HUD (Head Up Display) film containing SiO2 and Ti and preparation process thereof
By using SiO2 and TiO2 layers in the HUD film, combined with magnetron coating sputtering process and specific target materials and gas combinations, the problem of poor wear resistance of the HUD film is solved, achieving better driving information projection effect and driving safety.
Patent Information
- Application Number
- CN202410983665.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-11-05
AI Technical Summary
The HUD film is prone to friction or scratches after being used on the front windshield of the car for a long time, which affects the projection effect of driving information and makes driving safety difficult to ensure.
Using a HUD film containing SiO2 and Ti, the SiO2 layer is formed through magnetron coating sputtering process, and a mixed target material including silicon and aluminum and a mixture of argon, nitrogen and oxygen is used to form a TiO2 layer and a metal layer to improve the film's Wear resistance and permeability.
显著提高了HUD膜的耐磨性和透过性,确保驾驶信息的清晰性和完整性,提高了驾驶安全性。
Smart Images

Figure CN118895480A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of HUD films, and in particular relates to a HUD film containing SiO2 and Ti and a preparation process thereof. Background Art
[0002] HUD (Head-up Display) is a technology evolved from the military field. Its characteristic is that it can display some important tactical information within the field of view of the fighter's normal observation direction without affecting the driver's attention to the environment. The driver does not have to always divert his eyes to observe the pointers and data on the dashboard.
[0003] Currently, this technology is applied to the front windshield of the car. By setting a HUD film on the front windshield, important driving information such as speed and navigation can be projected onto the windshield in front of the driver, allowing the driver to see important driving information such as speed and navigation without lowering or turning his head, so as to improve driving safety.
[0004] After the HUD film is used on the car windshield for a long time, certain friction or scratches may occur on the HUD film, which may affect the projection effect of driving information and may even cause the driver to misjudge the driving information, making it difficult to ensure driving safety.
[0005] Therefore, in view of the above technical problems, it is necessary to provide a HUD film containing SiO2 and Ti and a preparation process thereof. Summary of the invention
[0006] The object of the present invention is to provide a HUD film containing SiO2 and Ti and a preparation process thereof, which can solve the problem that the wear resistance of the HUD film is poor, resulting in poor driving information projection effect.
[0007] In order to achieve the above object, a technical solution provided by a specific embodiment of the present invention is as follows:
[0008] In one or more embodiments of the present invention, a HUD film containing SiO2 and Ti is provided, comprising a substrate layer, a primer layer, a TiO2 layer, a metal layer and a SiO2 layer stacked in sequence, wherein the SiO2 layer is formed by a magnetron coating sputtering process, wherein the target material selected in the magnetron coating sputtering process is a mixed target including silicon and aluminum, and the reaction gas bombarding the target material is a mixed gas including argon, nitrogen and oxygen.
[0009] In one or more embodiments of the present invention, the thickness of the TiO2 layer is in the range of 5-125 nm.
[0010] In one or more embodiments of the present invention, in the mixed target, silicon accounts for 82-99% and aluminum accounts for 18-1%.
[0011] In one or more embodiments of the present invention, in the mixed gas, argon accounts for 60-78%, nitrogen accounts for 18-35%, and oxygen accounts for 3-8%.
[0012] In one or more embodiments of the present invention, the thickness of the SiO2 layer is in the range of 20-220 nm.
[0013] In one or more embodiments of the present invention, the base layer is selected from one of SiO2, Ti, TiO2, Si, Al2O3, MgF2, SiO, HfO2, SnO2, and Y2O3.
[0014] In one or more embodiments of the present invention, the thickness of the primer layer is in the range of 0.2-20 nm.
[0015] In one or more embodiments of the present invention, the metal layer is a nickel-chromium layer, wherein nickel accounts for 50-90% and chromium accounts for 50-10%.
