Low-viscosity delayed-gelling solvent-free two-component aliphatic polyurea coating and application thereof
Through the combination of low viscosity, regel solvent-free two-component aliphatic polyurea coating and low pressure sprayer, the defects of water-based coating construction performance and powder coating are solved, and the efficiency, environmental protection and wear resistance of container coating are achieved. and anticorrosion requirements.
Patent Information
- Application Number
- CN202410988605.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-05
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing water-based container coatings are prone to bulging, falling off and cracking during construction, and have low wear resistance and hardness, high energy consumption. The powder coating film is hard and brittle, has poor impact resistance, and has high energy consumption. The investment is large and it is difficult to meet the strict requirements of container coating.
Develop a low viscosity, regel-free solvent-free two-component aliphatic polyurea coating, using amino resin components and isocyanate curing agent components, using aldehyde imine as active diluents and urea-containing formate polyisocyanate As the main component, solvate-free film coating is achieved in combination with a low-pressure sprayer.
Improve the anti-corrosion, environmental protection and construction efficiency of container coatings, realize solvate-free film coating, reduce energy consumption and sewage treatment difficulty, enhance the impact and wear resistance of the coating, and meet the high efficiency of the container. Environmentally friendly coating needs.
Smart Images

Figure CN118895082A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of coatings, and in particular relates to a low-viscosity, slow-gelling solvent-free two-component aliphatic polyurea coating and application thereof. Background Art
[0002] Container coatings refer to coatings used for the inside and outside of containers, including workshop pre-coating primer, container interior paint, container exterior intermediate layer, topcoat and container bottom anti-corrosion paint. Container coatings play an important role in cargo transportation and container stacking. They are not only a key means to extend the service life of containers and protect cargo, but also an important guarantee for improving the appearance quality and environmental protection safety of containers.
[0003] Container coatings need to meet certain specific performance requirements, such as corrosion resistance, abrasion resistance, high temperature and humidity resistance, weather resistance, and repairability. Because containers are exposed to a variety of harsh environmental conditions during use, such as wind and rain, strong ultraviolet radiation, high-salinity marine atmospheric erosion, and seawater impact, etc. Therefore, the performance requirements for container coatings are very strict.
[0004] Since the China Container Coating Industry Association issued relevant standards in April 2017, requiring domestic standard dry container coating production lines to replace the original solvent-based coating system with water-based coating systems, ordinary dry container coatings in my country's container coating industry have basically achieved water-based coating replacement. Although these water-based coatings are close to traditional oil-based coatings in terms of performance, the construction performance, anti-corrosion and protection performance of water-based coatings still need to be further optimized and improved.
[0005] Due to its own characteristics, waterborne container coatings must maintain a certain temperature and humidity range and good ventilation conditions during the construction process, otherwise it is very easy to produce bulging, shedding and cracking. Therefore, quality accidents often occur in the actual construction of waterborne container coatings. In addition, waterborne container coatings are relatively thin and have low strength. Their wear resistance and hardness are lower than those of traditional coatings, resulting in reduced resistance to friction and scratches during storage and transportation. At the same time, in terms of energy consumption and sewage treatment, waterborne container coatings have higher energy consumption than traditional solvent-based coatings, and because waterborne coatings contain water-soluble substances, sewage treatment becomes more difficult.
[0006] In order to overcome the defects of water-based paint in container coating, the industry has begun to try to replace water-based paint with powder coating, and called powder coating an environmentally friendly coating with "zero three wastes". However, powder coating also has its own inherent defects, including hard and brittle coating, poor impact resistance, high energy consumption for coating baking (high temperature>160℃) and large investment in coating equipment.
[0007] Therefore, the art is in urgent need of finding a new type of coating, which can avoid the above-mentioned performance and construction process defects of water-based coatings due to the presence of water medium on the one hand, and can comprehensively overcome the shortcomings of powder coatings on the other hand. Summary of the invention
[0008] Purpose of the Invention
[0009] The purpose of this patent is to invent a low-viscosity, slow-gel solvent-free two-component aliphatic polyurea coating, which can be used for solvent-free thin-film coating on containers through a special two-component low-pressure sprayer, thereby improving the anti-corrosion performance, environmental protection performance and construction efficiency of container coatings, and promoting new developments in container and other industrial coating technologies.
[0010] Technical Solution
[0011] A low-viscosity, slow-gelling solvent-free two-component aliphatic polyurea coating, comprising an amino resin component and an isocyanate curing agent component, characterized in that:
[0012] (1) The amino resin component contains
[0013] a at least one polyaspartic acid ester resin and its content is 60-90% by weight of the resin component, and most preferably 70-80%; b at least one reactive diluent characterized by aldimine and its content is 40-10% by weight of the resin component, and most preferably 30-10%;
[0014] (2) The isocyanate curing agent component contains
[0015] c. polyisocyanate containing allophanate and its content is 30-95% of the curing agent component;
[0016] d. other polyisocyanates and their content is 5-70% of the curing agent component.
