Anti-aging, anti-dust and anti-reflection coating liquid as well as preparation method and application thereof
Through the combination of silicon sol, anti-static weathering additives and template agents, an anti-dust, anti-static anti-reflective film layer is formed, which solves the problem of degradation in the performance of photovoltaic coating liquid in harsh environments, and realizes the long-term cleanliness and high transparency of photovoltaic glass Excessive rate, extending service life.
Patent Information
- Application Number
- CN202410934284.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-11
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-07-11
AI Technical Summary
The existing photovoltaic coating solution is difficult to meet the performance requirements of aging resistance, dust resistance and penetration at the same time, resulting in a reduced power generation efficiency of photovoltaic modules in harsh environments.
Using a combination of silicon sol, anti-static weathering additive and template agent, a dust-resistant anti-static anti-reflective film layer is formed through a specific preparation method, which gives photovoltaic glass good anti-reflection, dust-resistant and accelerated aging properties.
The long-term cleanliness and high transmittance of the film layer in harsh environments are achieved, extending the service life of photovoltaic glass and reducing maintenance costs.
Smart Images

Figure CN118895057A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of optical materials, and particularly relates to an aging-resistant, dust-resistant, and anti-reflection coating solution, and a preparation method and application thereof. Background Art
[0002] As a representative of new energy, the photovoltaic industry has increased its installed capacity by about 25 times in the past decade. It is estimated that by 2030, more than 10% of the world's total electricity supply will be provided by solar photovoltaic power generation. However, solar panels that have been operating for a long time in harsh environments usually accumulate a thick layer of dust on the surface, which greatly reduces the transmittance of the coated glass on the photovoltaic modules. The photoelectric conversion efficiency of the battery also decreases exponentially with the increase of dust density on the glass surface, which seriously affects the normal power generation of solar cells.
[0003] Chinese patent CN103044977A discloses a preparation method for a hydrophilic self-cleaning anti-reflection film coating. It mainly solves the problem that the coating does not have the hydrophilic self-cleaning function and the anti-reflection and anti-transmittance function. At the same time, it is also necessary to solve the problem of curing at high temperature. Specifically, it includes the following steps: 1) mixing ammonia water, alcohol and deionized water in a volume ratio of 1:10-60:0.5-5 and heating to 30-90°C; 2) mixing an organic silicon source and alcohol in a volume ratio of 1:1-30 to obtain a mixed solution; 3) adding the reaction solution prepared in step 2) to the mixed solution prepared in step 1) at one time to react and obtain the finished product. The film layer formed by this method is uniform, the surface nanostructure is regular, and the hydroxyl density of the particle surface is large, so the transmittance is greatly improved. When the single-sided coating is applied, the transmittance is increased by more than 3%, and it has good hydrophilic self-cleaning properties. However, the film layer does not have antistatic or anti-accelerated aging properties, and it is difficult to maintain stability for long-term use.
[0004] Chinese patent CN102153292A provides a high-transmittance nano-silica anti-reflection film and its preparation method and application. Specifically, it includes the following steps: using tetraethyl orthosilicate, ethanol and water as raw materials, ammonia water or hydrochloric acid as a catalyst, and making silica sol according to the molar ratio of tetraethyl orthosilicate: ethanol: water: catalyst = 1: 2-4: 30-80: 1-5, diluting the silica sol, and adding polyvinyl pyrrolidone stabilizer according to the addition amount of 1-5g / liter of coating liquid, and adding resin adhesive according to the addition amount of 5-15g / liter of coating liquid to obtain coating liquid. The coated glass is pre-cured at a temperature of 100-200°C for 20-300s, and then tempered. However, the film layer does not have a self-cleaning function.
[0005] Chinese patent CN114772942A provides a photovoltaic glass self-cleaning nano coating and a processing method thereof, wherein the raw materials include nano silicon dioxide, nano titanium dioxide, waterborne polyurethane, polymer emulsion, dispersing aid and siloxane, wherein the content of nano silicon dioxide is less than 4 / 5, and the content of nano titanium dioxide is not less than 3%; the processing steps include the construction and synthesis of the surface microstructure of core-shell nanoparticles, wherein the core-shell nanoparticles are complex core-shell micro-nano materials with a multi-layer core-shell structure, the film thickness of the microstructure is 1 to 3 microns, the microstructure is constructed by a three-dimensional cross-linking method, the three-dimensional cross-linking method forms the surface microstructure by covalent bonds, has swelling ability, and first forms a linear polymer during the formation process, and then forms crosslinks by reaction between polymers, and the core-shell nanoparticles are mass-produced and synthesized by grafting modification; the organic and inorganic cross-linking doping technology is adopted to dope conductive element intermediates and photocatalytic element intermediates, and the conductive element doping causes the surface resistance of the coated glass to be between 1×10 4 Ω~1×10 11 Ω, the photocatalytic element intermediate is an inorganic intermediate. However, the film layer does not have the performance of resisting accelerated aging and is difficult to be used for a long time in a harsh environment.
[0006] That is, the film layer formed by the coating solution in the prior art cannot simultaneously meet the performance requirements of aging resistance, dust resistance, and anti-reflection, which is not conducive to the application of the coating solution in the photovoltaic industry.
[0007] Therefore, there is an urgent need to provide a new coating solution so that the film layer formed by the coating solution in the photovoltaic field has the functions of anti-aging, anti-dust and anti-reflection. Summary of the invention
[0008] The present invention aims to solve at least one of the technical problems existing in the above-mentioned prior art. To this end, the present invention provides an anti-aging, anti-dust, anti-reflection coating solution and its preparation method and application. The film layer formed by the coating solution of the present invention simultaneously meets the performance requirements of anti-aging, anti-dust, and anti-reflection (or anti-reflection).
