Low-melting-point metal halide scintillator ink as well as preparation method and application thereof in customized X-ray imaging

Through the physical mixing of low-melting point metal halide scintillator ink with polymer polymer, a high-transparent, recoverable scintillation screen was prepared, which solved the problems of light crosstalk and light scattering in X-ray imaging, significantly improving spatial resolution and reducing Cost has promoted the development of X-ray imaging technology.

CN118895065APending Publication Date: 2024-11-05KUNMING UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410833126.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-26
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

In the existing X-ray imaging technology, the complex process of scintillator materials, high cost, insufficient environmental stability, and problems with light crosstalk and light scattering lead to insufficient spatial resolution.

Method used

The low-melting point metal halide scintillator ink and its preparation method are used to prepare a scintillator screen by physically mixing it with polymers, and use low-temperature thermoplastic ink to achieve customized imaging, suppress light scattering and light crosstalk, and improve spatial resolution.

Benefits of technology

The spatial resolution of X-ray imaging is significantly improved, cost reduction, and resource savings are alleviated by recyclable utilization, and internal light scattering problems are alleviated.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004912370700000011
    Figure HDA0004912370700000011
  • Figure HDA0004912370700000012
    Figure HDA0004912370700000012
  • Figure HDA0004912370700000021
    Figure HDA0004912370700000021
Patent Text Reader

Abstract

The invention relates to low-melting-point metal halide scintillator ink as well as a preparation method and application thereof in customized X-ray imaging, and belongs to the technical field of X-ray imaging. The structural general formula of the metal halide scintillator ink is AmBXn, m and n respectively represent stoichiometric ratios of elements on crystal lattice positions of A bit and X bit, m is greater than or equal to 1 and less than or equal to 2, and n is greater than or equal to 1 and less than or equal to 7; a site is an organic group C16H36N or Bmmim, B site is a metal element Cu, Mn, Sb or Te, and X is halogen Cl, Br or I. After a metal halide scintillator (C16H36N) mBXn or [Bmmim] mBXn is directly melted, the metal halide scintillator is brushed or sprayed on the surface of an object to be detected to complete a customization process, and high-resolution X-ray imaging is realized. According to the low-melting-point metal halide scintillator ink, the transparency and machinability can be improved through structural design, meanwhile, the viscosity is reduced, the brushing or spraying performance is optimized, the problems of light scattering, light crosstalk and the like in the imaging process are effectively inhibited, and high spatial resolution and low detection limit are obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a low-melting-point metal halide scintillator ink and a preparation method thereof and application thereof in customized X-ray imaging, belonging to the technical field of X-ray imaging. Background Art

[0002] X-ray imaging technology plays an important role in the fields of medical treatment, industrial security, etc. This technology benefits from the different absorption effects of X-rays on materials of different densities, so it can achieve non-destructive detection of the internal structure of the material. However, in the current commercial X-ray imaging system, the scintillator materials commonly used are CdWO4, GOS:Tb, NaI:Tl, CsI:Tl or Bi4Ge3O 12 Single crystal materials face problems such as complex processing, high cost, insufficient environmental stability and serious afterglow phenomenon, which have seriously hindered the development of X-ray imaging technology.

[0003] In recent years, metal halide scintillators have been used as favorable candidates for high-performance commercial scintillator materials due to their advantages such as simple preparation process, high dielectric constant, wide absorption range, high light absorption coefficient, efficient exciton luminescence, short fluorescence lifetime and tunable wavelength. However, there are still a series of problems to be solved in practical applications, such as the inability of the scintillator screen to be closely attached to the object to be tested, causing light scattering problems; the scintillator screen and the object to be tested do not match the geometric dimensions, resulting in light crosstalk problems. Therefore, how to reasonably and effectively solve or suppress the above problems is the key to achieving high spatial resolution X-ray imaging.