[0017] The polyaspartic acid ester resin described in a has a structure as shown in Formula 1:
[0018]
[0019] Wherein R1, R2, R3, and R4 are C1-C4 alkyl groups, which may be the same or different; X may be the following structure (Formula 2):
[0020]
[0021] It can also be the following structure (Formula 3):
[0022]
[0023] Or formula 4:
[0024] -CH2-CH2-CH2-CH2-CH2-CH2-
[0025] Formula 4
[0026] Aliphatic polyaspartic acid ester products containing the structures of Formula 2, Formula 3 and Formula 4 in Formula 1 are available on the market, such as AP-104, AP-105 and AP-102 from Weixin Paint.
[0027] The at least one polyaspartic acid ester resin mentioned in a refers to one or more combinations of adducts obtained by Michael addition reaction of aliphatic polyamines and unsaturated dialkyl maleates or dialkyl fumarates, including but not limited to the above-mentioned polyaspartic acid esters, and the combination ratio can be arbitrary; the content of 60-90% of the resin component means that the total weight of the polyaspartic acid esters formed by the above-mentioned one or more combinations accounts for 60-90% of the weight of the amino resin component, and most preferably 60-80%.
[0028] The active diluent characterized by aldimine described in b refers to a difunctional aldehyde formed by nucleophilic addition of a diprimary amine and a monofunctional aldehyde, wherein the diprimary amine has the following structure (Formula 5):
[0029] H2N——R——NH2
[0030] Formula 5
[0031] Where R represents C2-C 18 aliphatic, aromatic or alicyclic groups, which may be saturated or unsaturated. Suitable diamines include, but are not limited to, ethylenediamine, ethylene glycol diamine, propylene glycol diamine and alicyclic diamines. Suitable alicyclic diamines include, but are not limited to, p-(m-)cyclohexanediamine, p-(m-)cyclohexanedimethylamine, isophoronediamine, 2,4-diaminomethylcyclohexane, 4,4-diaminodicyclohexylmethane, 3,3-dimethyl-4,4-diaminodicyclohexylmethane, and the like.
[0032] The monofunctional aldehydes include but are not limited to acetaldehyde, propionaldehyde, butyraldehyde, isobutyraldehyde, benzaldehyde and the like.
[0033] The synthesis principle and method of the above-mentioned bifunctional aldimine can be found in Chapter 16 and Chapter 26 of Organic Chemistry (Douglas C. Naik et al., Chemical Industry Press, first edition, 1984). Corresponding commercial products can also be obtained from the market, such as Aldrez A or Aldrez BH from Iconrez Limited, UK.
[0034] The active diluent containing at least one aldimine as mentioned in b refers to one or more combinations including but not limited to the above-mentioned bifunctional aldehydes, and the combination ratio can be arbitrary; the content of 40-10% of the resin component means that the total weight of the bifunctional aldehydes composed of the above-mentioned one or more combinations accounts for 10-40% of the weight of the amino resin component, and most preferably 10-30%.
[0035] The polyisocyanate containing allophanate described in c refers to the product of the reaction of monohydroxy alcohol and polyisocyanate, which can be theoretically obtained by reacting 1 mol of monohydroxy alcohol with 2 mol of polyisocyanate. The actual reaction process can be a two-step method: firstly, monohydroxy alcohol reacts with polyisocyanate to obtain carbamate isocyanate (carbamateization), and then reacts with polyisocyanate to obtain polyisocyanate containing allophanate (allophamateization); or it can be a one-step method: that is, the monohydroxy compound directly reacts with an excess (mol ratio>1) of polyisocyanate in situ to obtain the polyisocyanate containing allophanate. The patent of the present invention preferably adopts a one-step method.
[0036] The above-mentioned allophanate-containing polyisocyanate has the following structure (Formula 6):
[0037]
[0038] Wherein R2 is the residue of monohydroxy alcohol, R represents an aliphatic alkane group containing C6-C10, and n is 1-4.
[0039] The above-mentioned suitable polyisocyanates include, but are not limited to, hexamethylene diisocyanate (HDI), isophorone diisocyanate (IPDI), dicyclohexylmethane diisocyanate (HMDI), 1,4-cyclohexane diisocyanate (CHDI) and cyclohexane dimethylene diisocyanate (HXDI), etc. The above-mentioned polyisocyanates can be used alone or mixed in any proportion.
[0040] The above-mentioned suitable monohydroxy compound refers to a monohydroxy compound with a molecular weight of 30-500, preferably 30-300, which can be a monohydroxy alcohol monomer, or a monohydroxy polyoxypropylene ether, polyoxyethylene ether or monohydroxy polyester, including but not limited to methanol, ethanol, propanol, isopropanol, allyl alcohol, butanol, amyl alcohol, hexanol, 2-ethylhexanol, and a fatty alcohol containing 10-20 carbon atoms and polypropylene oxide monomethyl ether, polyethylene oxide monomethyl ether, etc. The above-mentioned monohydroxy compounds can be used alone or mixed in any proportion.
[0041] The above-mentioned urethanization reaction and allophanation reaction are carried out according to the common process control method in the field of polyurethane chemistry, that is, the urethanization reaction temperature is controlled at 50-80°C until the NCO% content reaches the theoretical value; the allophanation reaction temperature is controlled at 90-120°C until the NCO% content reaches the theoretical value. In the one-step reaction process, the actual temperature and time control are also carried out according to the above-mentioned two reaction stages of urethanization and allophanation, and the corresponding NCO% theoretical value is monitored until the end point.
