Photocuring high-resistance PVD (Physical Vapor Deposition) primer universal for metal and glass and preparation method of photocuring high-resistance PVD primer
By using aliphatic polyurethane acrylate, modified polyester acrylate and other materials in PVD primer, the combination of phosphate acrylate and silane coupling agents, the primer in the prior art under harsh environments is solved. Inadequate adhesion performance and durability problems have achieved efficient and universal primer for glass and metal substrates, and have high temperature resistance and boiling resistance.
Patent Information
- Application Number
- CN202410988408.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-07-23
AI Technical Summary
The prior art lacks light cured PVD primer that can meet the common glass and hardware substrates, high temperature resistance and boiling resistance, resulting in the problem of the coating being prone to foaming and insufficient adhesion performance under harsh environments.
Combining phosphate acrylates, modified polyester acrylates, epoxy acrylates, active monomer diluents, adhesion accelerators, photoinitiators and solvents, combined with phosphate acrylates and silane coupling agents, Photocured high resistance metal, glass universal PVD primer is prepared by specific formula ratios and process steps.
The primer has achieved excellent adhesion, high temperature resistance and boiling resistance on glass and metal substrates, avoiding the foaming and coloring of the coating, and improving the stability and commercial value of the product.
Smart Images

Figure BDA0004958159490000071
Abstract
Description
Technical Field
[0001] The invention relates to the field of coatings, in particular to the field of C09D163 / 00, and more specifically to a photocurable high-resistance metal and glass universal PVD primer and a preparation method thereof. Background Art
[0002] At present, common coating processes include primer and topcoat. Primer refers to the primer directly applied on the surface of the substrate, which can be regarded as a basic material of the substrate. During the coating process, the primer can form a strong bond with the surface of the substrate, so that the coating can be firmly attached to the substrate, which can effectively prevent the coating from peeling or falling off. The primer can fill the unevenness and pores on the surface of the substrate, making the coating surface smoother and improving the beauty and texture. The coating will be affected by factors such as wear, oxidation, and ultraviolet radiation during use, resulting in a decrease in the performance of the coating. Therefore, the primer can increase the stability and weather resistance of the coating, making the coating more durable and less susceptible to damage from external factors. Topcoat is the second process after the primer is applied. It is generally the last layer of paint applied in multiple layers of paint and has the function of protecting the primer.
[0003] Primers usually need to have high adhesion and weather resistance to be better used in practice; the prior art CN116656216A discloses a high-temperature resistant glass electroplating UV primer, including UV polymer, epoxy acrylate, aliphatic polyurethane acrylate resin, monomer, initiator, additive and solvent, which has high adhesion and high temperature resistance after being bonded to the surface of the glass substrate; the prior art CN103097473B discloses a primer composition for metal materials, which can have high adhesion to the surfaces of various metal materials such as ordinary steel, stainless steel, aluminum alloy, copper, galvanized steel, etc., and has excellent bonding strength and bonding durability; however, there are relatively few PVD primers that can meet the requirements of glass and hardware substrates and are resistant to high temperatures and boiling water. Summary of the invention
[0004] In order to solve the above-mentioned technical problems, the first aspect of the present invention provides a photocurable high-resistance metal and glass universal PVD primer, the preparation raw materials of which include, by weight: 8-12 parts of aliphatic polyurethane acrylate, 10-18 parts of modified polyester acrylate, 110-20 parts of epoxy acrylate, 5-10 parts of active monomer diluent, 5-10 parts of adhesion promoter, 1-5 parts of photoinitiator, 45-55 parts of solvent, and 0.1-1 part of auxiliary agent.
[0005] Preferably, the functionality of the aliphatic polyurethane acrylate is 2-6; when the functionality is 2, it includes ST808, ST852, ST2260H, ST8052, ST8052M, ST8132; when the functionality is 6, it includes ST8736; all are purchased from Shanghai Santong.
[0006] More preferably, the viscosity of the aliphatic polyurethane acrylate at 60° C. is 50,000-70,000 cps, which is ST808.
[0007] Preferably, the modified polyester acrylate includes ST6052, purchased from Santong Technology.
[0008] Preferably, the functionality of the epoxy acrylate is 2-6.