[0009] The present invention mainly provides an aging-resistant, dust-resistant and anti-transmittance coating liquid, which aims to solve the problem that photovoltaic coated glass is prone to dust accumulation on the surface, thereby reducing the power generation efficiency of photovoltaic modules. In order to improve the hardness of the traditional photovoltaic glass anti-reflection film layer, the film layer will be regulated to form a dense structure, resulting in the film layer easily absorbing dust. There is also a hydrophobic self-cleaning anti-reflection film layer, which is prepared by inorganic-doped organic silica sol. The surface of the film layer has super-hydrophobic properties. After rainfall, the super-hydrophobicity can be used to repel dust on the surface of the film layer, thereby achieving a self-cleaning effect. However, this hydrophobic film layer is easily destroyed by ultraviolet rays, resulting in poor hydrophobic performance; at the same time, due to the hydrophobic property, the film layer is easy to form separate water droplets after being washed by rainwater, and becomes spots mixed with water and dust after drying, which greatly reduces the transmittance of the coated glass in this area.
[0010] The coating liquid of the present invention includes silica sol, template agent, antistatic weathering agent, and the coating liquid is evenly coated on the surface of the anti-reflection film layer of photovoltaic glass, and an anti-dust and anti-static anti-reflection film layer is formed after the glass is tempered, which gives the photovoltaic glass good anti-reflection, anti-dust, anti-static and anti-accelerated aging properties. The film layer can maintain good cleanliness after rain scouring, mechanical vibration and air convection, so that the photovoltaic module can maintain a stable power generation efficiency for a long time in harsh environment.
[0011] The membrane liquid preparation process of the present invention is simple, easy to use, and has high stability, so it is suitable for large-scale industrial production. It can give photovoltaic glass good anti-reflection, anti-dust, anti-static and anti-accelerated aging properties, which can greatly extend the service life of photovoltaic glass and reduce the maintenance cost of photovoltaic glass.
[0012] The first aspect of the present invention provides an aging-resistant, dust-resistant and anti-reflective coating solution.
[0013] Specifically, an anti-aging, anti-dust, and anti-transmittance coating solution includes silica sol, antistatic weathering additive, and template agent;
[0014] The preparation process of the silica sol includes: mixing silicate with a diluent to obtain liquid A; mixing water, a stabilizer, and an alkaline catalyst to obtain liquid B; mixing liquid A and liquid B to react to prepare the silica sol;
[0015] In the liquid B, the mass of the stabilizer is less than 0.35% of the mass of the water;
[0016] The antistatic weathering agent includes tin halide and antimony halide.
[0017] Preferably, the mass of the stabilizer is 0.01-0.35% of the mass of the water, for example, 0.01-0.33%, 0.1-0.33%, 0.05-0.33%.
[0018] Preferably, the silicate is selected from at least one of methyl orthosilicate, ethyl orthosilicate, propyl orthosilicate, methyltrimethoxysilane, methyltriethoxysilane, methyltripropoxysilane, ethyltrimethoxysilane, ethyltriethoxysilane, ethyltripropoxysilane, dimethyldimethoxysilane, dimethyldiethoxysilane, dimethyldipropoxysilane, trimethylmethoxysilane or trimethylethoxysilane; further preferably, the silicate is selected from at least one of ethyl orthosilicate, methyltriethoxysilane, dimethyldiethoxysilane or trimethylethoxysilane.
[0019] Preferably, the water is purified water or deionized water.
[0020] Preferably, the diluent is selected from at least one of methanol, ethanol, isopropanol or n-butanol.
[0021] Preferably, in the liquid A, the mass ratio of the silicate to the diluent is 15-30:(15-50), and more preferably 15-30:(20-40).
[0022] Preferably, during the preparation of the liquid B, a diluent and / or a pore-forming agent is also added.
[0023] Preferably, the stabilizer includes at least one of diethanolamine, dimethylethanolamine, dimethylformamide or dimethylacetamide. When the stabilizer is present, the silica sol, the template agent and the antistatic weathering agent are mixed to ensure the stability of the silica sol.
[0024] Preferably, the alkaline catalyst includes at least one of aqueous ammonia, sodium hydroxide or potassium hydroxide.
[0025] Preferably, the pore-forming agent is polyethylene glycol, more preferably polyethylene glycol with a molecular weight of 200 to 1000.
[0026] Preferably, in the liquid B, the mass ratio of water to alkaline catalyst is 15-30:(0.1-1.0).
[0027] Preferably, when the B liquid contains a diluent and a pore-forming agent, the mass ratio of water to the diluent and the pore-forming agent is 15-30:(10-50):(0.01-0.2), and more preferably 15-30:(20-40):(0.01-0.15).
[0028] Preferably, liquid A is added to the stirred liquid B at room temperature at a uniform speed for 10 to 30 minutes, and then liquid A and liquid B react.
[0029] Preferably, the mixture of liquid A and liquid B is reacted at 15-40°C for 1 to 8 hours, more preferably at room temperature for 2 to 8 hours.
[0030] Preferably, after the reaction of liquid A and liquid B is completed, they are aged at room temperature for 2 to 6 days.
[0031] Preferably, the tin halide includes at least one of tin tetrachloride pentahydrate, tin tetrachloride, tin fluoride, and tin tetrabromide, and more preferably tin tetrachloride.
[0032] Preferably, the antimony halide includes at least one of antimony trichloride, antimony tribromide and antimony pentafluoride, and antimony trichloride is more preferred.
[0033] The antistatic weathering additive can not only improve the antistatic effect of the film layer formed by the plating solution, but also significantly improve the aging resistance of the film layer.
[0034] Preferably, in the antistatic weathering agent, the mass ratio of tin halide to antimony halide is 20 to 100:1, more preferably 40 to 80:1.
[0035] Preferably, the antistatic weather-resistant additive also includes a diluent.
[0036] Preferably, the template is silica core-shell microspheres. The template is prepared according to the method described in "2.2 Experimental Section" of "Study on the Preparation and Formation Mechanism of Hollow Silica Spheres and Core-shell Structures", Wan Yong, PhD thesis, University of Science and Technology of China.
[0037] Preferably, in the plating solution, the mass ratio of silica sol, antistatic weathering agent and template agent is 1:(0.1-1.0):(0.005-0.1) in terms of effective solid content ratio; more preferably, it is 1:(0.1-0.8):(0.005-0.04).