[0042] The content of the allophanate polyisocyanate in c is 30-95% of the curing agent component, which means that the weight of the allophanate polyisocyanate accounts for 30-95% of the total weight of the isocyanate curing agent component, and most preferably 50-70%.
[0043] The other polyisocyanates described in d are aliphatic polyisocyanates or modified products thereof, including but not limited to HDI trimer, HDI biuret, IPDI trimer or adducts thereof. They can be used alone or in any proportion.
[0044] The content of other polyisocyanates in d is 70-5% of the curing agent component, which means that the weight of the polyisocyanates accounts for 70-5% of the total weight of the isocyanate curing agent component, and most preferably 50-30%.
[0045] In the amino resin component, in addition to at least one polyaspartic acid ester resin and an active diluent having aldimine properties, fillers, coupling agents, dispersants, thixotropic agents, pigments, leveling agents, defoamers, ultraviolet light absorbers and antioxidants may be added as needed.
[0046] The filler can be calcium carbonate, talc, titanium dioxide, silicon powder, barium sulfate, etc. They can be used alone or mixed in any proportion. The total amount of the filler can account for 10-30% of the total weight of the resin component, and most preferably 10-20%.
[0047] The coupling agent can be KH-550, KH-560, KH-602, etc. The amount of the coupling agent used is 0.1%-1% of the total weight of the pigment and filler in the resin component, preferably 0.1-0.5%.
[0048] The dispersant may be BYK-110, BYK-163, BYK-180, etc. The amount of the dispersant used is determined according to the supplier's recommendations.
[0049] The thixotropic agent can be fumed silica, kaolin, attapulgite, etc. The thixotropic agent can be used alone or mixed in any proportion. The total amount of the thixotropic agent used is 0-20%, preferably 0-15%.
[0050] The pigment can be carbon black, titanium dioxide, iron yellow, iron red, phthalocyanine blue, etc. The amount of pigment used depends on the color requirements of the coating.
[0051] The leveling agent can be BYK-333, BYK-354, etc. The leveling agent can be used alone or mixed in any proportion, and the amount used is determined according to the supplier's recommendation.
[0052] The defoamer can be BYK-066N, BYK-085, etc. The defoamer can be used alone or mixed in any proportion, and the amount used is determined according to the supplier's recommendation.
[0053] The ultraviolet light absorber can be 1130, 770 and 292, etc. The ultraviolet light absorber can be used alone or mixed in any proportion, and the amount used is determined according to the supplier's recommendation.
[0054] The antioxidants described can be 1010, B225 and 330, etc. The antioxidants can be used alone or mixed in any proportion, and the amount used is determined according to the supplier's recommendation.
[0055] The preparation method of the amino resin component of the low-viscosity, slow-gelling solvent-free two-component aliphatic polyurea coating described in the present invention is implemented in the following order:
[0056] 1 First, weigh polyaspartic acid ester or its mixture and mix and stir evenly in a container.
[0057] 2. Add measured coupling agent, dispersant, leveling agent, defoamer, UV absorber, antioxidant and other additives, and stir thoroughly.
[0058] 3. Add the measured filler, thixotropic agent and color paste and stir thoroughly, then increase the stirring speed (2000rpm) and disperse at high speed for 30 minutes.
[0059] 4. Add a measured amount of active diluent having aldimine properties and stir evenly to obtain the amino resin component.
[0060] The preparation method of the polyisocyanate curing agent component of a low-viscosity, slow-gelling solvent-free two-component aliphatic polyurea coating described in the present invention is carried out in the following order:
[0061] 1 First, weigh the allophanate-containing polyisocyanate into a container.
[0062] 2. Add other polyisocyanates in measured amounts and stir evenly to obtain the curing agent component.
[0063] The reaction ratio of the low-viscosity, slow-gelling solvent-free two-component aliphatic polyurea coating is calculated based on the total amino equivalents of the secondary amino groups of the polyaspartic acid resin and the (potential) primary amino groups of the aldimine in the amino resin component and the total isocyanate equivalents in the curing agent component, and NCO / (NH+NH2)=1.1-1.3:1, preferably 1.1-1.15:1. The weight mixing ratio of the amino resin component to the curing agent component is controlled in the range of 1:1-1:0.1, preferably 1:1-1:0.5.
[0064] The present invention further relates to the application of a low-viscosity, slow-gelling solvent-free two-component aliphatic polyurea coating on containers, which is characterized by achieving continuous thin-film spraying construction through a special two-component low-pressure air sprayer.
[0065] The special two-component low-pressure air sprayer is a sprayer customized for the low-viscosity, slow-gelling solvent-free two-component aliphatic polyurea coating involved in the patent of this invention. Its main technical specifications are shown in Table 1:
[0066] Table 1 Main technical specifications of two-component low-pressure sprayer
[0067]
[0068]
[0069] The design of the two-component low-pressure sprayer is based on the low viscosity and slow gel properties of the solvent-free two-component aliphatic polyurea coating involved in the patent of this invention. The low viscosity property ensures that the two-component mixture has good compatibility and low mixing energy, so it can be mixed using a static mixer; and the slow gel property ensures that the two-component materials have a sufficiently long flow time (Pot-Life) after mixing without gelling and solidifying, so that the static mixer can operate for a long time, avoiding the blockage and shutdown of the static mixer and the mixed material delivery pipe due to the gelling of the materials.
