Near-alpha type medium-high strength titanium alloy with low yield ratio and preparation method thereof
By adding Sn elements to the near-α medium-high strength titanium alloy and adopting segmented heating and cross-rolling technology, combined with heat treatment, the problem of difficulty in controlling the yield ratio in the prior art is solved, and the tensile strength of the material is improved and the destructive ability after yielding and deformation reduces production costs and improves application competitiveness.
Patent Information
- Application Number
- CN202411151771.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-05
AI Technical Summary
The existing technology is difficult to effectively control the low yield-strength ratio of near-α medium and high strength corrosion-resistant titanium alloys, resulting in insufficient resistance to damage after yield deformation at high temperatures, and the forging process is a discontinuous process, resulting in long material processing flow, deformation amount and Difficult to control temperature increases production costs.
By optimizing the alloy composition, adding Sn elements to improve heat resistance, and using segmented heating and cross-rolling technology, combined with heat treatment, the low yield strength ratio stability control of near-α medium and high strength titanium alloys is achieved, reducing yield strength To improve tensile strength.
The damage capability of the near-α medium and high-strength titanium alloy after yield deformation is achieved, the yield-strength ratio is reduced, the application competitiveness and production efficiency of materials are improved, and the production cost is reduced.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of materials and metallurgy, and more specifically to a near-alpha type medium-high strength titanium alloy with a low yield ratio and a preparation method thereof. Background Art
[0002] Near-α medium-high strength corrosion-resistant titanium alloy is a type of titanium alloy whose main microstructure is single-phase α type, generally containing α-stabilizing elements such as Al and neutral elements such as Zr as alloying elements. This type of alloy has high high-temperature mechanical properties and thermal stability, good fatigue resistance, and can be mainly used in aircraft engines, ship piping systems, and nuclear reactor steam generators.
[0003] Yield strength ratio is one of the main reference indicators for formulating metal plastic processing technology, and is also an important evaluation indicator for the application of metal materials. The yield strength ratio of near-α-type medium-high strength corrosion-resistant titanium alloy is generally between 0.75 and 0.9. Since the performance of near-α-type medium-high strength corrosion-resistant titanium alloy is sensitive to the change of yield strength ratio, a higher yield strength ratio will reduce the ability of the alloy to resist damage after yield deformation. The prior art with publication number CN116987991A discloses a method for regulating Ti 2 The yield strength ratio method of AlNb-based alloy is based on the forging process by using Ti, which is an intermetallic compound material. 2 AlNb-based alloys are subjected to solid solution aging process parameter changes to achieve the purpose of regulating the yield strength ratio. However, the forging products involved are for small parts and high-strength components, and are not suitable for the manufacture of products such as plates and pipes. At the same time, since the forging process of the prior art is a discontinuous processing process, multiple firings are required to reheat the blanks, resulting in a long material processing process, and it is difficult to control the deformation and temperature during the processing. Multiple heating will also cause serious oxidation of the blank surface, increase material burnout, and increase production costs.
[0004] Therefore, the research and development of near-α-type medium- and high-strength corrosion-resistant titanium alloys with both high strength and low yield ratio is crucial to further enhance the service performance of titanium alloy materials. Summary of the invention
[0005] The purpose of the present invention is to overcome the above-mentioned defects of the prior art, and to provide a near-α-type medium-high strength titanium alloy with a low yield ratio and a preparation method thereof, which can efficiently realize the stable control of the low yield ratio of the near-α-type single-α-phase medium-high strength corrosion-resistant titanium alloy, and can effectively improve the ability of the alloy to resist damage after yield deformation, so that the application of this product in the fields of aviation engines, ship piping systems and nuclear reactor steam generators has greater competitive advantages, and has considerable application prospects and a broad application market.
[0006] To achieve the above object, the technical solution of the present invention is as follows:
[0007] A near-α-type medium-high strength titanium alloy with a low yield ratio, comprising the following components in percentage by mass: Al: 1.5%-3%, Zr: 2.50%-2.60%, Fe: 0.05%-0.25%, C: 0.01%-0.015%, N≤0.04%, H≤0.006%, O≤0.15%, Sn≤0.05%, and the rest being Ti and impurities.