[0038] The effective solid content ratio refers to the weight ratio of the remaining solid matter after the solution substance is tested for solid content.
[0039] Preferably, the plating solution also includes a volatilization inhibitor.
[0040] Preferably, the volatility inhibitor is selected from at least one of ethylene glycol methyl ether, ethylene glycol ethyl ether, ethylene glycol butyl ether, diethylene glycol butyl ether, propylene glycol methyl ether, propylene glycol butyl ether or diacetone.
[0041] Preferably, the volatilization inhibitor accounts for 1 to 15% of the total mass of the coating solution, and more preferably 4 to 8%.
[0042] The second aspect of the present invention provides a method for preparing an aging-resistant, dust-resistant and anti-reflective coating solution.
[0043] Specifically, a method for preparing an aging-resistant, dust-resistant and anti-reflective coating solution comprises the following steps:
[0044] The silica sol is mixed with an antistatic weather-resistant additive and a template agent to obtain the coating solution.
[0045] Preferably, the tin halide is mixed with a diluent, and then antimony halide is added and stirred to obtain the antistatic weathering agent.
[0046] Preferably, tin tetrachloride pentahydrate is added to a diluent to prepare a solution with a molar concentration of 0.4 to 1.0 mol / L, and then antimony trichloride is added according to a mass ratio of tin tetrachloride pentahydrate to antimony trichloride of 20 to 100:1, and stirred and dissolved at room temperature, and then stirred at a constant temperature of 60 to 100° C. for 3 to 8 hours, cooled and aged for 2 to 6 days to obtain an antistatic weathering additive.
[0047] Preferably, after the silica sol is mixed with the antistatic weathering aid and the template, a diluent with a total solid content of 2 to 4% of the silica sol, the antistatic weathering aid and the template is added to prepare a prefabricated plating solution, and finally a volatilization inhibitor is added according to 4 to 8% of the mass of the prefabricated plating solution to prepare the plating solution.
[0048] Preferably, the method for preparing the coating solution comprises the following steps:
[0049] (1) premixing a silicate and a diluent in a mass ratio of 15-30:20-40 to prepare a liquid A, and mixing purified water, a diluent, a pore former, a stabilizer and aqueous ammonia in a mass ratio of 15-30:20-40:0.01-0.15:0.005-0.05:0.1-1.0 to prepare a liquid B;
[0050] (2) adding the liquid A described in step (1) into the stirred liquid B at room temperature at a uniform speed for 10 to 30 minutes, then continuing to react at room temperature for 3 to 8 hours, and aging at room temperature for 2 to 6 days after the reaction to obtain a silica sol;
[0051] (3) adding tin tetrachloride pentahydrate to a diluent to prepare a solution with a molar concentration of 0.4 to 1.0 mol / L, then adding antimony trichloride according to a mass ratio of tin tetrachloride pentahydrate to antimony trichloride of 20 to 100:1, stirring and dissolving at room temperature, then stirring and reacting at a constant temperature of 60 to 100° C. for 3 to 8 hours, cooling and aging for 2 to 6 days to obtain an antistatic weathering agent;
[0052] (4) Prepare the template according to the method described in "2.2 Experimental Section" of "Study on the Preparation and Formation Mechanism of Hollow Silica Spheres and Core-Shell Structures", Wan Yong, University of Science and Technology of China, PhD thesis;
[0053] (5) Silica sol, template agent and antistatic weathering agent are mixed according to an effective solid content ratio of 1:0.1-0.8:0.005-0.04, and a diluent is added at 2-4% of the final solid content to prepare a pre-coating solution, and finally a volatilization inhibitor is added at 4-8% of the mass of the pre-coating solution to prepare the coating solution.
[0054] The third aspect of the present invention provides an application of an aging-resistant, dust-resistant and anti-reflective coating solution.
[0055] Specifically, a glass includes a film layer formed by the above coating solution.
[0056] Preferably, the glass comprises photovoltaic glass
[0057] A method for preparing photovoltaic glass comprises the following steps:
[0058] The coating liquid is coated on the glass by roller coating, and then solidified, and then tempered to obtain the photovoltaic glass.
[0059] Preferably, the curing temperature is 140-160°C, more preferably 150-160°C.
[0060] Preferably, the temperature of the tempering treatment is 680-720°C, more preferably 690-710°C.
[0061] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0062] The coating liquid of the present invention includes silica sol, antistatic weathering agent, and template agent, wherein the silica sol is prepared by the specific method of the present invention. In the process of preparing the silica sol, a stabilizer and an alkaline catalyst need to be used, and the stabilizer needs to be used in a specific amount. The antistatic weathering agent includes tin halide and antimony halide. The antistatic weathering agent can not only improve the antistatic effect of the film layer formed by the coating liquid, but also significantly improve the aging resistance of the film layer. The film layer formed on the glass surface by the coating liquid allows the photovoltaic glass to simultaneously meet the performance requirements of aging resistance, dust resistance, and anti-reflection (or anti-reflection), and further has good antistatic properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0063] Figure 1 is a cross-sectional view of the coated glass of Example 1;
[0064] Figure 2 This is a cross-sectional view of the coated glass of Comparative Example 2. DETAILED DESCRIPTION
[0065] In order to make the technical scheme of the present invention more clearly understood by those skilled in the art, the following embodiments are listed for illustration. It should be pointed out that the following embodiments do not limit the protection scope of the present invention.
[0066] Unless otherwise specified, the raw materials, reagents or devices used in the following examples can be obtained from conventional commercial sources or by existing known methods.
[0067] The solid content is tested according to this method: Liquid A is quantitatively weighed into a beaker on a precision electronic balance, and the empty beaker weight G is recorded. 杯 and weight of liquid A G 液 Place the beaker containing liquid A in a 160℃ constant temperature drying oven and dry for 1 hour. After taking it out, transfer it to a drying dish and cool it to room temperature. Then weigh the total weight of the beaker and the solid in the cup to obtain G. 杯+固 , calculate solid content = (G 杯+固 -G 杯 ) / G 液 .