[0070] definition
[0071] Among them, "solvent-free" means that the solid content of the sprayed material is 100%, that is, it does not contain any VOCs; "thin film spraying" means that the dry film thickness after spraying can be controlled within the range of 80-140μm; "aliphatic polyurea coating" refers to a two-component polyaspartic acid ester polyurea coating with aliphatic isocyanate as curing agent.
[0072] The "two-component low-pressure sprayer" involved in the patent of this invention refers to a two-component sprayer with a nominal pipeline pressure of less than 1.5 MPa and capable of air atomization.
[0073] Beneficial Effects
[0074] Two-component solvent-free polyurea is a type of coating composed of amino resin and isocyanate curing agent. It has excellent impact resistance, friction resistance, aging resistance and corrosion resistance, and can be quickly cured at room temperature. It is the fastest-growing new type of high-performance environmentally friendly synthetic coating.
[0075] The development process of polyurea coatings has always been in line with the requirements of increasingly environmental protection and high performance in the field of coatings. So far, two-component solvent-free polyurea coatings are divided into two systems: aromatic and aliphatic. The former uses terminal (primary) amino polyether and aromatic isocyanate as raw materials. Its characteristics are high viscosity and fast curing speed of two-components, and it must be constructed using special high-pressure airless spray equipment. Therefore, it cannot meet the requirements of container film coating (80-140μm) and flatness and decorativeness. The aliphatic polyurea system is a new type of polyurea coating. It uses secondary amino compounds and aliphatic isocyanate as raw materials, and has the characteristics of relatively low two-component viscosity and relatively moderate curing speed. Therefore, aliphatic polyurea coatings are usually applied by hand brushing and roller coating to obtain a smooth and flat coating. However, manual brushing and roller coating cannot meet the requirements of container film coating and efficient construction.
[0076] In fact, using a sprayer to achieve continuous thin-film coating of two-component solvent-free aliphatic polyurea coatings has always been the goal of the industry. The molecular structure and characteristics of polyaspartic acid ester resins and their compatible aliphatic isocyanate curing agents determine that these resins and curing agents have unique viscosity and reactivity, which can meet the requirements of manual construction in a solvent-free state, but cannot achieve continuous thin-film coating using a low-pressure air sprayer in a solvent-free state. This is because the viscosity of polyaspartic acid ester resins and their curing agents (≥2500mPas.) and the operable time after mixing the two components (10-15min) limit the use of ordinary low-pressure air spraying. Therefore, in recent years, the spraying construction of two-component aliphatic polyurea coatings generally requires the addition of 25-40% of volatile solvents to reduce the viscosity of the material and extend the operable time, but cannot achieve solvent-free thin-film coating.
[0077] 1One of the innovations of the present invention is that aldimine is used as a reactive diluent in the resin component. Using aldimine as a reactive diluent can significantly reduce the viscosity of the resin component, thereby avoiding the use of volatile solvents (VOCs) to achieve solvent-free spraying. At the same time, aldimine also has the function of a latent curing agent. By selecting and combining the activity of the polyaspartic acid ester resin in the resin component, the resin component and the curing agent component are mixed to produce a significant delayed curing effect, that is, a slow gel effect, thereby extending the flowable time (Pot-Linfe) of the mixed material.
[0078] 2 The second innovation of the present invention is that the curing agent component uses allophanate polyisocyanate as the main component. Since allophanate and aldimine have good compatibility, the compatibility between the curing agent component and the resin component is improved, and the flowability and product performance of the two components after mixing are further improved.
[0079] 3 It is precisely because of the above two innovative points that the two-component solvent-free aliphatic polyurea coating involved in the patent of this invention has the characteristics of low viscosity and slow gelation, so that it can be sprayed in a solvent-free thin film by a two-component low-pressure sprayer, thereby maximizing the outstanding advantages of the two-component solvent-free aliphatic polyurea coating, such as excellent performance, energy saving and environmental protection, convenience and high efficiency.
[0080] 4 The coating structure advantages and energy-saving and environmental protection advantages of the two-component solvent-free aliphatic polyurea coating involved in the present invention patent applied on containers are described in Table 2, Table 3 and Table 4 respectively:
[0081] Table 2 Comparison of coating structure between solvent-free polyurea coating and water-based coating for containers
[0082]
[0083] Table 3 Comparison of energy saving effects of solvent-free polyurea coating process for packaging
[0084]
[0085] Table 4 Comparison of emission reduction effects of packaging solvent-free polyurea coating process
[0086]
[0087] It can be seen from Table 2, Table 3 and Table 4 that the two-component solvent-free polyurea coating involved in the patent of the present invention has significant advantages in shortening the process of container painting, improving production efficiency, saving coating baking energy consumption and reducing "three wastes" emissions. BRIEF DESCRIPTION OF THE DRAWINGS
[0088] Figure 1 is the infrared spectrum of allophanate-containing polyisocyanate A1;
[0089] Figure 2 is the infrared spectrum of allophanate-containing polyisocyanate A2;
[0090] Figure 3 It is the infrared spectrum of allophanate-containing polyisocyanate A3. DETAILED DESCRIPTION
[0091] The main raw materials used in the embodiments of the present invention are shown in Table 5:
[0092] Table 5 List of main raw materials of examples
[0093]
[0094] Main testing instrument: Fourier transform infrared spectrometer WAF-530 (Beijing North Branch Rayleigh Analytical Instrument Co., Ltd.)