[0004] In order to solve the problem of insufficient spatial resolution of X-ray imaging caused by light crosstalk and light scattering, researchers proposed a solution of physically mixing metal halides with high molecular polymers (PMMA, PVDF, PDMS, PS, epoxy resin, etc.) to prepare scintillator screens. However, during the preparation process of this type of scintillator screens, serious particle agglomeration occurs, and the uniformity of the scintillator screen is severely reduced, thereby reducing the spatial resolution. Summary of the invention

[0005] In view of the problem of insufficient spatial resolution of X-ray imaging caused by existing light crosstalk and light scattering problems, the present invention proposes a low-melting-point metal halide scintillator ink and its preparation method and application in customized X-ray imaging. The present invention proposes a customized imaging strategy of low-temperature thermoplastic scintillator ink. The low-melting-point metal halide scintillator ink can realize customized imaging of irregular objects to be tested, greatly suppressing external light scattering and light crosstalk problems; at the same time, the scintillator screen proposed by the present invention has high transparency, which greatly alleviates the problem of internal light scattering, and significantly improves the spatial resolution of the scintillator screen. In addition, the scintillator ink can be recycled, effectively saving costs and promoting the development of the field of X-ray imaging.

[0006] A low melting point metal halide scintillator ink, the metal halide scintillator ink has a general structural formula of: A m BX n , where m and n represent the stoichiometric ratio of the elements at the A and X lattice positions, 1≤m≤2, 1≤n≤7; the A position is an organic group C 16 H 36 N or Bmmim, B is a metal element Cu, Mn, Sb or Te, and X is a halogen Cl, Br or I.

[0007] The low-melting-point metal halide scintillator ink not only exhibits extremely high light yield and stability, but also has a relatively low melting point (50-140° C.), and can be customized by brushing or spraying, thereby suppressing the problems of light scattering and light crosstalk, and effectively improving spatial resolution.

[0008] The method for preparing the low melting point metal halide scintillator ink comprises the following specific steps:

[0009] (1) The metal halide scintillator ink has the general structural formula A m BX n The stoichiometric ratio (C 16 H 36 N)X or [Bmmim]X, BX are dissolved in a solvent in proportion to form C 16 H 36 N system precursor solution or Bmmim system precursor solution;

[0010] (2)C 16 H 36 The N system precursor solution is slowly evaporated at a temperature of 30-60°C for 12-24h to obtain (C 16 H 36 N) m BX n Scintillator ink;

[0011] (3) The precursor solution of the Bmmim system is heated at a temperature of 120 to 150°C for 30 to 120 minutes and then cooled to room temperature to obtain [Bmmim] m BX n Scintillator ink.

[0012] Preferably, the solvent in step (1) is DMF, DMSO, dichloromethane, acetonitrile, alcohol or isopropanol.

[0013] Preferably, in step (1), BX is CuI, MnCl2, SbCl3, MnBr2 or TeCl4.

[0014] The step (1) prepares C 16 H36 When preparing the N system precursor solution, 1-15% of the volume of the solvent is added with commercially available hypophosphorous acid.

[0015] Application of the low-melting-point metal halide scintillator ink in customized X-ray imaging: preparing a customized scintillator screen using the low-melting-point metal halide scintillator ink.

[0016] Preparation method of the customized scintillation screen:

[0017] 1)(C 16 H 36 N) m BX n The scintillator ink is melted at a temperature of 60 to 130°C to form (C 16 H 36 N) m BX n Scintillator melt, (C 16 H 36 N) m BX n The scintillator melt is brushed or sprayed onto the target surface and cured for 10-30 minutes to obtain a customized (C 16 H 36 N) m BX n Flashing screen;

[0018] 2) [Bmmim] m BX n The scintillator ink is melted at a temperature of 50 to 150°C to form [Bmmim] m BX n Scintillator melt, [Bmmim] m BX n The scintillator melt is brushed or sprayed onto the target surface and cured for 10-30 minutes to obtain a customized [Bmmim] m BX n Flashing screen.