[0016] In one or more embodiments of the present invention, a preparation process for preparing the above-mentioned HUD film containing SiO2 and Ti is also provided, comprising the following steps:
[0017] A primer layer, a TiO2 layer, a metal layer and a SiO2 layer are sequentially plated on the substrate layer by a magnetron coating sputtering process;
[0018] Wherein, in the step of plating the SiO2 layer, the following steps are also included:
[0019] Providing a mixed target material including silicon and aluminum and a mixed gas including argon, nitrogen and oxygen;
[0020] evacuating the coating chamber and driving the mixed target to rotate in the coating chamber;
[0021] The target material sputtering deposition is started, and the mixed target material is bombarded by the mixed gas.
[0022] In one or more embodiments of the present invention, in the step of evacuating the coating chamber, the vacuum degree of the coating chamber is controlled to be less than 1×10 -4 pa, water vapor value is less than 9×10 -5 pa.
[0023] Compared with the prior art, the present invention forms a SiO2 layer by providing a TiO2 layer and bombarding a mixed target including silicon and aluminum with a mixed gas including argon, nitrogen and oxygen, so that the HUD film finally formed has good wear resistance and excellent transmittance, and has good reflection effects of P light and S light and good environmental detection effect. Therefore, it can be effectively applied to the front windshield of the car to provide the driver with clear and complete driving information and ensure driving safety. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0025] Figure 1 It is a schematic diagram of the structure of a low-reflection and low-transmittance flexible optical film in one embodiment of the present invention;
[0026] Figure 2 is the P light reflection contrast curve;
[0027] Figure 3 is the S light reflection contrast curve;
[0028] Figure 4 Through contrasting curves.
[0029] Description of main reference numerals:
[0030] 1. Release film; 2. Lower coating layer; 3. Base material layer; 4. Upper coating layer; 5. Primer layer; 6. TiO2 layer; 7. Metal layer; 8. SiO2 layer; 9. AF layer; 10. PET high temperature positive insulation layer. DETAILED DESCRIPTION
[0031] In order to enable those skilled in the art to better understand the technical solutions in the present invention, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
[0032] like Figure 1 As shown, the HUD film containing SiO2 and Ti in one embodiment of the present invention includes a substrate layer, a primer layer, a TiO2 layer, a metal layer and a SiO2 layer stacked in sequence.
[0033] The substrate layer can be a PET layer, a transparent PI layer, a TAC layer, a COP layer or a PC layer, and the thickness of the substrate layer ranges from 5.7 to 250 μm. The upper coating layer and the lower coating layer are respectively provided on both sides of the substrate layer by a coating process, and the upper coating layer and the lower coating layer are formed by coating an acrylic resin coating liquid, the coating thickness of the upper coating layer is 40-320 nm, and the coating thickness of the lower coating layer is 0.3-3.9 μm. After coating, a 30-188 μm high-temperature protective film is attached to the lower coating layer to ensure the appearance protection of the film surface and the stability of the coating during the magnetron sputtering coating process.
[0034] The primer layer is plated on the side of the upper coating layer away from the substrate layer, and the primer layer is selected from one of SiO2, Ti, TiO2, Si, Al2O3, MgF2, SiO, HfO2, SnO2, and Y2O3. The thickness of the primer layer ranges from 0.2 to 20 nm. A TiO2 layer is plated on the primer layer, and the thickness of the TiO2 layer ranges from 5 to 125 nm. A metal layer is plated on the TiO2 layer, and the metal layer is a nickel-chromium layer, in which nickel accounts for 50-90%, chromium accounts for 50-10%, and the thickness of the metal layer ranges from 5 to 125 nm. A SiO2 layer is plated on the metal layer, and the thickness of the SiO2 layer ranges from 20 to 220 nm. The SiO2 layer is formed by a magnetron coating sputtering process, and the target material selected in the magnetron coating sputtering process is a mixed target including silicon and aluminum, and the reaction gas bombarding the target material is a mixed gas including argon, nitrogen and oxygen. In the mixed target, silicon accounts for 82-99% and aluminum accounts for 18-1%. In the mixed gas, argon accounts for 60-78%, nitrogen accounts for 18-35%, and oxygen accounts for 3-8%.