[0008] Optionally, the yield strength of the near-α-type medium-high strength titanium alloy is 430MPa-680MPa, the tensile strength is 612MPa-919MPa, and the yield strength ratio is 0.70-0.74.
[0009] The present invention also discloses a method for preparing the above-mentioned near-α-type medium-high strength titanium alloy with low yield ratio, which is characterized by comprising the following steps:
[0010] After being melted into ingots twice in a vacuum non-consumable arc furnace, and then successively subjected to a heating process, a rolling process and a heat treatment process, the near-α-type medium-high strength titanium alloy with a low yield ratio is obtained;
[0011] In the heating process, the ingot is heated by a segmented heating method; the heating process includes an air preheating section, a billet preheating section, a heating section and a soaking section.
[0012] Optionally, the heating rate of the air preheating section is 50°C / min to 80°C / min, the temperature is 400°C to 600°C, and the insulation time is 20min to 30min.
[0013] Optionally, the heating rate of the blank in the preheating stage is 50°C / min to 80°C / min, the temperature is 800°C to 850°C, and the holding time is 10min to 15min.
[0014] Optionally, the heating rate of the heating section is 80°C / min to 120°C / min, the temperature is 950°C to 980°C, and the insulation time is 10min to 15min.
[0015] Optionally, the temperature of the soaking section is 980°C to 1000°C, and the insulation time is 60min to 100min.
[0016] Optionally, in the rolling process, the heated ingot is subjected to rough rolling and finish rolling in sequence; in the rough rolling, the temperature range of rolling deformation is 940°C to 960°C, 1-3 rolling passes are performed, the single-pass reduction range is 25% to 30%, and the total deformation is controlled not to exceed 60%; the temperature is reversed and when the temperature drops to a preset temperature, longitudinal finish rolling is performed, at which time the temperature range is controlled at 800°C to 850°C, multiple rolling passes are performed, the single-pass reduction range is 15% to 25%, and the total deformation is controlled not to be less than 40%.
[0017] Optionally, the two times of smelting in a vacuum non-consumable arc furnace are used to form ingots, and the main raw materials used for smelting are sponge titanium, sponge zirconium, aluminum beans, titanium dioxide, ferrotitanium alloy and high-purity tin particles. The raw materials are fully and evenly mixed and pressed into electrodes. After the electrode is pressed, it is welded in a vacuum welding box. The vacuum degree of the welding box is <5Pa, and the vacuum leakage rate is <1Pa / min. The first smelting is carried out within 1.5 hours after the electrode welding is completed. After the electrode rod is transferred to the smelting furnace, it is welded with the auxiliary electrode. The welding process requires an initial vacuum degree of <3Pa and a leakage rate of ≤1Pa / min. After the auxiliary electrode is welded and checked, the furnace is reloaded, vacuumed, and vacuum consumable smelting is carried out. The smelting requires an initial vacuum degree of ≤1Pa and a leakage rate of ≤1Pa / min during the smelting process.
[0018] Optionally, in the heat treatment process, the heat treatment temperature is 600°C to 750°C, and the temperature is kept for 0.5h to 2h. After the heat treatment, the furnace is cooled to 450°C to 500°C and then air-cooled to room temperature.
[0019] Implementing the embodiments of the present invention will have the following beneficial effects:
[0020] 1. The present invention optimizes the existing near-α-type medium-high strength corrosion-resistant titanium alloy component system and designs a reasonable addition of the eutectoid element Sn of Ti in the alloy component system, which can improve the heat resistance of the alloy on the basis of solid solution strengthening, and at the same time increase the tensile strength by 3% to 5%, thereby achieving the purpose of reducing the yield ratio to a certain extent.
[0021] 2. The present invention proposes a four-stage heating temperature method and clearly gives the key parameters of each heating stage, which effectively solves the problems of low thermal conductivity of titanium alloy and easy hydrogen absorption and oxidation burning during high-temperature heating. It matches the reasonable rolling parameter setting of cross-rolling and obtains a rolled billet with good uniformity of the entire cross-section structure.