[0019] The beneficial effects of the present invention are:

[0020] (1) The present invention uses a solution method to prepare a metal halide scintillator ink (C 16 H 36 N) m BX n , [Bmmim] m BX n , it has high stability and a low melting point (50-140°C), and can be recycled and reused;

[0021] (2) The metal halide scintillator (C 16 H36 N) m BX n , [Bmmim] m BX n Customized scintillation screens can be prepared by brushing or spraying onto the target surface; scintillation screens have the characteristics of thin thickness, high density, customization, and also have extremely high light yield, spatial resolution and low detection limit;

[0022] (3) The metal halide scintillator ink of the present invention has high scintillation, high transparency, low viscosity and recoverability. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 For Example 1 (C 16 H 36 N) CuI2 metal halide scintillator XRD pattern;

[0024] Figure 2 For Example 1 (C 16 H 36 N) Thermogravimetric analysis spectrum of CuI2 metal halide scintillator;

[0025] Figure 3 For Example 1 (C 16 H 36 N) Emission spectrum of CuI2 metal halide scintillator under X-ray excitation;

[0026] Figure 4 The XRD pattern of the [Bmmim]2MnCl4 metal halide scintillator in Example 4;

[0027] Figure 5 This is the emission spectrum of the [Bmmim]2MnCl4 metal halide scintillator under X-ray excitation in Example 4;

[0028] Figure 6 The X-ray imaging effect diagram of the [Bmmim]2MnCl4 metal halide scintillator screen for a flat object (a) and a special-shaped object (b) in Example 4;

[0029] Figure 7 is the XRD spectrum of the [Bmmim]2SbCl5 metal halide scintillator in Example 5;

[0030] Figure 8 This is the emission spectrum of the [Bmmim]2SbCl5 metal halide scintillator under X-ray excitation in Example 5;

[0031] Fig. 9 This is the emission spectrum of the [Bmmim]2TeCl6 metal halide scintillator under X-ray excitation in Example 7. DETAILED DESCRIPTION

[0032] The present invention is further described in detail below in conjunction with specific implementation modes, but the protection scope of the present invention is not limited to the described contents.

[0033] Embodiment 1: The chemical formula of the metal halide scintillator in this embodiment is (C 16 H 36 N)CuI2;

[0034] A method for preparing a low melting point metal halide scintillator ink, the specific steps are as follows:

[0035] (1) According to the general structural formula of metal halide scintillator ink (C 16 H 36 N)CuI2 stoichiometric ratio (1:1), (C 16 H 36 N)I and CuI were dissolved in DMF solvent (DMF solvent contained 15% of commercial hypophosphorous acid by volume) in proportion to form C 16 H 36 N system precursor solution;

[0036] (2)C 16 H 36 The N system precursor solution was placed in a fume hood and the solvent was slowly evaporated at 30°C for 12 h to obtain (C 16 H 36 N) CuI2 scintillator ink;

[0037] The XRD spectrum of the metal halide scintillator in this example is shown in Figure 1 , compared with the calculated spectrum, the experimental data showed no impurity peaks, indicating that a pure phase was prepared;

[0038] This embodiment (C 16 H 36 N) CuI2 metal halide scintillator has a low melting point of about 100°C. Its thermogravimetric analysis shows Figure 2 ;(C 16 H 36 N) CuI2 metal halide scintillator emits white light, and the emission spectrum under X-ray excitation is shown in Figure 3 ;

[0039] Application of the low melting point metal halide scintillator ink in customized X-ray imaging: Preparation of customized scintillator screen using low melting point metal halide scintillator ink:

[0040] (C 16 H 36 N)CuI2 scintillator ink is melted at 90-100℃ to form (C 16 H36 N)CuI2 scintillator melt,

[0041] (C 16 H 36 N)CuI2 scintillator melt is brushed or sprayed onto the target surface and cured for 30 minutes to obtain a customized (C 16 H 36 N) CuI2 scintillation screen;

[0042] This embodiment (C 16 H 36 N) CuI2 scintillator screen has the characteristics of thin thickness, high density and recoverability, which can achieve high-quality customized X-ray imaging;

[0043] This embodiment (C 16 H 36 N) The resolution of CuI2 metal halide scintillator screen is 18lpmm -1 .