[0068] Example 1: Preparation of coating solution
[0069] An anti-aging, anti-dust and anti-transmittance coating solution, comprising silica sol, antistatic weathering additive, template agent and ethylene glycol butyl ether;
[0070] 25 g of purified water, 25 g of ethanol, 0.05 g of dimethylformamide, 0.5 g of ammonia water (ammonia water mass fraction concentration is 20%) and 0.06 g of polyethylene glycol were added to a conical flask with a magnetic stirrer to form a B solution. 20 g of tetraethyl orthosilicate and 30 g of ethanol were added to a constant pressure funnel to form a A solution. The A solution in the constant pressure funnel was added dropwise to the B solution in the conical flask under stirring at a constant speed for 25 min. The mixture was then stirred for 5 h at room temperature. After aging for 4 days, a silica sol with a solid content of 6.0 wt.% was obtained.
[0071] In liquid B, the mass of the stabilizer dimethylformamide is 0.2% of the mass of purified water.
[0072] A method for preparing an aging-resistant, dust-resistant and anti-reflective coating solution comprises the following steps:
[0073] (1) 25 g of purified water, 25 g of ethanol, 0.05 g of dimethylformamide, 0.5 g of ammonia water (ammonia water mass fraction concentration is 20%) and 0.06 g of polyethylene glycol were added to a conical flask with a magnetic stirrer to form a B solution, 20 g of tetraethyl orthosilicate and 30 g of ethanol were added to a constant pressure funnel to form a A solution, and the A solution in the constant pressure funnel was added dropwise to the B solution in the conical flask under stirring at a constant speed for 25 min, and then the stirring was continued at room temperature for 5 h. After aging for 4 days, a silica sol with a solid content of 6.0 wt.% was obtained;
[0074] (2) Add 39.45 g of ethanol to another conical flask with a magnetic stirrer, then add 12.25 g of tin tetrachloride pentahydrate and 0.21 g of antimony trichloride to the ethanol, stir and dissolve at room temperature, then stir at 80° C. for 5 h, cool and age for 4 days to obtain an antistatic weathering additive with a solid content of 2.0 wt.%;
[0075] (3) According to the method described in "2.2 Experimental Section" of "Study on the Preparation and Formation Mechanism of Hollow Silica Spheres and Core-shell Structures", Wan Yong, University of Science and Technology of China, PhD thesis, silica core-shell microspheres were prepared as templates with a solid content of 3.0 wt.%;
[0076] (4) Silica sol, template agent and antistatic weathering agent are mixed according to an effective solid content ratio of 1:0.6:0.015, and ethanol is added to adjust the solid content to 3wt.% to prepare a pre-coating solution. Finally, ethylene glycol butyl ether is added according to 5% of the mass of the pre-coating solution to prepare a coating solution.
[0077] A method for preparing dust-proof, antistatic and anti-reflective coated glass comprises the following steps:
[0078] The coating liquid is applied on the photovoltaic glass by roller coating, and then baked and cured at 160°C, and then tempered at 710°C to obtain dust-resistant, antistatic and anti-reflective coated glass.
[0079] Example 2
[0080] A method for preparing an aging-resistant, dust-resistant and anti-reflective coating solution comprises the following steps:
[0081] (1) 15 g of purified water, 35 g of ethanol, 0.005 g of diethanolamine, 0.5 g of ammonia water (the mass fraction concentration of ammonia water is 20%) and 0.15 g of polyethylene glycol were added to a conical flask with a magnetic stirrer to form a B solution (in the B solution, the mass of the stabilizer diethanolamine is 0.03% of the mass of the purified water), 20 g of tetraethyl orthosilicate and 30 g of ethanol were added to a constant pressure funnel to form a A solution, and the A solution in the constant pressure funnel was added dropwise to the B solution in the conical flask under stirring at a constant speed for 20 min, and then the stirring was continued at room temperature for 4 h. After aging for 3 days, a silica sol with a solid content of 6.2 wt.% was obtained;
[0082] (2) Add 39.45 g of ethanol to another conical flask with a magnetic stirrer, then add 15.75 g of tin tetrachloride pentahydrate and 0.61 g of antimony trichloride to the ethanol, stir and dissolve at room temperature, then stir at 80° C. for 5 h, cool and age for 4 days to obtain an antistatic weathering agent with a solid content of 2.2 wt.%;
[0083] (3) The template is the same as in Example 1;
[0084] (4) Silica sol, template agent and antistatic weathering agent are mixed according to an effective solid content ratio of 1:0.4:0.01, and ethanol is added to adjust the solid content to 3wt.% to prepare a pre-coating solution. Finally, ethylene glycol butyl ether is added according to 8% of the mass of the pre-coating solution to prepare a coating solution.
[0085] A method for preparing dust-proof, antistatic and anti-reflective coated glass comprises the following steps:
[0086] The coating liquid is applied on the photovoltaic glass by roller coating, and then baked and cured at 160°C, and then tempered at 710°C to obtain dust-resistant, antistatic and anti-reflective coated glass.
[0087] Example 3
[0088] A method for preparing an aging-resistant, dust-resistant and anti-reflective coating solution comprises the following steps:
[0089] (1) 30 g of purified water, 25 g of ethanol, 0.01 g of dimethylacetamide, 0.6 g of ammonia water (the mass fraction concentration of ammonia water is 20%) and 0.01 g of polyethylene glycol were added to a conical flask with a magnetic stirrer to form a B solution (in the B solution, the mass of the stabilizer dimethylacetamide is 0.03% of the mass of the purified water), 15 g of tetraethyl orthosilicate and 25 g of ethanol were added to a constant pressure funnel to form a A solution, and the A solution in the constant pressure funnel was added dropwise to the B solution in the conical flask under stirring at a constant speed for 30 min, and then the stirring was continued at room temperature for 6 h. After aging for 5 days, a silica sol with a solid content of 5.0 wt.% was obtained;
[0090] (2) Add 39.45 g of ethanol to another conical flask with a magnetic stirrer, then add 8.75 g of tin tetrachloride pentahydrate and 0.12 g of antimony trichloride to the ethanol, stir and dissolve at room temperature, then stir at 80° C. for 5 h, cool and age for 4 days to obtain an antistatic weathering agent with a solid content of 1.8 wt.%;
[0091] (3) The template is the same as in Example 1;
[0092] (4) Silica sol, template agent and antistatic weathering agent are mixed according to an effective solid content ratio of 1:0.3:0.04, and ethanol is added to adjust the solid content to 3wt.% to prepare a pre-coating solution. Finally, ethylene glycol butyl ether is added according to 4% of the mass of the pre-coating solution to prepare a coating solution.