[0009] Further preferably, the functionality of the epoxy acrylate is 2; as an implementable case, the 2-functionality epoxy acrylate includes one or more of ST500, ST502, ST5027, ST602, ST604M, ST605, ST615, ST625, all of which are purchased from Shanghai Santong.
[0010] More preferably, the viscosity of the epoxy acrylate at 60° C. is 4000-6000 cps, which is ST604M.
[0011] Preferably, the active monomer diluent is an acrylate monomer, including one or more of dicyclopentenyl acrylate, isobornyl methacrylate, triethylene glycol diacrylate, pentaerythritol triacrylate, hydroxyethyl methacrylate, and tetrahydrofuran acrylate.
[0012] Further preferably, the acrylate monomer comprises hydroxyethyl methacrylate and pentaerythritol triacrylate in a mass ratio of (3-6):(4-6).
[0013] Preferably, the adhesion promoter comprises a phosphate acrylate promoter and a silane coupling agent in a mass ratio of 1:(1-4).
[0014] More preferably, the phosphate acrylate accelerator has a viscosity of 100-600 cps at 60°C.
[0015] More preferably, the phosphate acrylate accelerator has a viscosity of 160-320 cps at 60° C., model number SZ1771, and is purchased from Shanghai Santong.
[0016] Further preferably, the silane coupling agent includes one of Z-6040, Z-6020, Z-6030, Z-6011, and Z-6121, all of which are purchased from Dow Corning.
[0017] More preferably, the silane coupling agent is Z-6040.
[0018] The present invention does not further limit the photoinitiator, and any initiator that can promote the photocuring process of the system may be used, including but not limited to: STCure-184, STCure-1173, STCure-917, STCure-1219 of Shanghai Santong; long-day photoinitiator 1103, 1055, MBF; one or more of IGM omnirad184, IGM omnirad651; IGM omnirad 184 and IGM omnirad 651 are preferred in the present invention, and the mass ratio is 1:1.
[0019] Preferably, the solvent includes one or more of ethyl acetate, butyl acetate, methyl isobutyl ketone, propylene glycol methyl ether, xylene, ethanol, n-butanol, ethylene glycol butyl ether, ethylene glycol monoethyl ether, ethylene glycol monoethyl ether acetate, butanone, and acetone.
[0020] Further preferably, the solvent includes ethyl acetate, butyl acetate, methyl isobutyl ketone, and propylene glycol methyl ether in a mass ratio of (10-30):(10-20):(5-20):(1-10).
[0021] The additives in the present invention may include antioxidants, defoamers, leveling agents, pigments, etc.; antioxidants include antioxidant 1010, antioxidant 168, etc.; defoamers include BYK-024, BYK-011, etc.; leveling agents include tego-1484, tego-410, BYK-306, etc.; pigments include iron oxide, chrome yellow, titanium dioxide, zinc oxide, etc.; they can be used as needed according to the actual production and processing conditions. The preferred additive in the present invention is the leveling agent BYK-306.
[0022] The second aspect of the present invention provides a method for preparing a photocurable photocurable high-resistance metal and glass universal PVD primer, comprising the following steps:
[0023] S1. Adding materials: preparing epoxy acrylate, modified polyester acrylate, aliphatic polyurethane acrylate and active monomer diluent according to the formula ratio to obtain component A; preparing adhesion promoter, photoinitiator, auxiliary agent and solvent according to the formula ratio to obtain component B;
[0024] S2, dispersion: the prepared A component material is dispersed at a high speed of 500-1000rpm for 30-60min, and stirring is stopped after mixing evenly to obtain A solution; the prepared B component material is dispersed at a medium speed of 200-500rpm for 5-20min, and stirring is stopped after mixing evenly to obtain B solution;
[0025] S3, mixing: slowly pour solution B into solution A, and stir at a low speed of 100-200 rpm until the mixture is evenly mixed.
[0026] Beneficial Effects
[0027] (i) In order to ensure that the primer has excellent adhesion performance, the present invention preferably uses aliphatic polyurethane acrylate ST808 and modified polyester acrylate ST6052 as raw materials; polyurethane acrylate has excellent low temperature resistance; it has high mechanical strength, excellent adhesion to glass substrates, and has excellent recovery and good paintability, and is suitable for large-area bonding.