[0044] Embodiment 2: The chemical formula of the metal halide scintillator in this embodiment is (C 16 H 36 N)2MnCl4;

[0045] A method for preparing a low melting point metal halide scintillator ink, the specific steps are as follows:

[0046] (1) According to the general structural formula of metal halide scintillator ink (C 16 H 36 N)2MnCl4 stoichiometric ratio (2:1), at a temperature of 90-100°C, (C 16 H 36 N)Cl and MnCl2 were dissolved in DMSO solvent (DMSO solvent contained 7% of commercial hypophosphorous acid by volume) in proportion to form C 16 H 36 N system precursor solution;

[0047] (2)C 16 H 36 The N system precursor solution was placed in a fume hood and the solvent was slowly evaporated at 40°C for 18 h to obtain (C 16 H 36 N) 2MnCl4 scintillator ink;

[0048] This embodiment (C 16 H 36 N)2MnCl4 metal halide scintillator has a low melting point, about 60°C.

[0049] (C 16 H 36N)2MnCl4 metal halide scintillator emits green light;

[0050] Application of the low melting point metal halide scintillator ink in customized X-ray imaging: Preparation of customized scintillator screen using low melting point metal halide scintillator ink:

[0051] (C 16 H 36 N)2MnCl4 scintillator ink is melted at 60-75℃ to form (C 16 H 36 N)2MnCl4 scintillator melt, (C 16 H 36 N)2MnCl4 scintillator melt is brushed or sprayed onto the target surface and cured for 20 minutes to obtain a customized (C 16 H 36 N) 2MnCl4 scintillation screen;

[0052] This embodiment (C 16 H 36 N)2MnCl4 scintillator screen has the characteristics of thin thickness, high density and recoverability, which can achieve high-quality customized X-ray imaging;

[0053] This embodiment (C 16 H 36 N)2MnCl4 metal halide scintillator screen has a resolution of 12lpmm -1 .

[0054] Embodiment 3: The chemical formula of the metal halide scintillator in this embodiment is (C 16 H 36 N)2SbCl5;

[0055] A method for preparing a low melting point metal halide scintillator ink, the specific steps are as follows:

[0056] (1) According to the general structural formula of metal halide scintillator ink (C 16 H 36 N)2SbCl5 stoichiometric ratio (2:1), at a temperature of 120-130°C, (C 16 H 36 N)Cl and SbCl3 were dissolved in DMF solvent (DMF solvent contained 1% of commercial hypophosphorous acid by volume of solvent) in proportion to form C 16 H 36 N system precursor solution;

[0057] (2)C 16 H 36 The N system precursor solution was placed in a fume hood and the solvent was slowly evaporated at 50°C for 24 h to obtain (C 16H 36 N)2SbCl5 scintillator ink;

[0058] This embodiment (C 16 H 36 N)2SbCl5 metal halide scintillator has a low melting point, about 120°C.

[0059] (C 16 H 36 N)2SbCl5 metal halide scintillator emits yellow light;

[0060] Application of the low melting point metal halide scintillator ink in customized X-ray imaging: Preparation of customized scintillator screen using low melting point metal halide scintillator ink:

[0061] (C 16 H 36 N)2SbCl5 scintillator ink is placed at a temperature of 120-130°C and melted to form (C 16 H 36 N)2SbCl5 scintillator melt, (C 16 H 36 N)2SbCl5 scintillator melt is brushed or sprayed onto the target surface and cured for 25 minutes to obtain a customized (C 16 H 36 N)2SbCl5 scintillation screen;

[0062] This embodiment (C 16 H 36 N)2SbCl5 scintillator screen has the characteristics of thin thickness, high density and recoverability, which can achieve high-quality customized X-ray imaging;

[0063] This embodiment (C 16 H 36 The resolution of N2SbCl5 metal halide scintillator screen is 13lpmm -1 .