[0022] 3. The heat treatment method proposed in the present invention clearly provides the heat treatment window and key heat treatment parameters for this type of alloy. The billet with good uniformity of the entire cross-section structure undergoes recrystallization. The recovery and recrystallization of the structure continuously reduce the dislocation structure generated by rolling, that is, the softening of the structure further reduces the yield strength ratio of the billet.
[0023] 4. The two-stage cooling method proposed in the present invention specifies that the furnace discharge temperature is 450°C to 500°C, which effectively avoids the operational risks caused by high-temperature furnace discharge and the risk of uneven structure caused by rapid cooling of the finished product surface. In addition, the furnace temperature corresponding to the furnace discharge is within the temperature range of the air preheating section in the four-stage heating system, which better enables the furnace temperature control parameters in the present invention to achieve a closed loop, facilitates the continuous production of products, and can better improve the production rate. By furnace cooling to below the recrystallization start temperature and then air cooling to room temperature, the billet structure with good uniformity of the entire cross-section and refined grains can be better solidified, which helps to finally obtain a low yield ratio near-α-type medium-high strength corrosion-resistant titanium alloy finished product. DETAILED DESCRIPTION
[0024] The present invention is further described below in conjunction with specific embodiments, but the present invention is not limited in any way.
[0025] 1. Chemical composition and mechanical properties
[0026] The invention discloses a near-α-type medium-high strength titanium alloy with a low yield ratio. The near-α-type medium-high strength titanium alloy comprises the following components in mass percentage: Al: 1.5%-3%, Zr: 2.50%-2.60%, Fe: 0.05%-0.25%, C: 0.01%-0.015%, N≤0.04%, H≤0.006%, O≤0.15%, Sn≤0.05%, and the rest are Ti and impurities.
[0027] In a specific embodiment, the yield strength of the near-α-type medium-high strength titanium alloy is 430 MPa to 680 MPa, the tensile strength is 612 MPa to 919 MPa, and the yield strength ratio is 0.70 to 0.74.
[0028] 2. Production technology
[0029] The present invention discloses a method for preparing a near-α-type medium-high strength titanium alloy with a low yield ratio as described in any embodiment of the present invention, comprising the following steps: smelting into ingots twice in a vacuum non-consumable arc furnace, and then sequentially undergoing a heating process, a rolling process and a heat treatment process to obtain a near-α-type medium-high strength titanium alloy with a low yield ratio.
[0030] Specifically:
[0031] S1. Melt into ingots in two vacuum non-consumable arc furnaces. The main raw materials used for smelting are sponge titanium, sponge zirconium, aluminum beans, titanium dioxide, ferrotitanium alloy and high-purity tin particles. The raw materials are fully and evenly mixed and pressed into electrodes. After the electrode is pressed, it is welded in a vacuum welding box. The vacuum degree of the welding box is <5Pa, and the vacuum leakage rate is <1Pa / min. The first smelting is carried out within 1.5 hours after the electrode welding is completed. After the electrode rod is transferred to the smelting furnace, it is welded with the auxiliary electrode. The welding process requires an initial vacuum degree of <3Pa and a leakage rate of ≤1Pa / min. After the auxiliary electrode is welded and checked, the furnace is reinstalled, vacuumed, and vacuum consumable smelting is carried out. The smelting requires an initial vacuum degree of ≤1Pa, and a leakage rate of ≤1Pa / min during the smelting process.
[0032] S2. In the heating process, the ingot is heated by a segmented heating method. Specifically, since the thermal conductivity of titanium alloy is low and it is more prone to hydrogen absorption reaction at high temperature, hydrogen embrittlement may occur in severe cases. Therefore, a segmented heating method is preferably adopted. In the present invention, the heating process includes a four-stage heating method of air preheating section, billet preheating section, heating section and soaking section for heating. In order to alleviate the occurrence of hydrogen absorption during the heating process, the atmosphere in the furnace is controlled to be slightly oxidizing.