[0093] A method for preparing dust-proof, antistatic and anti-reflective coated glass comprises the following steps:
[0094] The coating liquid is applied on the photovoltaic glass by roller coating, and then baked and cured at 160°C, and then tempered at 710°C to obtain dust-resistant, antistatic and anti-reflective coated glass.
[0095] Example 4
[0096] A method for preparing an aging-resistant, dust-resistant and anti-reflective coating solution comprises the following steps:
[0097] (1) 30 g of purified water, 25 g of ethanol, 0.025 g of dimethylformamide, and 0.4 g of ammonia water (the mass fraction concentration of ammonia water is 20%) were added to a conical flask with a magnetic stirrer to form a B solution (in the B solution, the mass of the stabilizer dimethylformamide is 0.08% of the mass of the purified water), 20 g of ethyl orthosilicate, 1 g of methyltriethoxysilane, and 25 g of ethanol were added to a constant pressure funnel to form a A solution, and the A solution in the constant pressure funnel was added dropwise to the B solution in the stirred conical flask at a constant speed for 20 min, and then the stirring was continued at room temperature for 5 h. After aging for 4 days, a silica sol with a solid content of 6.9 wt.% was obtained;
[0098] (2) Add 39.45 g of ethanol to another conical flask with a magnetic stirrer, then add 12.25 g of tin tetrachloride pentahydrate and 0.16 g of antimony trichloride to the ethanol, stir and dissolve at room temperature, then stir at 80° C. for 5 h, cool and age for 4 days to obtain an antistatic weathering agent with a solid content of 2.0 wt.%;
[0099] (3) The template is the same as in Example 1;
[0100] (4) Silica sol, template agent and antistatic weathering agent are mixed according to an effective solid content ratio of 1:0.2:0.01, and ethanol is added to adjust the solid content to 3wt.% to prepare a pre-coating solution. Finally, diethylene glycol butyl ether is added according to 4% of the mass of the pre-coating solution to prepare a coating solution.
[0101] A method for preparing dust-proof, antistatic and anti-reflective coated glass comprises the following steps:
[0102] The coating liquid is applied on the photovoltaic glass by roller coating, and then baked and cured at 160°C, and then tempered at 710°C to obtain dust-resistant, antistatic and anti-reflective coated glass.
[0103] Example 5
[0104] A method for preparing an aging-resistant, dust-resistant and anti-reflective coating solution comprises the following steps:
[0105] (1) 25 g of purified water, 25 g of ethanol, 0.025 g of dimethylformamide, 0.5 g of ammonia water (the mass fraction concentration of ammonia water is 20%) and 0.06 g of polyethylene glycol were added to a conical flask with a magnetic stirrer to form a B solution (in the B solution, the mass of the stabilizer dimethylformamide is 0.1% of the mass of the purified water), 16 g of tetraethyl orthosilicate, 4 g of methyltriethoxysilane and 30 g of ethanol were added to a constant pressure funnel to form a A solution, and the A solution in the constant pressure funnel was added dropwise to the B solution in the stirred conical flask at a constant speed for 25 min, and then the stirring was continued at room temperature for 5 h. After aging for 4 days, a silica sol with a solid content of 6.3 wt.% was obtained;
[0106] (2) Add 39.45 g of ethanol to another conical flask with a magnetic stirrer, then add 12.25 g of tin tetrachloride pentahydrate and 0.16 g of antimony trichloride to the ethanol, stir and dissolve at room temperature, then stir at 80° C. for 5 h, cool and age for 4 days to obtain an antistatic weathering agent with a solid content of 2.0 wt.%;
[0107] (3) The template is the same as in Example 1;
[0108] (4) Silica sol, template agent and antistatic weathering agent are mixed according to an effective solid content ratio of 1:0.1:0.005, and ethanol is added to adjust the solid content to 3wt.% to prepare a pre-coating solution. Finally, ethylene glycol butyl ether is added according to 5% of the mass of the pre-coating solution to prepare a coating solution.
[0109] A method for preparing dust-proof, antistatic and anti-reflective coated glass comprises the following steps:
[0110] The coating liquid is applied on the photovoltaic glass by roller coating, and then baked and cured at 160°C, and then tempered at 710°C to obtain dust-resistant, antistatic and anti-reflective coated glass.
[0111] Example 6
[0112] A method for preparing an aging-resistant, dust-resistant and anti-reflective coating solution comprises the following steps:
[0113] (1) 20 g of purified water, 25 g of ethanol, 0.01 g of dimethylformamide, and 0.6 g of ammonia water (the mass fraction concentration of ammonia water is 20%) were added to a conical flask with a magnetic stirrer to form a B solution (in the B solution, the mass of the stabilizer dimethylformamide is 0.05% of the mass of the purified water), 29 g of tetraethyl orthosilicate, 1 g of methyltriethoxysilane, and 25 g of ethanol were added to a constant pressure funnel to form a A solution, and the A solution in the constant pressure funnel was added dropwise to the B solution in the stirred conical flask at a constant speed for 20 min, and then the stirring was continued at room temperature for 5 h. After aging for 4 days, a silica sol with a solid content of 9.9 wt.% was obtained;
[0114] (2) Add 39.45 g of ethanol to another conical flask with a magnetic stirrer, then add 12.25 g of tin tetrachloride pentahydrate and 0.16 g of antimony trichloride to the ethanol, stir and dissolve at room temperature, then stir at 80° C. for 5 h, cool and age for 4 days to obtain an antistatic weathering agent with a solid content of 2.0 wt.%;
[0115] (3) The template is the same as in Example 1;
[0116] (4) Silica sol, template agent and antistatic weathering agent are mixed according to an effective solid content ratio of 1:0.8:0.03, and ethanol is added to adjust the solid content to 3wt.% to prepare a pre-coating solution. Finally, ethylene glycol butyl ether is added according to 5% of the mass of the pre-coating solution to prepare a coating solution.