[0035] In the magnetron coating sputtering process, the weather resistance of the final product can be increased by setting up a mixed target and a mixed gas. In the prior art, a silicon oxide layer is usually formed by bombarding a pure silicon target with argon gas, and compared with a pure silicon target, a silicon-aluminum target doped with alloy aluminum can make the target sputtering more stable, more uniform, and more efficient. Selecting a mixed gas as the reaction gas can effectively solve the problem of uniformity of the film surface during sputtering of a pure silicon target, and overall improve the optical stability and yield rate after superposition, while also improving the environmental test performance.
[0036] In an optional embodiment, an AF layer may be stacked on a side of the silicon oxide layer away from the metal layer. The AF layer is mainly obtained by coating with a perfluoropolyether coating, and the thickness of the AF layer is in the range of 1-90 nm.
[0037] In an optional embodiment, a PET high temperature positive protective layer can be stacked on one side of the AF layer away from the silicon oxide layer. The PET high temperature positive protective layer can further enhance the high temperature resistance of the low reflection and low transmittance flexible optical film and enhance the protection effect on other film layers.
[0038] The above is the overall concept of the present invention, and detailed embodiments are provided below on the basis of the overall concept to further illustrate the present invention.
[0039] Example 1
[0040] The HUD film containing SiO2 and Ti in this embodiment includes a substrate layer, a lower coating layer, a substrate layer, an upper coating layer, a primer layer, a TiO2 layer, a metal layer and a SiO2 layer stacked in sequence.
[0041] The coating thickness of the upper coating layer is 180nm, and the coating thickness of the lower coating layer is 0.35μm. After coating, a 109μm high-temperature protective film is attached to the lower coating layer. SiO2 is used as the base layer, and the thickness of the base layer is 10.1nm. The thickness of the TiO2 layer is 75nm, the thickness of the metal layer is 75nm, nickel accounts for 70%, and chromium accounts for 30%. The thickness of the SiO2 layer is 125nm. The SiO2 layer is formed by a magnetron sputtering process. The target material used in the magnetron sputtering process is a mixed target including silicon and aluminum, and the reaction gas bombarding the target material is a mixed gas including argon, nitrogen and oxygen. In the mixed target, silicon accounts for 91% and aluminum accounts for 9%. In the mixed gas, argon accounts for 69%, nitrogen accounts for 26%, and oxygen accounts for 5%.
[0042] Comparative Example 1
[0043] The difference between Comparative Example 1 and Example 1 is that Comparative Example 1 does not include TiO2, and the SiO2 layer is formed in a different manner. In Comparative Example 1, the SiO2 layer is formed by a magnetron sputtering process, the target material selected in the magnetron sputtering process is a pure silicon target, and the reaction gas bombarding the target material is argon.
[0044] For comparison of wear resistance, see Table 1 and Table 2 below.
[0045] The wear resistance of steel wool is shown in Table 1 below.
[0046]
[0047] Unified test method, the back of the experimental sample is attached with OCA glue, and then attached to the transparent glass. After attachment, the degassing machine is used to degas. After degassing, the surface is wiped clean, the coated surface faces up, the wear machine is loaded with a 1000g weight, and the wear head is fixed with Bonstar 0000# steel wool placed on the membrane surface. The stroke is 60mm long, and one back and forth grinding is one stroke. The left, middle, and right in the table refer to the film sheet path. The width of the film is 1200mm. Take the left, middle, and right points for testing.
[0048] When the wear resistance test was performed for 1000 and 2000 times, no scratches were found on the film surfaces of Comparative Example 1 and Example 1, and the results were judged to be OK.
[0049] When the wear resistance test was performed 2500 times, one scratch appeared on the left and middle sides of Comparative Example 1, and it was judged as NG. No scratch appeared in Example 1, indicating that Example 1 is superior to Comparative Example 1.
[0050] When the wear resistance test was performed 3000 times, 3-5 scratches appeared on Comparative Example 1, which was judged as NG. No scratches appeared on Example 1, which indicated that Example 1 was superior to Comparative Example 1.
[0051] Therefore, the steel wool in Example 1 has relatively good wear resistance.
[0052] Further, the wear resistance of the eraser is shown in Table 2 below.