[0033] In a specific embodiment, in the air preheating section, in order to reduce the heating time of the billet in the furnace and reduce the amount of oxide scale generated on the surface of the billet, the heating rate of the air preheating section is 50℃ / min~80℃ / min, the temperature is 400℃~600℃, and in order to prevent the heating furnace from burning empty and causing the oxidation rate to increase and the energy consumption of the heating furnace to increase, the holding time is 20min~30min.
[0034] In a specific embodiment, during the billet preheating stage, in order to allow the furnace bottom to quickly reach the furnace temperature requirement, the heating rate during the billet preheating stage is 50°C / min-80°C / min, the temperature is 800°C-850°C, and the insulation time is 10min-15min.
[0035] In a specific embodiment, in the heating section, in view of the low thermal conductivity of titanium alloy, in order to reduce burning, the heating rate of the heating section is 80°C / min to 120°C / min, the temperature is 950°C to 980°C, and the holding time is 10min to 15min.
[0036] In a specific embodiment, in the soaking section, in order to stabilize the quality of the soaking heating of the billet and prevent the billet from being overburned, the temperature of the soaking section is 980° C. to 1000° C., and the holding time is 60 min to 100 min.
[0037] S3. In the rolling process, the heated ingot is subjected to rough rolling and finish rolling in sequence. Specifically, after the ingot reaches the temperature, it is taken out of the furnace, the roller cooling water and dephosphorization water at the furnace end are turned off, and a reversible rolling mill is used for large reduction and widening rough rolling. In the rough rolling, the temperature range of rolling deformation is 940℃~960℃, and 1-3 rollings are carried out. The reduction range of a single pass is 25%~30%, and the total deformation is controlled not to exceed 60%; the temperature is reversed and when the temperature drops to the preset temperature, longitudinal finish rolling is carried out. At this time, the temperature range is controlled at 800℃~850℃, and multiple rollings are carried out. The reduction range of a single pass is 15%~25%, and the total deformation is controlled not to be less than 40%.
[0038] S4. In the heat treatment process, the heat treatment temperature is 600℃~750℃, and the temperature is kept for 0.5h~2h. In order to ensure the uniformity of the blank structure after annealing, the furnace is cooled to 450℃~500℃ after the heat treatment, and then air-cooled to room temperature. Specifically, if the heat treatment temperature is lower than the set range of the present invention, the blank will have insufficient grain refinement due to insufficient recrystallization, thereby reducing the mechanical properties of the material. If the heat treatment temperature is higher than the range of the present invention, a certain number of twins begin to appear in the blank structure, and the structure is strengthened to increase the yield strength ratio.
[0039] The following are specific embodiments
[0040] Examples 1-3 are examples of preparing near-α-type medium-high strength corrosion-resistant titanium alloy products using the preparation method of the present invention. After the finished product is prepared, an electronic universal testing machine is used to test its room temperature tensile properties. Among them, the tensile test is carried out in accordance with GB / T228.1-2017 "Metallic Material Tensile Test Part 1 Room Temperature Test Method" mechanical sample preparation and testing.
[0041] Example 1
[0042] The chemical composition of the blank in this embodiment is as follows by weight percentage: Al: 2%, Zr: 2.50%, Fe: 0.05%, C: 0.01%, N: 0.004%, H: 0.005%, O: 0.12%, Sn: 0.05%, and the rest are Ti and impurities.
[0043] In this embodiment, an ingot is obtained by smelting twice in a vacuum consumable arc furnace, and then a finished product is obtained by ingot heating-rough rolling-finishing rolling-heat treatment. The hot rolling is heated by a four-stage heating method of air preheating section, billet preheating section, heating section and soaking section, and the atmosphere in the furnace is controlled to be slightly oxidizing. Among them, in the air preheating section, the heating rate is 50℃ / minute, the temperature control should be maintained at 450℃, and the insulation time is 20 minutes. In the preheating stage, a heating rate of 50℃ / minute is used, and the temperature is controlled to be maintained at 820℃, and the insulation time is 10 minutes. In the heating stage, a heating rate of 80℃ / minute is used, and the temperature is controlled to be maintained at 950℃, and the insulation time is 10 minutes. In the soaking stage, the temperature is controlled to be maintained at 980℃, and the insulation time is 60 minutes. After reaching the temperature, the billet is discharged from the furnace, the roller cooling water and dephosphorization water at the furnace end are turned off, and a reversible rolling mill is used for large reduction and widening rough rolling. The temperature range of rolling deformation is 950℃, and three rollings are performed. The range of single-pass reduction is 25-28%, and the total deformation is controlled not to exceed 55%. After reversing and waiting for temperature, when the temperature drops to the preset temperature, longitudinal finishing rolling is performed. At this time, the temperature range is controlled at 800℃, and multiple rollings are performed. The range of single-pass reduction is 15% to 20%, and the total deformation is controlled to be 47%. The rolled billet is heat treated, and the heat treatment temperature is controlled at 600℃, and the temperature is kept for 2 hours. The cooling method is furnace cooling to 500℃ and air cooling to room temperature.