[0064] Embodiment 4: The chemical formula of the metal halide scintillator in this embodiment is [Bmmim]2MnCl4;

[0065] A method for preparing a low melting point metal halide scintillator ink, the specific steps are as follows:

[0066] (1) According to the stoichiometric ratio (2:1) of the general structural formula of the metal halide scintillator ink [Bmmim]2MnCl4, [Bmmim]Cl and MnCl2 are added into a container in proportion, and heated and dissolved in an acetonitrile solvent at a temperature of 130 to 140° C. to form a Bmmim system precursor solution;

[0067] (2) The precursor solution of the Bmmim system is placed in a fume hood, heated at a temperature of 140-150° C. for 60 min, and slowly cooled for more than 4 hours until the temperature drops below 25° C. to obtain [Bmmim]2MnCl4 scintillator ink;

[0068] The XRD spectrum of the metal halide scintillator in this example is shown in Figure 4 , compared with the calculated spectrum, the experimental data showed no impurity peaks, indicating that a pure phase was prepared;

[0069] The metal halide scintillator [Bmmim]2MnCl4 in this embodiment has a relatively low melting point, which is about 50°C;

[0070] [Bmmim]2MnCl4 metal halide scintillator emits green light, and the emission spectrum under X-ray excitation is shown in Figure 5 ;

[0071] Application of the low melting point metal halide scintillator ink in customized X-ray imaging: Preparation of customized scintillator screen using low melting point metal halide scintillator ink:

[0072] The [Bmmim]2MnCl4 scintillator ink is placed at a temperature of 60 to 80° C. to melt to form a [Bmmim]2MnCl4 scintillator melt, and the [Bmmim]2MnCl4 scintillator melt is brushed or sprayed onto the surface of the target object and cured for 20 minutes to obtain a customized [Bmmim]2MnCl4 scintillator screen;

[0073] The [Bmmim]2MnCl4 scintillation screen of this embodiment has the characteristics of thin thickness, high density, and recoverability, and can achieve high-quality customized X-ray imaging;

[0074] The resolution of the [Bmmim]2MnCl4 metal halide scintillator screen in this embodiment is 20lpmm -1 The imaging effects of the scintillator ink coated plane (a) and the shaped object (b) under X-ray are shown in Figure 6 .

[0075] Embodiment 5: The chemical formula of the metal halide scintillator in this embodiment is [Bmmim]2SbCl5;

[0076] A method for preparing a low melting point metal halide scintillator ink, the specific steps are as follows:

[0077] (1) According to the stoichiometric ratio (2:1) of the general structural formula of the metal halide scintillator ink [Bmmim]2SbCl5, [Bmmim]Cl and SbCl3 are added into a high-pressure container in proportion, and heated and dissolved in an isopropanol solvent at a temperature of 120 to 125° C. to form a Bmmim system precursor solution;

[0078] (2) The precursor solution of the Bmmim system is placed in a fume hood, heated at a temperature of 120-125° C. for 120 min, and slowly cooled for more than 5 hours until the temperature drops below 20° C. to obtain [Bmmim]2SbCl5 scintillator ink;

[0079] The XRD spectrum of the metal halide scintillator [Bmmim]2SbCl5 in this example is shown in Figure 7 , compared with the calculated spectrum, the experimental data showed no impurity peaks, indicating that a pure phase was prepared;

[0080] The metal halide scintillator [Bmmim]2SbCl5 in this embodiment has a relatively low melting point, which is about 90°C;

