viscosity of the polyamic acid resin a is 100 Pa·s; the polyamic acid resin b is obtained by polycondensation of 4,4'-diaminodiphenyl ether and diphenyl ether tetracarboxylic dianhydride in N,N-dimethylformamide solvent; the molar ratio of 4,4'-diaminodiphenyl ether to diphenyl ether tetracarboxylic dianhydride is 1:1.011; the viscosity of the polyamic acid resin b is 90 Pa·s.

[0038] S3, firstly coating the polyamic acid resin a containing the composite particles on a steel belt at a casting temperature of 190° C. and a casting speed of 5 m / min to form a gel film a, then coating the polyamic acid resin b on the surface of the gel film a at an interval of 5 m under the same conditions and casting it into a gel film b, and then coating the polyamic acid resin a on the surface of the gel film b at an interval of 5 m under the same conditions to form a final aba type gel film;

[0039] S4, the aba type gel film is first longitudinally stretched, the longitudinal stretching ratio is 1.05; then thermal imidization is performed under the condition of gradient heating of 100-450°C (starting from 100°C in the first oven, each imidization oven increases by 50°C, 100°C, 150°C, 200°C, 250°C..., until it reaches 450°C), and transverse stretching is performed, the transverse stretching ratio is 1.1, and an aba type polyimide film is obtained, and the thickness is controlled to be 225±3μm;

[0040] S5. The aba type polyimide film is first subjected to a carbonization treatment at a temperature of 600°C, programmed to 1300°C, and vacuum conditions, and then subjected to a graphitization treatment at a temperature of 1000°C, programmed to 2900°C, and argon protection to obtain a polyimide graphite film.

[0041] Example 3

[0042] A method for preparing a polyimide film for preparing an ultra-thick graphite film, the method comprising the following steps:

[0043] S1. Add 2 parts of composite particles into N,N-dimethylacetamide solvent, stir and disperse, and obtain 4 parts of dispersion liquid; the composite particles are prepared as follows: add inorganic auxiliary agent barium carbonate with an average particle size of 1.5 μm to polyamic acid resin, stir evenly, then add catalyst triethylamine, heat to 150°C, continue stirring until granular precipitate appears, filter out the granular precipitate and wash it with acetone 2-3 times to remove residual solvent; put the obtained solid particles into a vacuum oven at 120°C for 8 hours, and then put it into a high-temperature oven at 250°C for 2 hours, and finally further grind the obtained solid particles to obtain the desired PI composite particles with an average particle size of 2 μm.

[0044] S2, adding 2 parts of the dispersion to 100 parts of polyamic acid resin a, stirring at a speed of 200 r / min for 4 hours, to obtain polyamic acid resin a containing composite particles; adding 2 parts of the dispersion to 100 parts of polyamic acid resin b, stirring at a speed of 200 r / min for 4 hours, to obtain polyamic acid resin b containing composite particles; the polyamic acid resin a is prepared by polycondensation of p-phenylenediamine and pyromellitic anhydride in N,N-dimethylformamide solvent The obtained product has a molar ratio of p-phenylenediamine to pyromellitic acid dianhydride of 1:0.98; the viscosity of the polyamic acid resin a is 100 Pa·s; the polyamic acid resin b is obtained by polycondensation of 4,4'-diaminodiphenyl ether and diphenyl ether tetracarboxylic dianhydride in N,N-dimethylformamide solvent; the molar ratio of 4,4'-diaminodiphenyl ether to diphenyl ether tetracarboxylic dianhydride is 1:1.011; the viscosity of the polyamic acid resin b is 90 Pa·s.

[0045] S3, firstly coating the polyamic acid resin a containing the composite particles on a steel belt at a casting temperature of 190° C. and a casting speed of 5 m / min to form a gel film a, then coating the polyamic acid resin b on the surface of the gel film a at an interval of 5 m under the same conditions and casting it into a gel film b, and then coating the polyamic acid resin a on the surface of the gel film b at an interval of 5 m under the same conditions to form a final aba type gel film;

[0046] S4, the aba type gel film is first longitudinally stretched, the longitudinal stretching ratio is 1.05; then thermal imidization is performed under the condition of gradient heating of 100-450°C (starting from 100°C in the first oven, each imidization oven increases by 50°C, 100°C, 150°C, 200°C, 250°C..., until it reaches 450°C), and transverse stretching is performed, the transverse stretching ratio is 1.1, and the aba type polyimide film is obtained, and the thickness is controlled to be 175±3μm;

[0047] S5. The aba type polyimide film is first subjected to a carbonization treatment at a temperature of 600°C, programmed to 1300°C, and vacuum conditions, and then subjected to a graphitization treatment at a temperature of 1000°C, programmed to 2900°C, and argon protection to obtain a polyimide graphite film.

[0048] Comparative Example 1

[0049] The difference between Comparative Example 1 and Example 1 is that no composite particles are added in Comparative Example 1, and the other preparation steps are the same as those in Example 1.

[0050] Comparative Example 2

[0051] The difference between Comparative Example 2 and Example 2 is that the composite particles added in Comparative Example 2 are conventional foaming aid calcium carbonate, and the other preparation steps are the same as those in Example 2.

[0052] Comparative Example 3

[0053] The difference between Comparative Example 3 and Example 1 is that the composite particles added in Comparative Example 3 are conventional foaming aids, and the other preparation steps are the same as those in Example 1.

[0054] Table 1 Performance test results of polyimide film and fired graphite film

[0055] Example Thickness(μm) Foam thickness (μm) Surface crystal point Thermal conductivity (W / (m·k)) Example 1 175±3 212 few 1392 Example 2 225±3 272 few 1476 Example 3 175±3 218 few 1452 Comparative Example 1 175±3 170 many 910 Comparative Example 2 225±3 263 less 1285 Comparative Example 3 175±3 208 less 1210

[0056] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0057] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments, and the above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, and these changes and improvements all fall within the scope of the present invention to be protected.