[0028] (ii) Polyurethane acrylate is susceptible to moisture and foaming, and powdering of the base film after curing is relatively common; this limits the application of PVD primers in certain harsh environments. Therefore, the present invention adds epoxy acrylate to the preparation system, which can reduce the foaming performance of the coating and improve the high temperature and boiling resistance of the primer. However, the viscosity of epoxy acrylate should not be too high. In the present invention, ST604M with a viscosity of 4000-6000cps at 25°C is preferred. If the viscosity is too high, it is not conducive to the dispersion uniformity of the raw material system and will cause a certain decrease in the stability of the primer.
[0029] (III) In the present invention, acrylate monomers are selected as active monomer diluents, especially hydroxyethyl methacrylate and pentaerythritol triacrylate. Hydroxyethyl methacrylate can improve the adhesion to the glass substrate through hydrogen bonding, while pentaerythritol triacrylate can increase the curing speed and leveling performance of the primer, thereby improving the weather resistance of the primer.
[0030] (IV) The phosphate acrylate selected in the present invention, especially SZ1771 with a viscosity of 100-800cps at 60°C, can significantly improve the adhesion performance of the primer on the surface of the metal substrate, mainly because the phosphoric acid group in the phosphate acrylate has a slight phosphating effect on the metal substrate, which is beneficial to improve the adhesion to the metal layer; at the same time, since the active monomer diluent in the present invention includes hydroxyethyl methacrylate, the technical effect common to glass and hardware substrates can be achieved.
[0031] (V) In order to improve the high temperature resistance of the primer, the inventors found that the use of silane coupling agent Z-6040 can achieve the technical effect of high temperature resistance. At the same time, Z-6040 and phosphate acrylate accelerator are compounded. After the primer is used, it is not easy to have the problem of coating coloration and high temperature bubbling, and the product stability is significantly improved.
[0032] (VI) The photocurable high-resistance metal and glass universal PVD primer provided by the present invention has both water boiling resistance and high temperature resistance, and at the same time achieves the technical effect of being universal for glass substrates and metal substrates. In addition, the primer of the present invention has good storage stability and a simple preparation process, and has good commercial use value. DETAILED DESCRIPTION
[0033] Example 1
[0034] The first aspect of this example provides a photocurable high-resistance metal and glass general-purpose PVD primer, the raw materials for its preparation are calculated by weight as follows: 10 parts of aliphatic polyurethane acrylate, 12.5 parts of modified polyester acrylate, 14 parts of epoxy acrylate, 9 parts of active monomer diluent, 3 parts of adhesion promoter, 50 parts of solvent, 4 parts of photoinitiator, and 0.1 part of auxiliary agent.
[0035] The aliphatic polyurethane acrylate has a functionality of 2 and a viscosity of 50,000-70,000 cps at 60° C. It is ST808 and is purchased from Shanghai Santong.
[0036] The modified polyester acrylate is ST6052, purchased from Shanghai Santong.
[0037] The epoxy acrylate is ST604M, with a functionality of 2 and a viscosity of 4000-6000 cps at 60° C., purchased from Shanghai Santong.
[0038] The active monomer diluent is hydroxyethyl methacrylate and pentaerythritol triacrylate, with a mass ratio of 5:4; the hydroxyethyl methacrylate is HEMA-98 from Wanhua Chemical, and the pentaerythritol triacrylate is EM235 from Changxing Chemical.
[0039] The adhesion promoter is a phosphate acrylate promoter and a silane coupling agent Z-6040, with a mass ratio of 1:2; the phosphate acrylate promoter is ST1771 purchased from Shanghai Santong, and the silane coupling agent Z-6040 is purchased from Dow Corning.
[0040] The photoinitiators are IGM omnirad184 and IGM omnirad 651, with a mass ratio of 1:1.
[0041] The auxiliary agent is the leveling agent BYK-306.
[0042] The solvent is ethyl acetate, butyl acetate, methyl isobutyl ketone and propylene glycol methyl ether, and the mass ratio is 4:3:2:1.