[0044] The mechanical properties of the product were tested and the results were: yield strength was 542MPa, tensile strength was 763MPa, and yield strength ratio was 0.71.
[0045] Example 2
[0046] The chemical composition of the billet is as follows by weight percentage: Al: 1.76%, Zr: 2.55%, Fe: 0.1%, C: 0.01%, N: 0.004%, H: 0.005%, O: 0.05%, Sn: 0.05%, and the rest are Ti and impurities. The ingot is obtained by smelting twice in a vacuum consumable arc furnace, and then the finished product is obtained by ingot heating-rough rolling-finishing rolling-heat treatment. The hot rolling adopts a four-stage heating method of air preheating section, billet preheating section, heating section and soaking section to control the atmosphere in the furnace to be slightly oxidizing. In the air preheating section, the heating rate is 60℃ / min, the temperature control should be maintained at 500℃, and the holding time is 20 minutes. In the preheating stage, the heating rate is 60℃ / min, the temperature control is maintained at 820℃, and the temperature is kept for 10 minutes. In the heating stage, the heating rate is 100℃ / min, the temperature control is maintained at 960℃, and the temperature is kept for 10 minutes. During the soaking stage, the temperature is controlled to be maintained at 1000℃ for 60 minutes. After reaching the temperature, the billet is taken out of the furnace, the roller cooling water and dephosphorization water at the furnace end are turned off, and a reversible rolling mill is used for large reduction and widening rough rolling. The temperature range of rolling deformation is 950℃, and two rollings are carried out. The range of single-pass reduction is 25% to 28%, and the total deformation is controlled not to exceed 55%. Reverse and wait for temperature. When the temperature drops to the preset temperature, longitudinal finishing rolling is carried out. At this time, the temperature range is controlled at 800℃, and multiple rollings are carried out. The range of single-pass reduction is 15% to 20%, and the total deformation is controlled to be 59%. The rolled billet is heat treated, and the heat treatment temperature is controlled at 700℃. It is kept warm for 1.5 hours. The cooling method is furnace cooling to 500℃ and air cooling to room temperature.
[0047] The mechanical properties of the product were tested and the results were: yield strength was 462MPa, tensile strength was 648MPa, and yield strength ratio was 0.71.
[0048] Example 3
[0049] The chemical composition of the billet is as follows by weight percentage: Al: 2.9%, Zr: 2.5%, Fe: 0.1%, C: 0.01%, N: 0.004%, H: 0.005%, O: 0.05%, Sn: 0.05%, and the rest are Ti and impurities. The ingot is obtained by smelting twice in a vacuum consumable arc furnace, and then the finished product is obtained by ingot heating-rough rolling-finishing rolling-heat treatment. The hot rolling adopts a four-stage heating method of air preheating section, billet preheating section, heating section and soaking section to control the atmosphere in the furnace to be slightly oxidizing. In the air preheating section, the heating rate is 60℃ / min, the temperature control should be maintained at 500℃, and the holding time is 20 minutes. In the preheating stage, the heating rate is 60℃ / min, the temperature control is maintained at 850℃, and the temperature is kept for 10 minutes. In the heating stage, the heating rate is 100℃ / min, the temperature control is maintained at 980℃, and the temperature is kept for 10 minutes. During the soaking stage, the temperature is controlled to be maintained at 1000℃ for 60 minutes. After reaching the temperature, the billet is taken out of the furnace, the roller cooling water and dephosphorization water at the furnace end are turned off, and a reversible rolling mill is used for large reduction and widening rough rolling. The temperature range of rolling deformation is 950℃, and two rollings are carried out. The range of single-pass reduction is 25% to 28%, and the total deformation is controlled not to exceed 55%. Reverse waiting for temperature, when the temperature drops to the preset temperature, longitudinal finishing rolling is carried out. At this time, the temperature range is controlled at 800℃, and multiple rollings are carried out. The range of single-pass reduction is 15% to 20%, and the total deformation is controlled to be 59%. The rolled billet is heat treated, and the heat treatment temperature is controlled at 750℃, and it is kept warm for 1 hour. The cooling method is furnace cooling to 500℃ and air cooling to room temperature.