[0081] [Bmmim]2SbCl5 metal halide scintillator emits yellow light, and the emission spectrum under X-ray excitation is shown in Figure 8 ;

[0082] Application of the low melting point metal halide scintillator ink in customized X-ray imaging: Preparation of customized scintillator screen using low melting point metal halide scintillator ink:

[0083] The [Bmmim]2SbCl5 scintillator ink is placed at a temperature of 90 to 100° C. to melt to form a [Bmmim]2SbCl5 scintillator melt, and the [Bmmim]2SbCl5 scintillator melt is brushed or sprayed onto the surface of the target object and cured for 30 minutes to obtain a customized [Bmmim]2SbCl5 scintillator screen;

[0084] The [Bmmim]2SbCl5 scintillator screen of this embodiment has the characteristics of thin thickness, high density, and recoverability, and can achieve high-quality customized X-ray imaging;

[0085] The resolution of the [Bmmim]2SbCl5 metal halide scintillator screen in this embodiment is 12lpmm -1 .

[0086] Embodiment 6: The chemical formula of the metal halide scintillator in this embodiment is [Bmmim]2MnBr4;

[0087] A method for preparing a low melting point metal halide scintillator ink, the specific steps are as follows:

[0088] (1) According to the structure of the metal halide scintillator ink and the stoichiometric ratio of [Bmmim]2MnBr4 (2:1), [Bmmim]Br and MnBr2 are added into a container in proportion, and heated and dissolved in acetonitrile solvent at a temperature of 90 to 100° C. to form a Bmmim system precursor solution;

[0089] (2) The precursor solution of the Bmmim system is placed in a fume hood, heated at a temperature of 130-140° C. for 30 min, and slowly cooled for more than 3 hours until the temperature drops below 20° C. to obtain [Bmmim]2MnBr4 scintillator ink;

[0090] The metal halide scintillator [Bmmim]2MnBr4 in this embodiment has a relatively low melting point, which is about 60°C;

[0091] [Bmmim]2MnBr4 metal halide scintillator emits green light;

[0092] Application of the low melting point metal halide scintillator ink in customized X-ray imaging: Preparation of customized scintillator screen using low melting point metal halide scintillator ink:

[0093] The [Bmmim]2MnBr4 scintillator ink is placed at a temperature of 60 to 70° C. to melt to form a [Bmmim]2MnBr4 scintillator melt, and the [Bmmim]2MnBr4 scintillator melt is brushed or sprayed onto the surface of the target object and cured for 30 minutes to obtain a customized [Bmmim]2MnBr4 scintillator screen;

[0094] The [Bmmim]2MnBr4 scintillator screen of this embodiment has the characteristics of thin thickness, high density, and recoverability, and can achieve high-quality customized X-ray imaging;

[0095] The resolution of the [Bmmim]2MnBr4 metal halide scintillator screen in this embodiment is 14lpmm -1 .

[0096] Embodiment 7: The chemical formula of the metal halide scintillator in this embodiment is [Bmmim]2TeCl6;

[0097] A method for preparing a low melting point metal halide scintillator ink, the specific steps are as follows:

[0098] (1) According to the stoichiometric ratio (2:1) of the general structural formula of the metal halide scintillator ink [Bmmim]2TeCl6, [Bmmim]Cl and TeCl4 are added into a container in proportion, and heated and dissolved in a DMF solvent at a temperature of 120 to 130° C. to form a Bmmim system precursor solution;

[0099] (2) The precursor solution of the Bmmim system is placed in a fume hood, heated at 120-130° C. for 50 min, and slowly cooled for more than 4 hours until the temperature drops below 20° C. to obtain [Bmmim]2TeCl6 scintillator ink;

[0100] The metal halide scintillator [Bmmim]2TeCl6 in this embodiment has a relatively low melting point, which is about 140°C;