[0043] The second aspect of this example provides a method for preparing a photocurable high-resistance metal and glass universal PVD primer, which is specifically prepared by the following steps:
[0044] S1. Adding materials: preparing epoxy acrylate, modified polyester acrylate, aliphatic polyurethane acrylate and active monomer diluent according to the formula ratio to obtain component A; preparing adhesion promoter, photoinitiator, auxiliary agent and solvent according to the formula ratio to obtain component B;
[0045] S2, dispersion: the prepared A component material is dispersed at a high speed of 800 rpm for 30 min, and stirring is stopped after mixing evenly to obtain A solution; the prepared B component material is dispersed at a medium speed of 400 rpm for 10 min, and stirring is stopped after mixing evenly to obtain B solution;
[0046] S3, mixing: slowly pour solution B into solution A, and stir at a low speed of 100 rpm until the mixture is evenly mixed.
[0047] Example 2
[0048] The specific implementation method of this example is the same as that of Example 1, except that the weight percentages of the raw materials are different; the raw materials for preparation are calculated by weight percentage as follows: 12 parts of aliphatic polyurethane acrylate, 10 parts of modified polyester acrylate, 15 parts of epoxy acrylate, 9 parts of active monomer diluent, 2.5 parts of adhesion promoter, 50 parts of solvent, 4 parts of photoinitiator, and 0.1 part of auxiliary agent; the adhesion promoter is a phosphate acrylate promoter and a silane coupling agent Z-6040, and the weight ratio is 2:3.
[0049] Example 3
[0050] The specific implementation method of this example is the same as that of Example 1, except that the weight percentages of the raw materials are different; the raw materials for preparation are calculated by weight percentage as follows: 8 parts of aliphatic polyurethane acrylate, 10 parts of modified polyester acrylate, 16.5 parts of epoxy acrylate, 9 parts of active monomer diluent, 4 parts of adhesion promoter, 50 parts of solvent, 4 parts of photoinitiator, and 0.1 part of auxiliary agent; the adhesion promoter is a phosphate acrylate promoter and a silane coupling agent Z-6040, and the weight ratio is 1:1.
[0051] Example 4
[0052] The specific implementation of this example is the same as that of Example 1, except that the aliphatic polyurethane acrylate is Shanghai Santong ST8142.
[0053] Comparative Example 1
[0054] The specific implementation of this example is the same as that of Example 1, except that the phosphate acrylate accelerator is Nippon Kayaku PM-2 (hydroxyethyl methacrylate phosphate) with a viscosity of 600 to 3000 mPa.s / 25°C.
[0055] Comparative Example 2
[0056] The specific implementation of this example is the same as that of Example 1, except that the silane coupling agent is Shin-Etsu KBE-903 from Japan.
[0057] Comparative Example 3
[0058] The specific implementation of this example is the same as that of Example 1, except that the adhesion promoter is 2 parts, which is the silane coupling agent Dow Corning Z-6040 (excluding ST1771).
[0059] Comparative Example 4
[0060] The specific implementation of this example is the same as that of Example 1, except that the adhesion promoter is 2 parts, namely ST1771 (excluding Dow Corning Z-6040).
[0061] Performance Evaluation
[0062] The primers obtained in Examples 1-4 and Comparative Examples 1-4 were electroplated onto glass substrates and then performance tests were performed. The test data are listed in Table 1. The specific electroplating method includes substrate treatment and vacuum electroplating, as follows:
[0063] Substrate treatment: The substrate can be ordinary glass or tinplate. Use a clean cloth dipped in isopropyl alcohol to remove contaminants on the substrate.
[0064] Vacuum plating:
[0065] 1. Primer electroplating: air spraying, air pressure 0.6MPa; spray gun caliber 1.3mm; spray gun and substrate surface distance 25cm, paint mist atomization angle 35°, paint film thickness 10μm; preheating at 55℃ for 5min; 900mJ / cm 2 UV curing, cooling at room temperature 25℃ for 30min after curing;
[0066] 2. Electroplated metal layer: vacuum aluminum is plated on the surface of the photocurable coating. The thickness of the electroplating is 0.3 μm and the surface density is 0.27 g / m 2 .
[0067] Test items:
[0068] 1. Adhesion test: The products of the embodiments and comparative examples were made into samples, and the test was carried out according to the reference standard GB / T9286-1998 using the 100-grid method.