[0095] Rotational Viscometer SNB-AIShanghai Nirun Intelligent Technology Co., Ltd.
[0096] Synthesis of Allophanate-Containing Polyisocyanate
[0097] Synthesis of Example 1A1
[0098] Add 400g HDI to a 1000mL four-necked flask, and then install an electric stirrer, a thermometer, a condenser, a nitrogen tube and a dropping funnel. Replace the air in the flask with nitrogen twice and keep the nitrogen flowing. Start stirring and start dripping 35.6g isopropanol. Control the dripping speed so that the reaction temperature does not exceed 70°C. The entire dripping process is completed within 30 minutes. After the dripping is completed, keep the reaction at 70°C for about 2 hours until the NCO% content of the reaction material reaches 40.2%.
[0099] Keep stirring and nitrogen flowing, slowly raise the temperature of the reaction material to 90°C, add 1.3g of zinc decanoate to continue the reaction, then the material begins to gradually heat up, and the reaction stops when the temperature reaches 120°C. When the temperature drops to 60°C, add 0.4g of phosphoric acid and keep stirring for 30 minutes, then continue to cool to 40°C and discharge.
[0100] The obtained material was used to remove excess HDI using a thin film evaporator or a molecular evaporator to obtain 252.4 g of a clear, transparent allophanate-containing polyisocyanate with a measured NCO% of 14.9% and a viscosity of 2218 mPas., recorded as A1.
[0101] Figure 1 This is the infrared spectrum of A1, where 2271cm -1 The peak at 1714 cm is isocyanate. -1 The peak at is allophanate.
[0102] Synthesis of Example 2A2
[0103] Add 400g HDI to a 1000mL four-necked flask, and then install an electric stirrer, a thermometer, a condenser, a nitrogen tube and a dropping funnel. Replace the air in the flask with nitrogen twice and keep the nitrogen flowing. Start stirring and start dripping 187.4g MPPG-300. Control the dripping speed so that the reaction temperature does not exceed 70°C. The entire dripping process is completed within 30 minutes. After the dripping is completed, keep the reaction at 70°C for about 2 hours until the NCO% content of the reaction material reaches 30.3%.
[0104] Keep stirring and nitrogen flowing, slowly raise the temperature of the reaction material to 90°C, add 1.3g of zinc decanoate to continue the reaction, then the material begins to gradually heat up, and the reaction stops when the temperature reaches 120°C. When the temperature drops to 60°C, add 0.4g of phosphoric acid and keep stirring for 30 minutes, then continue to cool to 40°C and discharge.
[0105] The obtained material was used to remove excess HDI using a thin film evaporator or a molecular evaporator to obtain 228 grams of clear, transparent allophanate-containing polyisocyanate with a measured NCO% of 9.1% and a viscosity of 1631 mPas., recorded as A2.
[0106] Figure 2 This is the infrared spectrum of A2, where 2269cm -1 The peak at 1716 cm is isocyanate. -1 The peak at is allophanate.
[0107] Example 3 Synthesis of A3
[0108] Add 200g HDI and 200g IPDI to a 1000mL four-necked flask, and then install an electric stirrer, a thermometer, a condenser, a nitrogen tube and a dropping funnel. Replace the air in the flask with nitrogen twice and keep the nitrogen flowing. Start stirring and start dripping 31.0g isopropanol. Control the dripping speed so that the reaction temperature does not exceed 70°C. The entire dripping process is completed within 30 minutes. After the dripping is completed, keep the reaction at 70°C for about 2 hours until the NCO% content of the reaction material reaches 35.1%.
[0109] Keep stirring and nitrogen flowing, slowly raise the temperature of the reaction material to 90°C, add 1.3g of zinc decanoate to continue the reaction, then the material begins to gradually heat up, and the reaction stops when the temperature reaches 120°C. When the temperature drops to 60°C, add 0.4g of phosphoric acid and keep stirring for 30 minutes, then continue to cool to 40°C and discharge.
[0110] The obtained material was used to remove excess HDI using a thin film evaporator or a molecular evaporator to obtain 168 grams of clear, transparent allophanate-containing polyisocyanate with a measured NCO% of 15.1% and a viscosity of 2936 mPas., recorded as A3.
[0111] Figure 3 This is the infrared spectrum of A3, where 2262cm -1 The peak at 1716 cm is isocyanate. -1 The peak at is allophanate.