[0117] A method for preparing dust-proof, antistatic and anti-reflective coated glass comprises the following steps:
[0118] The coating liquid is applied on the photovoltaic glass by roller coating, and then baked and cured at 160°C, and then tempered at 710°C to obtain dust-resistant, antistatic and anti-reflective coated glass.
[0119] Comparative Example 1
[0120] The Yishang Transcend dust-proof coating liquid purchased from Shenzhen Yishang Nano Technology Co., Ltd. was coated on the photovoltaic glass by roller coating, then baked and cured at 160°C, and then tempered at 710°C to obtain the coated glass.
[0121] Comparative Example 2
[0122] A method for preparing a coating solution comprises the following steps:
[0123] (1) 20 g of purified water, 25 g of ethanol, and 0.4 g of hydrochloric acid (hydrochloric acid concentration is 0.2 mol / L) are added to a conical flask with a magnetic stirrer to form a B solution, 30 g of tetraethyl orthosilicate and 25 g of ethanol are added to a constant pressure funnel to form a A solution, and the A solution in the constant pressure funnel is added dropwise to the B solution in the conical flask under stirring at a constant speed for 20 min, and then the stirring is continued for 4 h at room temperature. After aging for 4 days, a silica sol with a solid content of 15.4 wt.% is obtained;
[0124] (2) Add 39.45 g of ethanol to another conical flask with a magnetic stirrer, then add 12.25 g of tin tetrachloride pentahydrate and 0.21 g of antimony trichloride to the ethanol, stir and dissolve at room temperature, then stir at 80° C. for 5 h, cool and age for 4 days to obtain an antistatic weathering agent with a solid content of 2.0 wt.%;
[0125] (3) The template is the same as in Example 1;
[0126] (4) Silica sol, template agent and antistatic weathering agent are mixed according to an effective solid content ratio of 1:0.8:0.02, and ethanol is added to adjust the solid content to 4wt.% to prepare a pre-coating solution. Finally, ethylene glycol butyl ether is added according to 5% of the mass of the pre-coating solution to prepare a coating solution.
[0127] A method for preparing dust-proof, antistatic and anti-reflective coated glass comprises the following steps:
[0128] The coating liquid is applied on the photovoltaic glass by roller coating, and then baked and cured at 160°C, and then tempered at 710°C to obtain dust-resistant, antistatic and anti-reflective coated glass.
[0129] Comparative Example 3
[0130] A method for preparing a coating solution comprises the following steps:
[0131] (1) 20 g of purified water, 25 g of ethanol, 0.1 g of dimethylformamide, and 0.6 g of ammonia water (the mass fraction concentration of ammonia water is 20%) were added to a conical flask with a magnetic stirrer in sequence to form liquid B (in liquid B, the mass of the stabilizer dimethylformamide is 0.5% of the mass of purified water), 25 g of tetraethyl orthosilicate and 25 g of ethanol were added to a constant pressure funnel to form liquid A, and the liquid A in the constant pressure funnel was added dropwise to the liquid B in the stirred conical flask at a constant speed for 25 min, and then the stirring was continued at room temperature for 5 h. After aging for 4 days, a silica sol with a solid content of 11.7 wt.% was obtained;
[0132] (2) Add 39.45 g of ethanol to another conical flask with a magnetic stirrer, then add 12.25 g of tin tetrachloride pentahydrate and 0.21 g of antimony trichloride to the ethanol, stir and dissolve at room temperature, then stir at 80° C. for 5 h, cool and age for 4 days to obtain an antistatic weathering agent with a solid content of 2.0 wt.%;
[0133] (3) The template is the same as in Example 1;
[0134] (4) Silica sol, template agent and antistatic weathering agent are mixed according to an effective solid content ratio of 1:0.6:0.02, and ethanol is added to adjust the solid content to 3wt.% to prepare a pre-coating solution. Finally, ethylene glycol butyl ether is added according to 5% of the mass of the pre-coating solution to prepare a coating solution.
[0135] A method for preparing coated glass comprises the following steps:
[0136] The coating liquid is applied to the photovoltaic glass by roller coating, then baked and cured at 160° C., and then tempered at 710° C. to obtain the coated glass.
[0137] Comparative Example 4
[0138] A method for preparing a coating solution comprises the following steps:
[0139] (1) 20 g of purified water, 25 g of ethanol, and 0.6 g of aqueous ammonia (the mass fraction concentration of aqueous ammonia is 20%) were added to a conical flask with a magnetic stirrer to form a liquid B, 20 g of tetraethyl orthosilicate and 25 g of ethanol were added to a constant pressure funnel to form a liquid A, and the liquid A in the constant pressure funnel was added dropwise to the liquid B in the conical flask under stirring at a constant speed for 25 min, and then the stirring was continued for 5 h at room temperature. After aging for 4 days, a silica sol with a solid content of 11.3 wt.% was obtained;
[0140] (2) Add 39.45 g of ethanol to another conical flask with a magnetic stirrer, then add 12.25 g of tin tetrachloride pentahydrate and 0.21 g of antimony trichloride to the ethanol, stir and dissolve at room temperature, then stir at 80° C. for 5 h, cool and age for 4 days to obtain an antistatic weathering agent with a solid content of 2.0 wt.%;
[0141] (3) The template is the same as in Example 1;
[0142] (4) Silica sol, template agent and antistatic weathering agent are mixed according to an effective solid content ratio of 1:0.6:0.02, and ethanol is added to adjust the solid content to 3wt.% to prepare a pre-coating solution. Finally, ethylene glycol butyl ether is added according to 5% of the mass of the pre-coating solution to prepare a coating solution.