[0050] The mechanical properties of the product were tested and the results were: yield strength was 430MPa, tensile strength was 612MPa, and yield strength ratio was 0.70.
[0051] Comparative Example 1 (Compared with Example 3)
[0052] The only difference between this comparative example and Example 3 is that Sn is not added. The details are as follows:
[0053] The chemical composition of the billet is as follows by weight percentage: Al: 2.9%, Zr: 2.5%, Fe: 0.1%, C: 0.01%, N: 0.004%, H: 0.005%, O: 0.05%, and the rest are Ti and impurities. The ingot is obtained by melting twice in a vacuum consumable arc furnace, and then the finished product is obtained by ingot heating-rough rolling-finishing rolling-heat treatment. The hot rolling adopts a four-stage heating method of air preheating section, billet preheating section, heating section and soaking section to heat, and the atmosphere in the furnace is controlled to be slightly oxidizing. In the air preheating section, the heating rate is 60℃ / min, the temperature control should be maintained at 500℃, and the holding time is 20 minutes. In the preheating stage, the heating rate is 60℃ / min, the temperature control is maintained at 850℃, and the temperature is kept for 10 minutes. In the heating stage, the heating rate is 100℃ / min, the temperature control is maintained at 980℃, and the temperature is kept for 10 minutes. In the soaking stage, the temperature control is maintained at 1000℃ and the temperature is kept for 60 minutes. After reaching the temperature, the billet is taken out of the furnace, the roller cooling water and dephosphorization water at the furnace end are turned off, and a reversible rolling mill is used for large reduction and widening rough rolling. The temperature range of rolling deformation is 950℃, and two rollings are carried out. The range of single-pass reduction is 25% to 28%, and the total deformation is controlled not to exceed 55%. Reverse and wait for temperature. When the temperature drops to the preset temperature, longitudinal finishing rolling is carried out. At this time, the temperature range is controlled at 800℃, and multiple rollings are carried out. The range of single-pass reduction is 15% to 20%, and the total deformation is controlled to be 59%. The billet after rolling is heat treated, and the heat treatment temperature is controlled at 750℃. It is kept warm for 1 hour, and the cooling method is furnace cooling to 500℃ and air cooling to room temperature.
[0054] The mechanical properties of the product were tested and the results were: yield strength was 423MPa, tensile strength was 581MPa, and yield strength ratio was 0.73.
[0055] The low yield ratio near-α medium-high strength titanium alloy of the present invention can stably reduce the yield ratio of the near-α medium-high strength titanium alloy, effectively improve the ability of the near-α medium-high strength titanium alloy to resist damage after yield deformation, increase the service life of such alloy products in special environments, and can replace the high yield ratio near-α medium-high strength titanium alloy prepared by the existing traditional method, and obtain a finished product with good uniformity of organization. After realizing mass application, it will have significant economic benefits.
[0056] According to the above results, it can be known that in the low yield ratio near-α medium-high strength titanium alloy composition of the present invention, the eutectoid element Sn of Ti is reasonably added to the alloy composition system, which can improve the heat resistance of the alloy on the basis of solid solution strengthening, and at the same time increase the tensile strength by 3% to 5%, thereby achieving the purpose of reducing the yield ratio to a certain extent; the ingot is obtained by two vacuum consumable arc furnace smeltings matching the alloy composition, and then the ingot heating-rough rolling-finishing rolling-heat treatment and other production processes are carried out, thereby achieving the result of reducing the yield ratio of the near-α medium-high strength corrosion-resistant titanium alloy.