[0069] 2. Water resistance test: Boil in water at 100℃ for 1h, observe whether bubbling, peeling, or coloring occurs on the surface, and measure the adhesion after boiling.
[0070] 3. High temperature resistance test: Bake at 180℃ for 2h, observe whether there is bubbling, peeling or coloring on the surface, and measure the adhesion after baking.
[0071] Table 1
[0072]
[0073] Note: “--” means: Since the first conventional adhesion test is 0B, there is no need to conduct subsequent water and temperature resistance tests.
Claims
1. A light-cured high-resistance metal and glass universal PVD primer, characterized in that: The raw materials for preparing the primer include, by weight: 8-12 parts of aliphatic polyurethane acrylate, 10-18 parts of modified polyester acrylate, 10-20 parts of epoxy acrylate, 5-10 parts of active monomer diluent, 5-10 parts of adhesion promoter, 1-5 parts of photoinitiator, 45-55 parts of solvent and 0.1-1 part of auxiliary agent.
2. The light-curing high-resistance metal and glass universal PVD primer according to claim 1, characterized in that: The functionality of the aliphatic polyurethane acrylate is 2-6.
3. The light-curing high-resistance metal and glass universal PVD primer according to claim 2, characterized in that: The viscosity of the aliphatic polyurethane acrylate at 60° C. is 50,000-70,000 cps.
4. The light-curing high-resistance metal and glass universal PVD primer according to claim 3, characterized in that: The functionality of the epoxy acrylate is 2-6.
5. The light-curing high-resistance metal and glass universal PVD primer according to claim 4, characterized in that: The viscosity of the epoxy acrylate at 60° C. is 4000-6000 cps.
6. The light-cured high-resistance metal and glass universal PVD primer according to claim 5, characterized in that: The active monomer diluent is an acrylate monomer, including one or more of dicyclopentenyl acrylate, isobornyl methacrylate, triethylene glycol diacrylate, pentaerythritol triacrylate, hydroxyethyl methacrylate, and tetrahydrofuran acrylate.
7. The light-cured high-resistance metal and glass universal PVD primer according to claim 6, characterized in that: The adhesion promoter comprises a phosphate acrylate promoter and a silane coupling agent, and the mass ratio of the phosphate acrylate promoter to the silane coupling agent is 1:(1-4).
8. The light-curing high-resistance metal and glass universal PVD primer according to claim 7, characterized in that: The viscosity of the phosphate acrylate accelerator at 60° C. is 100-600 cps; the silane coupling agent includes one of Z-6040, Z-6020, Z-6030, Z-6011, and Z-6121.
9. The light-cured high-resistance metal and glass universal PVD primer according to claim 8, characterized in that: The solvent includes one or more of ethyl acetate, butyl acetate, methyl isobutyl ketone, propylene glycol methyl ether, xylene, ethanol, n-butanol, ethylene glycol butyl ether, ethylene glycol monoethyl ether, ethylene glycol monoethyl ether acetate, butanone, and acetone.
10. A method for preparing the light-cured high-resistance metal and glass universal PVD primer according to claim 9, characterized in that: The following steps are involved: S1. Adding materials: preparing epoxy acrylate, modified polyester acrylate, aliphatic polyurethane acrylate, and active monomer diluent according to a formula ratio to obtain component A; preparing adhesion promoter, photoinitiator, auxiliary agent and solvent according to a formula ratio to obtain component B; S2, dispersion: the prepared A component material is dispersed at a high speed of 500-1000rpm for 30-60min, and stirring is stopped after mixing evenly to obtain A solution; the prepared B component material is dispersed at a medium speed of 200-500rpm for 5-20min, and stirring is stopped after mixing evenly to obtain B solution; S3, mixing: slowly pour solution B into solution A, stir at a low speed of 100-200 rpm until evenly mixed.
Citation Information
Patent Citations
primer composition
CN103097473B
High-temperature-resistant glass electroplating UV primer and preparation method thereof
CN116656216A
Ultraviolet curing coating for glass
CN106675377A
Vacuum plating UV primer as well as preparation method and application thereof
CN115029040A
Cited By
Glass ceramic metallization UV vacuum plating coating and preparation process thereof
CN119708967A