[0143] A method for preparing coated glass comprises the following steps:
[0144] The coating liquid is applied to the photovoltaic glass by roller coating, then baked and cured at 160° C., and then tempered at 710° C. to obtain the coated glass.
[0145] Comparative Example 5
[0146] A method for preparing a coating solution comprises the following steps:
[0147] (1) 20 g of purified water, 25 g of ethanol, 0.01 g of dimethylformamide and 0.5 g of ammonia water (the mass fraction concentration of ammonia water is 20%) were added to a conical flask with a magnetic stirrer to form a B solution (in the B solution, the mass of the stabilizer dimethylformamide is 0.05% of the mass of the purified water), 30 g of tetraethyl orthosilicate and 25 g of ethanol were added to a constant pressure funnel to form a A solution, and the A solution in the constant pressure funnel was added dropwise to the B solution in the conical flask under stirring at a constant speed for 25 min, and then the stirring was continued at room temperature for 5 h. After aging for 4 days, a silica sol with a solid content of 10.6 wt.% was obtained;
[0148] (2) The template is the same as in Example 1;
[0149] (3) The silica sol and the template are mixed at an effective solid content ratio of 1:0.6, and ethanol is added to adjust the solid content to 3wt.% to prepare a pre-coating solution. Finally, ethylene glycol butyl ether is added at 5% of the mass of the pre-coating solution to prepare a coating solution.
[0150] A method for preparing coated glass comprises the following steps:
[0151] The coating liquid is applied to the photovoltaic glass by roller coating, then baked and cured at 160° C., and then tempered at 710° C. to obtain the coated glass.
[0152] Comparative Example 6
[0153] A method for preparing a coating solution comprises the following steps:
[0154] (1) 30 g of purified water, 25 g of ethanol, 0.01 g of dimethylacetamide, 0.6 g of ammonia water (the mass fraction concentration of ammonia water is 20%) and 0.01 g of polyethylene glycol were added to a conical flask with a magnetic stirrer to form a B solution (in the B solution, the mass of the stabilizer dimethylacetamide is 0.03% of the mass of the purified water), 15 g of tetraethyl orthosilicate and 25 g of ethanol were added to a constant pressure funnel to form a A solution, and the A solution in the constant pressure funnel was added dropwise to the B solution in the conical flask under stirring at a constant speed for 30 min, and then the stirring was continued at room temperature for 6 h. After aging for 5 days, a silica sol with a solid content of 5.0 wt.% was obtained;
[0155] (2) Add 39.45 g of ethanol to another conical flask with a magnetic stirrer, then add 8.75 g of tin tetrachloride pentahydrate and 0.12 g of aluminum chloride to the ethanol, stir and dissolve at room temperature, then stir at 80° C. for 5 h, cool and age for 4 days to obtain an antistatic weathering additive with a solid content of 1.8 wt.%;
[0156] (3) The template is the same as in Example 1;
[0157] (4) Silica sol, template agent and antistatic weathering agent are mixed according to an effective solid content ratio of 1:0.3:0.04, and ethanol is added to adjust the solid content to 3wt.% to prepare a pre-coating solution. Finally, ethylene glycol butyl ether is added according to 4% of the mass of the pre-coating solution to prepare a coating solution.
[0158] A method for preparing dust-proof, antistatic and anti-reflective coated glass comprises the following steps:
[0159] The coating liquid is applied on the photovoltaic glass by roller coating, and then baked and cured at 160°C, and then tempered at 710°C to obtain dust-resistant, antistatic and anti-reflective coated glass.
[0160] Product effect testing
[0161] Observation of the film layers formed by the plating solutions of Example 1 and Comparative Example 2: Figure 1 is a cross-sectional view of the coated glass of Example 1; Figure 2 2 is a cross-sectional view of the coated glass of Comparative Example 2. Figure 1-2 It can be seen that the film layer formed by the coating solution of Example 1 has a microscopic peak structure, while the film layer formed by the coating solution of Comparative Example 1 is relatively flat.
[0162] The following performance tests were performed on the coated glasses prepared in the above embodiments and comparative examples:
[0163] (1) Transmittance test: The transmittance of the film layer (T) is measured using the Beijing Aobote GST-3 air-floating table-top embossed glass spectral transmittance measuring instrument. The coated glass to be measured is placed with the film surface facing upward on the instrument's measuring table and moved to the measuring point. When the instrument starts measuring, the glass is moved to continuously measure a total of 12 transmittance data at different positions. The maximum and minimum values are removed and the average value is taken. The transmittance enhancement (ΔT) is the measured transmittance minus the transmittance of the substrate glass.
[0164] (2) Dust test: prepare a clean coated glass with a size of 300×300 mm and a clean crucible with an inner ring area of S. First weigh the crucible on a 1 / 10,000 balance, then add 3 g of prickly heat powder into the crucible and record the total weight G'. Then, use a fixing ring and an antistatic elastic rope to turn the crucible upside down on the film surface of the coated glass. Flip it over several times to allow the prickly heat powder to fully contact and adhere to the film surface. After the test, remove the crucible and weigh it to obtain G", and calculate the dust amount according to the following formula:
[0165] Dust content = (G'-G") / S, unit: g / m 2 .
[0166] Tests were performed on 3 different areas of 3 different coated glasses and the average value was taken.
[0167] (3) Antistatic test: The MODEL-100 surface resistance tester is used for testing. At least 12 different areas are selected on the same coated glass for testing, and the median result is taken as the final result.
[0168] (4) PCT High-Pressure Accelerated Aging Test: The coated glass to be tested is cut into square pieces of 300×300 mm in size and then placed vertically in a high-pressure accelerated aging test chamber with a 3 cm distance between the glass pieces. The test is then conducted continuously for 48 hours at a temperature of 121°C, a humidity of 100%, and 2 standard atmospheres. A pass indicates that the service life of the film layer is approximately 20 years.
[0169] The test results are shown in Table 1.
[0170] Table 1
[0171]
[0172]
[0173] It can be seen from Table 1 that all embodiments have good anti-dust and antistatic properties, and can pass the PCT accelerated aging test. At the same time, after the accelerated aging test, the film surface transmittance decreases less, and can maintain the same anti-dust performance as before the accelerated aging test, which can ensure long-term use stability in harsh environments.