[0112] Preparation of curing agent components
[0113] Table 6 Curing agent component formula
[0114] Serial number Ingredients H1 H2 H3 H4 HC1 1 A1 (NCO 14.9%) 70 50 2 A2 (NCO 9.1%) 40 3 A3 (NCO 15.1%) 70 4 HT-100(NCO 23%) 30 60 30 50 100 Viscosity@25℃ / mPa.s 2162 2096 2282 2415 3391 Viscosity@50℃ / mPa.s 465 449 531 536 735
[0115] Preparation of Example 4H1
[0116] According to the formula in Table 6, weigh A1 and HT-100 respectively and mix them evenly to obtain curing agent component H1. The average NCO% is measured to be 17.3%, and the viscosity at 25℃ and 50℃ is 2162mPa.s and 465mPa.s respectively.
[0117] Example 5 Preparation of H2
[0118] According to the formula in Table 6, A2 and HT-100 were weighed and mixed evenly to obtain curing agent component H2. The average NCO% was measured to be 17.4, and the viscosities at 25°C and 50°C were 2096mPa.s and 449mPa.s respectively.
[0119] Preparation of Example 6H3
[0120] According to the formula in Table 6, A3 and HT-100 were weighed and mixed evenly to obtain the curing agent component H3. The average NCO% was measured to be 17.5, and the viscosities at 25°C and 50°C were 2282 mPa.s and 531 mPa.s respectively.
[0121] Preparation of Example 7H4
[0122] According to the formula in Table 6, A1 and HT100 were weighed and mixed evenly to obtain curing agent component H4. The average NCO% was measured to be 19, and the viscosities at 25°C and 50°C were 2415mPa.s and 536mPa.s respectively.
[0123] Comparative Example 1 Preparation of HC1
[0124] According to the formula in Table 6, HT-100 is the curing agent component control example HC1. The measured NCO% is 23, and the viscosity at 25°C and 50°C is 3391mPa.s and 735mPa.s respectively. They all exceed the requirements of Table 1.
[0125] Preparation of amino resin component
[0126] Table 7 Amino resin component formula
[0127]
[0128] Example 8 Preparation of R1
[0129] According to the R1 formula in Table 7:
[0130] 1. First, use a high-speed disperser to fully stir the liquid raw materials numbered 1-3;
[0131] 2. Slowly add the raw materials No. 4-5 in sequence while stirring, and then increase the speed to 2000rpm for high-speed dispersion for 30 minutes; 3. Add the raw materials No. 6-10 in sequence while stirring and stir thoroughly;
[0132] 4 Finally, add raw material No. 11 and stir thoroughly to obtain R1.
[0133] 5 The viscosities at 25°C and 50°C were measured to be 384 mPa.s and 91 mPa.s respectively.
[0134] Example 9 Preparation of R2
[0135] According to the R2 formula in Table 7:
[0136] 1. First, use a high-speed disperser to fully stir the liquid raw materials numbered 1-3;
[0137] 2. Slowly add the raw materials No. 4-5 in sequence while stirring, and then increase the speed to 2000rpm for high-speed dispersion for 30 minutes; 3. Add the raw materials No. 6-10 in sequence while stirring and stir thoroughly;
[0138] 4 Finally, add raw material No. 11 and stir thoroughly to obtain R2.
[0139] 5 The viscosity at 25°C and 50°C was measured to be 350 mPa.s and 83 mPa.s respectively.
[0140] Example 10 Preparation of R3
[0141] According to the R3 formula in Table 7:
[0142] 1. First, use a high-speed disperser to fully stir the liquid raw materials numbered 1-3;
[0143] 2. Slowly add the raw materials No. 4-5 in sequence while stirring, and then increase the speed to 2000rpm for high-speed dispersion for 30 minutes; 3. Add the raw materials No. 6-10 in sequence while stirring and stir thoroughly;
[0144] 4 Finally, add raw material No. 11 and stir thoroughly to obtain R3.
[0145] 5 The viscosities at 25°C and 50°C were measured to be 451 mPa.s and 98 mPa.s respectively.
[0146] Comparative Example 2 Preparation of RC 1
[0147] According to the RC1 formula in Table 7:
[0148] 1. First, use a high-speed disperser to fully stir the liquid raw materials numbered 1-3;
[0149] 2. Slowly add the raw materials No. 4-5 in sequence while stirring, and then increase the speed to 2000rpm for high-speed dispersion for 30 minutes; 3. Add the raw materials No. 6-10 in sequence while stirring, and stir well to obtain RC1.
[0150] The viscosity of 4 at 25°C and 50°C was 1552 mPa.s and 294 mPa.s respectively, which both exceeded the requirements of Table 1.
[0151] Comparative Example 3 Preparation of RC2
[0152] According to the RC2 formula in Table 7:
[0153] 1. First, use a high-speed disperser to fully stir the liquid raw materials numbered 1-3;
[0154] 2. Slowly add the raw materials No. 4-5 in sequence while stirring, and then increase the speed to 2000rpm for high-speed dispersion for 30 minutes; 3. Add the raw materials No. 6-10 in sequence while stirring, and stir well to obtain RC2.