[0053]
[0054] Unified test method, OCA glue is applied to the back, and it is attached to the transparent glass. After bonding, it is degassed with a degassing machine. After degassing, the surface is wiped clean, and the coated surface faces up. The wear-resistant machine is loaded with a 1000g weight, and the wear-resistant head is fixed with a CS-6# eraser and placed on the film surface. The stroke is 60mm long, and one back and forth grinding is one stroke. The left, middle, and right in the table refer to the film sheet path. The film width is 1200mm. Take the left, middle, and right points for testing.
[0055] When the wear resistance test was performed 50-100 times, no scratches were found on the film surfaces of Comparative Example 1 and Example 1, and the films were judged to be OK.
[0056] When the wear resistance test was performed 200 times, 1-2 scratches appeared on the comparative example 1, and it was judged as NG. No scratches appeared on the example 1, indicating that the example 1 was superior to the comparative example 1.
[0057] After 500 abrasion tests, 4-7 scratches appeared on Comparative Example 1, and it was judged as NG. One scratch appeared on the left side of Example 1, and no scratches appeared in the middle and right sides. Overall comparison shows that Example 1 is better than Comparative Example 1.
[0058] In summary, the HUD film containing SiO2 and Ti in the embodiment of the present invention has better overall wear resistance. When the driver uses the HUD film subsequently, he can obtain clear and accurate driving information, thereby improving driving safety.
[0059] On this basis, the HUD film containing SiO2 and Ti in the embodiment of the present invention also has good transmittance and reflectivity. The test data are as follows:
[0060] Comparison of P light reflection and S light reflection, refer to Figure 2-Figure 4 .in, Figure 2-Figure 4 In FIG. 1 , the dotted line represents the experimental curve of Comparative Example 1, and the solid line represents the experimental curve of Example 1.
[0061] The test method is unified. Before the test, the back is attached with OCA glue and attached to a black acrylic board. After attachment, the degassing machine is used to degas. After degassing, the surface is wiped clean and tested with a Hitachi spectrophotometer.
[0062] Reference Figure 2 , test the P light reflection at 60° angle, the test method is eyepiece 0° angle, small circle 60° angle, large circle 120° angle. The test results show that in the 380-780nm band range, the average value of comparative example 1 is 22.9%, and the average value of embodiment 1 is 25.5%. In the 400-700nm band range, the average value of comparative example 1 is 22.8%, and the average value of embodiment 1 is 25.6%. It shows that the average value of P light reflection of embodiment 1 is higher than that of comparative example 1, and embodiment 1 is slightly better.
[0063] Reference Figure 3 , test the S light reflection at 60° angle, the test method is eyepiece 0° angle, small circle 60° angle, large circle 120° angle. The test results show that in the 380-780nm band range, the average value of comparative example 1 is 15.4%, and the average value of embodiment 1 is 18.1%. In the 400-700nm band range, the average value of comparative example 1 is 12.5%, and the average value of embodiment 1 is 15.2%. It shows that the average value of S light reflection of embodiment 1 is higher than that of comparative example 1, and embodiment 1 is slightly better.
[0064] Reference Figure 4 , test transmission, bare film test, angle 0°, no need to adjust the angle. The test results show that comparative example 1 transmits 23.4% in the range of 380-780nm, and embodiment 1 transmits 26.6%. In the range of 400-700nm, comparative example 1 transmits 24.1%, and embodiment 1 transmits 27.2%. This shows that the average transmittance of embodiment 1 is higher than that of comparative example 1, and embodiment 1 is slightly better.
[0065] Therefore, combined with the above data, it can be seen that the HUD film containing SiO2 and Ti in this embodiment has high transmittance and good reflection effect of P light and S light, so it can be effectively applied to the front windshield of the car to provide navigation information for the driver. Since there is no need to look down to see the specific driving information, it can effectively improve driving safety.
[0066] It should be noted that P light and S light are two different polarized lights, which have different characteristics in optical phenomena, and therefore their performance needs to be tested separately.
[0067] At the same time, the HUD film containing SiO2 and Ti in the embodiment of the present invention also has good environmental testing performance.
[0068] The performance comparison of various environmental tests is shown in Table 3 and Table 4.