[0174] Comparative Example 1 has good dust resistance and high transmittance, but it is difficult to pass the PCT accelerated aging test. The transmittance decreases significantly before and after the test, and the dust resistance also decreases. Comparative Example 2 uses hydrochloric acid as a catalyst, and the film surface does not have good dust resistance. In Comparative Example 3, the amount of stabilizer used in the coating solution is too much, and the particle size of the formed silica sol is too large, which will greatly reduce the transmittance performance of the film layer. In Comparative Example 4, no stabilizer is added to the coating solution, and the stability of the silica sol is poor. The transmittance of the formed film layer is low, and the dust resistance is poor. In Comparative Example 5, no antistatic weathering agent is added to the coating solution, the surface resistance is high, and it cannot pass the PCT accelerated aging test. In Comparative Example 6, the antistatic weathering agent in the coating solution is replaced by aluminum chloride, and the antistatic and weathering properties are poor.
[0175] In order to achieve high hardness, the traditional photovoltaic glass anti-reflection film will adjust the film to form a dense structure, which makes it easy to absorb dust. There is also a hydrophobic self-cleaning anti-reflection film, which is made of inorganic-doped organic silica sol, so that the film has super hydrophobic properties, which can repel surface dust after rainfall and achieve self-cleaning. However, this hydrophobic film is easily damaged by ultraviolet rays, resulting in poor performance; and the film is easy to form separate water droplets after being washed by rain, which will become spots mixed with water and dust after drying, greatly reducing the transmittance of the coated glass in this area.
[0176] The silica sol formed by the sol-gel method under alkaline catalytic conditions in the present invention has a granular structure, and the particle size can be freely controlled by changing the formula. After the silica sol, template agent and antistatic agent are matched and coated on the surface of photovoltaic glass, an uneven microscopic peak structure can be formed on the glass surface, giving the film layer good dust resistance. At the same time, the antistatic weathering agent provides good electrical conductivity for the film layer, which can effectively avoid the electrostatic adsorption generated by dust friction. In addition, the combination of silica sol and antistatic weathering agent can make the film layer have good weather resistance. After passing the PCT accelerated aging test, the film layer can still maintain a high transmittance and good dust and antistatic performance, so that the photovoltaic glass can maintain a clean surface during long-term use in harsh environments, extending the service life of the photovoltaic module and maintaining the stable power generation efficiency of the module.
Claims
1. A coating solution, characterized in that: Including silica sol, antistatic weathering additives, and template agents; The preparation process of the silica sol includes: mixing silicate with a diluent to obtain liquid A; mixing water, a stabilizer, and an alkaline catalyst to obtain liquid B; mixing liquid A and liquid B to react to prepare the silica sol; In the liquid B, the mass of the stabilizer is less than 0.35% of the mass of the water; The antistatic weathering agent includes tin halide and antimony halide.
2. The coating solution according to claim 1, characterized in that: The mass of the stabilizer is 0.01 to 0.35% of the mass of the water; and / or the silicate is selected from at least one of methyl orthosilicate, ethyl orthosilicate, orthopropyl orthosilicate, methyltrimethoxysilane, methyltriethoxysilane, methyltripropoxysilane, ethyltrimethoxysilane, ethyltriethoxysilane, ethyltripropoxysilane, dimethyldimethoxysilane, dimethyldiethoxysilane, dimethyldipropoxysilane, trimethylmethoxysilane or trimethylethoxysilane.
3. The coating solution according to claim 1, characterized in that: During the preparation of the B solution, a diluent and / or a pore-forming agent is also added.
4. The coating solution according to claim 1, characterized in that: The stabilizer includes at least one of diethanolamine, dimethylethanolamine, dimethylformamide or dimethylacetamide; and / or the alkaline catalyst includes at least one of ammonia water, sodium hydroxide or potassium hydroxide; and / or, in the liquid B, the mass ratio of water to the alkaline catalyst is 15-30: (0.1-1.0).
5. The coating solution according to claim 3, characterized in that: The pore-forming agent is polyethylene glycol.
6. The coating solution according to claim 3, characterized in that: When the liquid B contains a diluent and a pore-forming agent, the mass ratio of water to the diluent and the pore-forming agent is 15-30:(10-50):(0.01-0.2).
7. The coating solution according to claim 1, characterized in that: The mixed reaction of liquid A and liquid B is carried out at 15-40°C for 1-8 hours; and / or, after the reaction of liquid A and liquid B is completed, they are aged at room temperature for 2-6 days; and / or, the tin halide includes at least one of tin tetrachloride pentahydrate, tin tetrachloride, tin fluoride, and tin tetrabromide; and / or, the antimony halide includes at least one of antimony trichloride, antimony tribromide, and antimony pentafluoride, and antimony trichloride is more preferred.
8. The coating solution according to claim 1, characterized in that: In the coating solution, the mass ratio of silica sol, antistatic weathering agent and template agent is 1:(0.1-1.0):(0.005-0.1) in terms of effective solid content ratio; and / or, the coating solution also includes a volatilization inhibitor.
9. The method for preparing the coating solution according to any one of claims 1 to 8, characterized in that: The following steps are involved: The silica sol is mixed with an antistatic weather-resistant additive and a template agent to obtain the coating solution.
10. A glass, characterized in that: A film layer formed by the plating solution according to any one of claims 1 to 8.
Citation Information
Patent Citations
Antireflective coating solution and preparation method thereof, as well as photovoltaic glass and preparation method of photovoltaic glass
CN102531406A
Nanometer core-shell silicon dioxide microsphere as well as preparation and application of antireflection composite coating solution
CN105964195A
Coating with antireflection, dustproof, antifogging and antistatic functions and preparation method thereof
CN115404003A
Template agent for anti-reflection coating liquid with small particle size and high stability and application of template agent
CN116102685A
Coating composition for forming ultra water repellentcoating layer, preparation method thereof and caotingmethod using the same
KR1020060011218A