[0155] 4 The measured viscosities at 25°C and 50°C were 1684mPa.s and 290mPa.s respectively. They all exceeded the requirements of Table 1. Comparison of process performance of two-component solvent-free aliphatic polyurea coatings with different formulations
[0156] The curing agent components H1, H2, H3, H4 and HC1 prepared in Examples 4-7 and Comparative Example 1 and the amino resin components R1, R2, R3 and RC1, RC2 prepared in Examples 8-10 and Comparative Examples 2-3 were combined into a two-component coating system according to the order and proportion (weight) in Table 8, so as to obtain two-component solvent-free aliphatic polyurea coatings F1, F2, F3, F4, F5, F6, FC1, FC2 and FC3 of different formulations, among which FC1, FC2 and FC3 are comparative examples. The viscosities of the resin components and curing agent components of different formulations at 25°C and 50°C are also listed in Table 8, and the pot life, surface dry time and actual dry time of the two-components of different formulations after mixing are also listed in Table 8.
[0157] Table 8 List of proportions (weight) and process properties of two-component solvent-free aliphatic polyurea coatings with different formulations
[0158]
[0159]
[0160] Notes:
[0161] Operating time: The time required for the viscosity of the two components to increase to twice the initial viscosity after mixing. The operating time of the two-component low-pressure sprayer is required to be 30-60 minutes.
[0162] Surface drying time: the time it takes for the coating to initially solidify into a film, marked by the surface becoming non-sticky and able to withstand a certain amount of material pressure.
[0163] The surface drying time requirement for two-component solvent-free polyurea coating for container painting is ≤40min.
[0164] Drying time: The shortest time for the coating to form a solid coating film, which is marked by the surface being able to withstand finger pressure. The dry time requirement for two-component solvent-free polyurea coatings for container coatings is ≤90min.
[0165] As shown in Table 8, the viscosity of the resin components of Examples F1-F6 at 25°C and 50°C is within the range of 400±50mPa.s and ≤100mPa.s, while the viscosity of their curing agent components under corresponding conditions is within the range of 2000±500mPa.s and ≤550mmPa.s, which can meet the requirements of the viscosity range of the two-component low-pressure sprayer in Table 1; at the same time, the operable time (Pot Life) and drying time of F1-F6 also meet the corresponding requirements of Table 1 and container coating. Therefore, the two-component solvent-free polyurea coatings of the F1-F6 system can meet the process requirements of the low-pressure sprayer for container coating.
[0166] As can be seen from Table 8, since the resin components of the control examples FC1 and FC2 do not contain active diluents with aldimine properties, their viscosities at 25°C and 50°C exceed the requirements in Table 1, the mixing and atomization effects are not good, and the operable time is less than 30 minutes, so they cannot meet the requirements of mechanical spraying.
[0167] As shown in Table 8, the curing agent component of the control example FC3 is only pure HDI trimer, lacking the polyisocyanate component containing allophanate, which affects the mixing effect of the two components. At the same time, the viscosity of the pure HDI trimer itself exceeds the requirements in Table 1, and the mixing and atomization effects are affected, and the surface of the formed coating is wrinkled and has orange stripes. In addition, the operable time of the system is less than 30 minutes, so it cannot meet the requirements of container coating.
[0168] Two-component solvent-free polyurea coating is sprayed on the container using a low-pressure sprayer
[0169] According to the analysis and comparison results of the contents in Table 8, two-component solvent-free polyurea coatings with formulations of F1, F3 and F5 were selected, and the containers (standard containers) were sprayed with the whole container using a low-pressure sprayer. The parameters of the main spraying processes and the coating film measurement data are summarized in Table 9.
[0170] Table 9 Main process parameters of two-component low-pressure sprayer in container coating construction
[0171]
[0172]
[0173] From the data in Table 9, it can be seen that after the two-component low-pressure spraying machine was used to spray F1, F3, and F5, the coatings on the inside and outside of the standard container all had excellent appearance effects, and the coating thickness met the container design requirements. Moreover, the coating can be quickly cured at the construction environment temperature, reaching a surface drying time of 40 minutes and a practical drying time of less than 90 minutes. At the same time, the two-component low-pressure sprayer continuously sprayed for more than 10 hours (during which F1, F3, and F2 were switched without stopping due to test needs), and the feed pipe and static mixing pipe of the sprayer did not gel or clog, indicating that the material had sufficient operating time (Pot Life) and fluidity.
[0174] The above examples and data illustrate that the two-component solvent-free aliphatic polyurea coating provided by the patent of the present invention has the characteristics of low viscosity and slow gelation, so it can achieve solvent-free thin film spraying, and can be used for anti-corrosion and protective coatings in containers and other industrial coating fields.
Claims
1. A low viscosity, slow gelling solvent-free two-component aliphatic polyurea coating, comprising an amino resin component and an isocyanate curing agent component, characterized in that: (1) The amino resin component contains a. at least one polyaspartic acid ester resin and its content is 60-90% by weight of the resin component; b. at least one reactive diluent characterized by aldimine and containing 10-40% by weight of the resin component; (2) The isocyanate curing agent component contains c. Allophanate-containing polyisocyanate, the content of which is 30-95% by weight of the curing agent component; d. Other polyisocyanates, and their content is 70-95% by weight of the curing agent component.
2. A low viscosity, slow gelling solvent-free two-component aliphatic polyurea coating according to claim 1, characterized in that: The polyaspartic acid ester resin described in a has a structure as shown in Formula 1: Wherein R1, R2, R3, and R4 are C1-C4 alkyl groups, and R1, R2, R3 and R4 may be the same or different; X is a structure as shown in Formula 2: Or the structure shown in formula 3: Or the structure shown in formula 4: -CH2-CH2-CH2-CH2-CH2-CH2- Formula 4.