[0101] [Bmmim]2TeCl6 metal halide scintillator emits red light, and the emission spectrum under X-ray excitation is shown in Fig. 9 ;

[0102] Application of the low melting point metal halide scintillator ink in customized X-ray imaging: Preparation of customized scintillator screen using low melting point metal halide scintillator ink:

[0103] The [Bmmim]2TeCl6 scintillator ink is placed at a temperature of 130-150° C. to melt to form a [Bmmim]2TeCl6 scintillator melt, and the [Bmmim]2TeCl6 scintillator melt is brushed or sprayed onto the surface of the target object and cured for 40 minutes to obtain a customized [Bmmim]2TeCl6 scintillator screen;

[0104] The [Bmmim]2TeCl6 scintillator screen of this embodiment has the characteristics of thin thickness, high density, and recoverability, and can achieve high-quality customized X-ray imaging;

[0105] The resolution of the [Bmmim]2TeCl6 metal halide scintillator screen in this embodiment is 12lpmm -1 .

[0106] The specific implementation modes of the present invention are described in detail above, but the present invention is not limited to the above implementation modes, and various changes can be made within the knowledge scope of ordinary technicians in this field without departing from the purpose of the present invention.

Claims

1. A low melting point metal halide scintillator ink, Features: The general structural formula of the metal halide scintillator ink is: m BX n , where m and n represent the stoichiometric ratio of the elements at the A and X lattice positions, 1≤m≤2, 1≤n≤7; the A position is an organic group C 16 H 36 N or Bmmim, B is a metal element Cu, Mn, Sb or Te, and X is a halogen Cl, Br or I.

2. The method for preparing the low melting point metal halide scintillator ink according to claim 1, It is characterized in that The specific steps are as follows: (1) According to the structural formula A of the metal halide scintillator ink m BX n The stoichiometric ratio (C 16 H 36 N)X or [Bmmim]X, BX are dissolved in a solvent in proportion to form C 16 H 36 N system precursor solution or Bmmim system precursor solution; (2)C 16 H 36 The N system precursor solution is slowly evaporated at a temperature of 30-60°C for 12-24h to obtain (C 16 H 36 N) m BX n Scintillator ink; (3) The precursor solution of the Bmmim system is heated at a temperature of 120 to 150°C for 30 to 120 minutes and then cooled to room temperature to obtain [Bmmim] m BX n Scintillator ink.

3. The method for preparing the low melting point metal halide scintillator ink according to claim 2, Features: The solvent of step (1) is DMF, DMSO, dichloromethane, acetonitrile, alcohol or isopropanol.

4. The method for preparing the low melting point metal halide scintillator ink according to claim 2, Features: Step (1) BX is CuI, MnCl 2 、SbCl 3 、MnBr 2 or TeCl 4 .

5. The method for preparing the low melting point metal halide scintillator ink according to claim 2, Features: Step (1) Preparation of C 16 H 36 When preparing the N system precursor solution, add 1-15% of the solvent volume of hypophosphorous acid.

6. Application of the low melting point metal halide scintillator ink according to claim 1 in customized X-ray imaging, Features: Customized scintillator screens were prepared using low melting point metal halide scintillator inks.

7. The use according to claim 6, Features: Preparation method of customized scintillation screen: 1)(C 16 H 36 N) m BX n The scintillator ink is melted at a temperature of 60-130°C to form (C 16 H 36 N) m BX n Scintillator melt, (C 16 H 36 N) m BX n The scintillator melt is brushed or sprayed onto the target surface and cured for 10-30 minutes to obtain a customized (C 16 H 36 N) m BX n Flashing screen; 2) [Bmmim] m BX n The scintillator ink is melted at a temperature of 50 to 150°C to form [Bmmim] m BX n Scintillator melt, [Bmmim] m BX n The scintillator melt is brushed or sprayed onto the target surface and cured for 10-30 minutes to obtain a customized [Bmmim] m BX n Flashing screen.