[0069] The unified testing method is as follows:
[0070] Before the ring test, the back is attached with OCA glue and attached to the black acrylic board. After attachment, the degassing machine is used to degas. After degassing, the surface is wiped clean. During the test, the test sample is cut with a grid knife, and then the surface of the test sample is pressed with tape. After standing for more than 30 seconds, the tape is pulled off. No peeling is 5B, slight peeling is 3-4B, barely OK, and 2B or less is NG.
[0071]
[0072] It can be seen from the above table:
[0073] The test was conducted using double 85 rings (high temperature 85°C, high humidity 85%). Compared to the 30-day test, all the grids were 5B. The 35-day test results for comparative example 1 were 2-3B, and all the grids for example 1 were 5B, indicating that example 1 was superior.
[0074] Tested for sunlight resistance (light 0.55w / (m 2 .nm), wavelength 340nm, filter Extended UV-Q / B, 3.8h of light + 1h of darkness as one cycle. The temperature of the illuminated blackboard was set at 89°C, the temperature of the box was 63°C, and the humidity was 50%; the temperature of the box and blackboard was set at 38°C and the humidity was 95% in the dark stage. The average of 100 grids was 5B in 30 days, 1-3B in Comparative Example 1 in 35 days, and 5B in Example 1, indicating that Example 1 is better.
[0075] In the QUV resistance test (UV-A (340nm) 0.63W / m2 (4h), condensation 50℃ (4h) as 1 cycle), the 30-day 100-grid value in comparative example 1 was 2-4B, the 35-day 100-grid value in comparative example 1 was 0-2B, and the 30-day and 35-day 100-grid values in example 1 were both 5B, indicating that example 1 is superior.
[0076] The high temperature ring test (95°C) showed that the 100 grids were all 5B after 30 days, 1-3B after 35 days for comparative example 1, and 5B after 35 days for example 1, indicating that example 1 is better.
[0077]
[0078]
[0079] It can be seen from the above table:
[0080] The low temperature environment test (-40°C) showed that the 100 grids were all 5B after 30 days, 3-4B after 35 days for comparative example 1, and 5B after 35 days for example 1, indicating that example 1 is better.
[0081] Test salt spray ring test (temperature 35℃, salt water concentration 5%). Preparation method of salt water: 500g sodium chloride and 9500ml pure water, stir evenly. Compared with 30 days, the average of 100 grids is 5B, 35 days of comparative example 1 is 2-3B, and Example 1 is 5B, which shows that Example 1 is better.
[0082] Test 65 / 93 ring test (temperature 65°C, humidity 93%), compared with 30 days 100 grids are 5B, 35 days comparative example 1 is 1-3B, embodiment 1 is 5B, indicating that embodiment 1 is better.
[0083] The xenon lamp ambient test (UV-A (340nm) 0.6W / m2, blackboard temperature 65°C, air temperature 65°C, relative humidity 30%) showed that the 100 grids were 3-4B after 20 days, 0-1B after 25 days for comparative example 1, and 5B for example 1, indicating that example 1 is better.
[0084] Therefore, combined with the above data, it can be seen that the HUD film containing SiO2 and Ti in the embodiment of the present invention also has good environmental testing performance.
[0085] In summary, the HUD film containing SiO2 and Ti disclosed in the present invention has excellent wear resistance, and also has excellent transmittance, reflection and environmental performance. It can be effectively applied to the front windshield of a car to provide the driver with clear and complete driving information and ensure driving safety.
[0086] Reference Figure 1 One embodiment of the present invention further discloses a preparation process for preparing the above-mentioned HUD film containing Nb2O5, comprising the following steps:
[0087] A primer layer, a TiO2 layer, a metal layer and a SiO2 layer are sequentially plated on the substrate layer by a magnetron coating sputtering process;
[0088] Wherein, in the step of plating the SiO2 layer, the following steps are also included:
[0089] A mixed target material including silicon and aluminum and a mixed gas including argon and oxygen are provided; in this embodiment, silicon accounts for 82-99% and aluminum accounts for 18-1% in the mixed target.
[0090] In this embodiment, the mixed gas may be argon, oxygen and nitrogen, with argon accounting for 60-78%, nitrogen accounting for 18-35%, and oxygen accounting for 3-8%.