3. A low viscosity, slow gelling solvent-free two-component aliphatic polyurea coating according to claim 2, characterized in that: The polyaspartic acid ester resin described in step a is one or more combinations of adducts obtained by Michael addition reaction of aliphatic polyamine and unsaturated dialkyl maleate or dialkyl fumarate, and the combination ratio is arbitrary.
4. A low viscosity, slow gelling solvent-free two-component aliphatic polyurea coating according to claim 1, characterized in that: The active diluent characterized by aldimine described in step b refers to a difunctional aldehyde formed by nucleophilic addition of a diprimary amine and a monofunctional aldehyde, and the difunctional aldehyde is any one or more combinations, and the combination ratio can be arbitrary; The diprimary amine has a structure as shown in Formula 5: H2N——R——NH2 Formula 5 In formula 5, R represents C2-C 18 aliphatic, aromatic or alicyclic groups; aliphatic diamines include ethylenediamine, ethylene glycol diamine, propylene glycol diamine and alicyclic diamines; alicyclic diamines include p-(m-)cyclohexanediamine, p-(m-)cyclohexanedimethylamine, isophoronediamine, 2,4-diaminomethylcyclohexane, 4,4-diaminodicyclohexylmethane or 3,3-dimethyl-4,4-diaminodicyclohexylmethane; wherein the monofunctional aldehyde includes acetaldehyde, propionaldehyde, butyraldehyde, isobutyraldehyde or benzaldehyde.
5. A low viscosity, slow gelling solvent-free two-component aliphatic polyurea coating according to claim 1, characterized in that: The polyisocyanate containing allophanate in step c has a structure as shown in Formula 6: Wherein R2 is the residue of monohydroxy alcohol, R represents an aliphatic alkane group containing C6-C10, and n is 1-4.
6. A low viscosity, slow gelling solvent-free two-component aliphatic polyurea coating according to claim 5, characterized in that: The allophanate-containing polyisocyanate is a product generated by the reaction of a monohydroxy alcohol and a polyisocyanate: The monohydroxy compound refers to a monohydroxy compound with a molecular weight of 30-500, which is a monohydroxy alcohol monomer, a monohydroxy polyoxypropylene ether, a polyoxyethylene ether or a monohydroxy polyester; the monohydroxy compound can be used alone or mixed in any proportion; The polyisocyanate includes hexamethylene diisocyanate HDI, isophorone diisocyanate IPDI, dicyclohexylmethane diisocyanate HMDI, 1,4-cyclohexane diisocyanate CHDI and cyclohexane dimethylene diisocyanate HXDI; one or more combinations of the above isocyanates can be used in any combination ratio.
7. A low viscosity, slow gelling solvent-free two-component aliphatic polyurea coating according to claim 1, characterized in that: The other polyisocyanates described in step d refer to aliphatic polyisocyanates or modified products thereof, including HDI trimer, HDI biuret, IPDI trimer or adducts thereof, which can be used alone or in any proportion.
8. A low-viscosity, slow-gelling, solvent-free two-component aliphatic polyurea coating according to any one of claims 1 to 7, characterized in that: Fillers, coupling agents, dispersants, thixotropic agents, pigments, leveling agents, defoamers, ultraviolet light absorbers or antioxidants may be added to the amino resin component as required.
9. The method for preparing a low-viscosity, slow-gelling solvent-free two-component aliphatic polyurea coating according to claim 8, characterized in that: (1) The preparation method of the amino resin component is carried out in the following order: a. First, weigh polyaspartic acid ester or its mixture and mix and stir evenly in a container; b. Add the measured coupling agent, dispersant, leveling agent, defoamer, UV absorber and antioxidant, and stir well; c. Add the measured filler, thixotropic agent and color paste and stir well, then disperse at a stirring speed for 30 minutes; d. Add a measured amount of reactive diluent having aldimine characteristics, stir evenly to obtain an amino resin component; calculate according to the total amino equivalent of the secondary amino group of the polyaspartic acid resin and the primary amino group of the aldimine in the amino resin component and the isocyanate equivalent in the curing agent component, and make NCO / (NH+NH2)=1.1-1.3:1; (2) The preparation method of the polyisocyanate curing agent component is carried out in the following order: e. First, weigh the allophanate-containing polyisocyanate into a container; f. Add other polyisocyanates in measured amounts and stir evenly to obtain the curing agent component; (3) Synthetic coatings: The amino resin component and the curing agent component are mixed in a weight ratio of 1:1-1:0.
1.
10. Use of the low-viscosity, slow-gelling solvent-free two-component aliphatic polyurea coating according to claims 1-9 on containers.
Citation Information
Patent Citations
Solvent-free polyaspartate polyurea coating and preparation method thereof
CN115820099A
Aldehyde (ketone) imine-containing polyether type aspartic acid ester and application thereof in wind power blade coating
CN117887063A
Binder composition comprising polyaspartic ester and sulfonated polyiscocyanate
CN1880393A
Polyisocyanate / polyamine mixtures and their use for the production of polyurea coatings
US5516873A
Cited By