Claims

1. A polyimide film for preparing an ultra-thick graphite film, wherein the polyimide film is a multilayer composite film and has an ABA type structure, characterized in that: The raw materials for preparing the polyimide graphite film include the following components: A film: 100 parts of polyamic acid resin a, 0.05-1 parts of composite particles; B film: 100 parts of polyamic acid resin b, 0.05-1 parts of composite particles; The composite particles are prepared as follows: adding an inorganic auxiliary agent to a polyamic acid resin, stirring evenly, then adding a tertiary amine compound catalyst, heating to 145-150° C., continuing stirring until a granular precipitate appears, filtering, washing, vacuum drying, and then treating at 250-300° C. for 2-4 hours, grinding, and obtaining the composite particles; the inorganic auxiliary agent is one or more of wollastonite, calcium carbonate, and barium carbonate; and the amount of the inorganic auxiliary agent added is 5-10% of the mass of the polyamic acid resin.

2. A polyimide film for preparing an ultra-thick graphite film according to claim 1, characterized in that: The polyamic acid resin a is obtained by polycondensation of diamine and dianhydride in a non-protonic strong polar solvent; the molar ratio of the diamine to the dianhydride is 1:(0.98-1.011); and the viscosity of the polyamic acid resin a is 50-150 Pa·s.

3. A polyimide film for preparing an ultra-thick graphite film according to claim 2, characterized in that: The diamine is one or two of p-phenylenediamine, m-phenylenediamine, 4,4'-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, and 4,4'-diaminodiphenyl sulfone; the dianhydride is one or two of pyromellitic acid dianhydride, 3,3',4,4'-biphenyltetracarboxylic acid dianhydride, and 3,3',4,4'-benzophenonetetracarboxylic acid dianhydride; and the aprotic strong polar solvent is one of N,N-dimethylformamide, N,N-dimethylacetamide, and N-methylpyrrolidone.

4. The polyimide film for preparing an ultra-thick graphite film according to claim 1, characterized in that: The polyamic acid resin b is obtained by polycondensation of diamine and dianhydride in a non-protonic strong polar solvent; the molar ratio of the diamine to the dianhydride is 1:(0.98-1.011); and the viscosity of the polyamic acid resin a is 50-150 Pa·s.

5. The polyimide film for preparing an ultra-thick graphite film according to claim 4, characterized in that: The diamine is one or two of p-phenylenediamine, 4,4'-diaminodiphenyl ether, and 2,2-bis[4-(4-aminophenoxy)phenyl]propane; the dianhydride is one or two of diphenyl ether tetracarboxylic dianhydride, 3,3',4,4'-dibenzophenone tetracarboxylic dianhydride, and 3,3',4,4'-biphenyltetracarboxylic dianhydride; and the aprotic strong polar solvent is one of N,N-dimethylformamide, N,N-dimethylacetamide, and N-methylpyrrolidone.

6. The polyimide film for preparing an ultra-thick graphite film according to claim 1, characterized in that: The average particle size of the inorganic auxiliary agent is 0.8-1.5 μm, the average particle size of the composite particles is 1.8-2.2 μm, and the tertiary amine compound is triethylamine or pyridine.

7. A method for preparing a polyimide film for preparing an ultra-thick graphite film, characterized in that: The preparation method comprises the following steps: S1, adding the composite particles into N,N-dimethylacetamide solvent, and stirring and dispersing the mixture to obtain a dispersion; S2, adding the dispersion liquid to polyamic acid resin a, stirring and dispersing, to obtain polyamic acid resin a containing composite particles; adding the dispersion liquid to polyamic acid resin b, stirring and dispersing, to obtain polyamic acid resin b containing composite particles; S3, firstly coating the polyamic acid resin a containing the composite particles on a steel belt to form a gel film a, then coating the polyamic acid resin b on the surface of the gel film a at intervals and casting it into a gel film b, and then coating the polyamic acid resin a on the surface of the gel film b at intervals to form a final aba type gel film; S4, the aba type gel film is longitudinally stretched and transversely stretched, and then subjected to thermal imidization treatment to obtain an aba type polyimide film; S5. Carbonize the aba type polyimide film and then graphitize it to obtain a polyimide graphite film.

8. The method for preparing a polyimide film for preparing an ultra-thick graphite film according to claim 7, characterized in that: In step S2, the stirring and dispersing time is 2 to 5 hours, and the stirring speed is 150 to 200 r / min; in step S3, the casting temperature is 150 to 200° C., the casting speed is 3 to 6 m / min, and the die head interval distance is 2 to 5 m; in step S4, the parameter conditions of thermal imidization are: 50° C. gradient temperature treatment from 100° C. to 450° C.; the longitudinal stretching ratio is 1.0 to 1.1, and the transverse stretching ratio is 1.0 to 1.

2.

9. The method for preparing a polyimide film for preparing an ultra-thick graphite film according to claim 7, characterized in that: In step S5, the carbonization treatment is carried out under vacuum conditions, and the carbonization temperature is programmed to rise from 500°C to 1200-1300°C; the graphitization treatment is carried out under argon protection, and the graphitization temperature is programmed to rise from 1000°C to 2800-3200°C; the programmed heating rate in the carbonization and graphitization treatments is 1-3°C / min.

10. Use of a polyimide film for preparing ultra-thick graphite film as claimed in claims 1 to 6 as a preparation material in electronic instruments and equipment.

Citation Information

Cited By

  • Polyimide film and preparation method thereof

    CN119144156A

  • High-foaming polyimide-based graphite film and preparation method thereof

    CN121823561A