[0091] The coating chamber is evacuated and the mixed target is driven to rotate in the coating chamber. The vacuum degree of the coating chamber is controlled to be less than 1×10 -4 pa, water vapor value is less than 9×10 -5 The rotation speed of the mixed target is preferably uniform.
[0092] The target material sputtering deposition is started, and the mixed target material is bombarded by the mixed gas. The thickness of the SiO2 layer is 20-220nm, and the thickness is controlled according to the target material bombardment time.
[0093] The HUD film prepared through the above steps has good wear resistance, transmittance, reflection effect and environmental testing performance, and can provide the driver with clear and complete driving information to ensure driving safety.
[0094] In an optional embodiment, before the step of coating the base layer on the substrate layer, an upper coating layer and a lower coating layer can be provided on both sides of the substrate layer by a coating process. The upper coating layer and the lower coating layer are formed by coating an acrylic resin coating liquid. The coating thickness of the upper coating layer is 40-320nm, and the coating thickness of the lower coating layer is 0.3-3.9μm. After coating, a 30-188μm high-temperature protective film is attached to the lower coating layer to provide protection for the appearance of the film surface during the subsequent magnetron sputtering coating process to ensure the stability of the coating. After the step of coating the SiO2 layer, an AF layer and a PET high-temperature positive protective layer can also be stacked in sequence on the side of the SiO2 layer away from the metal layer. The AF layer is mainly obtained by coating with a perfluoropolyether coating.
[0095] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered exemplary and non-limiting in all respects, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations falling within the meaning and scope of the equivalent elements of the claims be included in the invention. Any reference numeral in a claim should not be considered as limiting the claim to which it relates.
[0096] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.
Claims
1. A HUD film containing SiO2 and Ti, characterized in that: It includes a substrate layer, a base layer, a TiO2 layer, a metal layer and a SiO2 layer which are stacked in sequence. The SiO2 layer is formed by a magnetron sputtering process. The target material selected in the magnetron sputtering process is a mixed target including silicon and aluminum. The reaction gas bombarding the target material is a mixed gas including argon, nitrogen and oxygen.
2. The HUD film containing SiO2 and Ti according to claim 1, characterized in that: The thickness of the TiO2 layer is in the range of 5-125 nm.
3. The HUD film containing SiO2 and Ti according to claim 1, characterized in that: In the mixed target, silicon accounts for 82-99% and aluminum accounts for 18-1%.
4. The HUD film containing SiO2 and Ti according to claim 1, characterized in that: In the mixed gas, argon accounts for 60-78%, nitrogen accounts for 18-35%, and oxygen accounts for 3-8%.
5. The HUD film containing SiO2 and Ti according to claim 1, characterized in that: The thickness of the SiO2 layer is in the range of 20-220 nm.
6. The HUD film containing SiO2 and Ti according to claim 1, characterized in that: The base layer is selected from one of SiO2, Ti, TiO2, Si, Al2O3, MgF2, SiO, HfO2, SnO2, and Y2O3.
7. The HUD film containing SiO2 and Ti according to claim 6, characterized in that: The thickness of the base layer is in the range of 0.2-20 nm.
8. The HUD film containing SiO2 and Ti according to claim 1, characterized in that: The metal layer is a nickel-chromium layer, wherein nickel accounts for 50-90% and chromium accounts for 50-10%.
9. A process for preparing a HUD film containing SiO2 and Ti as claimed in any one of claims 1 to 8, characterized in that: The following steps are involved: A primer layer, a TiO2 layer, a metal layer and a SiO2 layer are sequentially plated on the substrate layer by a magnetron coating sputtering process; Wherein, in the step of plating the SiO2 layer, the following steps are also included: Providing a mixed target material including silicon and aluminum and a mixed gas including argon, nitrogen and oxygen; evacuating the coating chamber and driving the mixed target to rotate in the coating chamber; The target material sputtering deposition is started, and the mixed target material is bombarded by the mixed gas.
10. The process for preparing a HUD film containing SiO2 and Ti according to claim 9, characterized in that: In the step of evacuating the coating chamber, the vacuum degree of the coating chamber is controlled to be less than 1×10 -4 pa, water vapor value is less than 9×10 -5 pa.