[0057] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the patent application. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A near-α-type medium-high strength titanium alloy with low yield ratio, characterized in that: The near-α-type medium-high strength titanium alloy comprises the following components in percentage by mass: Al: 1.5%~3%, Zr: 2.50%~2.60%, Fe: 0.05%~0.25%, C: 0.01%~0.015%, N≤0.04%, H≤0.006%, O≤0.15%, Sn≤0.05%, and the rest are Ti and impurities.
2. The near-α-type medium-high strength titanium alloy with low yield ratio according to claim 1, characterized in that: The yield strength of the near-α-type medium-high strength titanium alloy is 430MPa-680MPa, the tensile strength is 612MPa-919MPa, and the yield strength ratio is 0.70-0.
74.
3. A method for preparing a near-α-type medium-high strength titanium alloy with a low yield ratio as claimed in any one of claims 1 to 2, characterized in that: The following steps are involved: After being melted into ingots twice in a vacuum non-consumable arc furnace, and then successively subjected to a heating process, a rolling process and a heat treatment process, the near-α-type medium-high strength titanium alloy with a low yield ratio is obtained; In the heating process, the ingot is heated by a segmented heating method; the heating process includes an air preheating section, a billet preheating section, a heating section and a soaking section.
4. The preparation method according to claim 3, characterized in that: The heating rate of the air preheating section is 50°C / min to 80°C / min, the temperature is 400°C to 600°C, and the insulation time is 20min to 30min.
5. The preparation method according to claim 3, characterized in that: The heating rate of the blank preheating stage is 50°C / min to 80°C / min, the temperature is 800°C to 850°C, and the insulation time is 10min to 15min.
6. The preparation method according to claim 3, characterized in that: The heating rate of the heating section is 80° C. / min to 120° C. / min, the temperature is 950° C. to 980° C., and the insulation time is 10 min to 15 min.
7. The preparation method according to claim 3, characterized in that: The temperature of the soaking section is 980° C. to 1000° C., and the insulation time is 60 min to 100 min.
8. The preparation method according to claim 3, characterized in that: In the rolling process, the heated ingot is subjected to rough rolling and finish rolling in sequence; in the rough rolling, the temperature range of rolling deformation is 940°C to 960°C, 1-3 rolling passes are performed, the reduction range of a single pass is 25% to 30%, and the total deformation is controlled not to exceed 60%; the temperature is reversed and when the temperature drops to a preset temperature, longitudinal finish rolling is performed, at which time the temperature range is controlled at 800°C to 850°C, multiple rolling passes are performed, the reduction range of a single pass is 15% to 25%, and the total deformation is controlled not to be less than 40%.
9. The preparation method according to claim 3, characterized in that: In the two vacuum non-consumable arc furnaces, the titanium sponge, zirconium sponge, aluminum beans, titanium dioxide, ferrotitanium alloy and high-purity tin particles are mixed and pressed into electrodes and then vacuum welded. The vacuum degree is set to <5Pa and the vacuum leakage rate is set to <1Pa / min. The first smelting is carried out within 1.5 hours after the electrode welding. After the electrode rod is transferred to the smelting furnace, it is welded with the auxiliary electrode, maintaining the initial vacuum degree <3Pa and the leakage rate ≤1Pa / min. After the auxiliary electrode welding is completed, vacuum consumable smelting is carried out, maintaining the initial vacuum degree ≤1Pa and the leakage rate ≤1Pa / min.
10. The preparation method according to claim 3, characterized in that: In the heat treatment process, the heat treatment temperature is 600° C. to 750° C., and the temperature is kept at 0.5 h to 2 h. After the heat treatment, the furnace is cooled to 450° C. to 500° C. and then air-cooled to room temperature.
Citation Information
Patent Citations
Method for regulating yield ratio of Ti2AlNb-based alloy
CN116987991A
Cited By
High-strength low-yield-ratio near-alpha type titanium alloy and preparation method thereof
CN119464833A