Stripping solution for nickel-plated automobile parts with copper alloy as base material and preparation method of stripping solution
By using a combination of sulfuric acid, hydrochloric acid, citric acid, thiourea and benzotriazole derivatives in the nickel plating deplating solution, the problems of high toxicity, high energy consumption and substrate damage in the nickel plating deplating process are solved. It achieves an environmentally friendly, low-energy-consuming deplating effect and protects the copper alloy substrate.
Patent Information
- Application Number
- CN202410984372.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-11-05
AI Technical Summary
The existing nickel plating deplating process has problems such as highly toxic, unenvironmental protection, high energy consumption, difficulty in treating wastewater and damage to the substrate.
Using sulfuric acid, hydrochloric acid, citric acid, thiourea and benzotriazole derivatives as nickel-removing liquid, sulfur atoms, ester groups, double bonds and alkyl chains are introduced into the benzotriazole molecule through two-step reactions to form An efficient organic corrosion inhibitor combined with thiourea and electric field effect to achieve safe removal of nickel layer.
A low-toxic and low-energy-consuming deplating process is achieved, the copper alloy substrate is protected, the wastewater treatment difficulty is reduced, and the deplating efficiency and product reuse rate are improved.
Smart Images

Figure BDA0004956970710000021 
Figure FDA0004956970700000011
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of chemical stripping, and in particular relates to a stripping solution for nickel-plated automobile parts with a copper alloy as a substrate and a preparation method thereof. Background Art
[0002] Chemical nickel plating has developed rapidly in just a few decades due to its unique characteristics in wear resistance and corrosion resistance. This technology has become a very mature high-tech in the United States, Japan, and Germany, and its application range covers almost all industrial fields, such as storage tanks, pipes, dosing devices, heat exchangers, and rotating machinery in contact with corrosive substances in chemical equipment; general equipment, bearings, and rollers in the machinery industry; refining equipment and petrochemical instruments and downhole tools in the petroleum industry, etc., thus reflecting its value in reducing wear, corrosion, preventing pollution, and reducing investment and maintenance costs. However, plating quality problems are inevitable in the nickel plating process, resulting in unqualified products. Usually, the production line will remove the nickel plating of unqualified products and then re-plating them to obtain qualified products that meet the process requirements.
[0003] Patent application number CN201310181588.0 provides an efficient and environmentally friendly nickel stripping agent, which includes the following main raw materials: ethylenediamine, sodium m-nitrobenzene sulfonate, citric acid, organic amine additives, and pure water. The invention uses the oxidizing ability of sodium m-nitrobenzene sulfonate and the coordination ability of ethylenediamine to promote the rapid stripping of the nickel layer, reduce the large amount of smoke generated during stripping, and thus avoid the problems of high toxicity and poor operating environment of cyanide stripping, and the generation of thick smoke and easy corrosion of the substrate by concentrated nitric acid from the source; Patent application number CN201310123266.0 provides a The invention discloses a stripping solution for chemical nickel plating of cast aluminum parts, comprising the following main raw materials: nitric acid, sodium m-nitrobenzene sulfonate, nickel powder, pure water, hydrofluoric acid, and sodium chloride. The stripping solution provided by the invention has a simple manufacturing process, is easy to control, and has an obvious stripping effect. After the stripping treatment, unqualified products can be reused, thereby reducing production costs and improving production efficiency and process levels. The above inventions all select sodium m-nitrobenzene sulfonate as the effective ingredient of the stripping solution, which is a dye-resistant salt-type stripping solution. When it is used for stripping nickel plating, the operating temperature is relatively high, and wastewater treatment is difficult, which in turn leads to high energy consumption in the stripping process. Summary of the invention
[0004] In view of the deficiencies in the prior art, the purpose of the present invention is to provide a deplating solution for nickel-plated automobile parts with copper alloy as the substrate and a preparation method thereof, wherein sulfuric acid, hydrochloric acid, citric acid and thiourea are used to achieve nickel stripping, wherein the sulfuric acid and hydrochloric acid in the deplating solution do not react with the copper alloy substrate, and citric acid is a weak acid and does not react with copper and the copper alloy substrate. The present invention adopts sulfuric acid, phosphoric acid, citric acid, hydrochloric acid and benzotriazole derivatives as a whole, thereby solving the problems that the traditional nickel stripping process is highly toxic, not environmentally friendly, has high energy consumption, is difficult to treat wastewater and the substrate is damaged after nickel stripping.
[0005] The technical solution adopted by the present invention to achieve the above-mentioned purpose is:
[0006] A deplating solution for nickel-plated automobile parts with a copper alloy as a substrate, wherein each liter of the deplating solution is composed of the following components: 100-200 mL of sulfuric acid, 5-10 mL of hydrochloric acid, 50-80 g of citric acid, 15-30 g of thiourea, and 0.2-0.4 g of a benzotriazole derivative, and the solvent is water; the mass fraction of the hydrochloric acid is 37-38%;
[0007] The preparation method of the benzotriazole derivative is as follows:
[0008] S1. Under stirring conditions, disperse benzotriazole in 2-methyltetrahydrofuran, add methylthiopropylene oxide and N,N-dimethylcyclohexylamine in sequence after complete dissolution, react at 80-100°C for 4-8h, cool to room temperature, filter, take the filtrate, distill under reduced pressure, and dry to obtain an intermediate;
[0009] S2. Disperse the intermediate obtained in step S1 and acrylic acid in toluene under stirring, add p-toluenesulfonic acid, react at 70-90° C. for 5-9 hours, add deionized water and sodium bicarbonate in sequence after cooling, continue to react for 0.5-1.5 hours, filter, take the filtrate, extract, distill under reduced pressure, and dry to obtain a benzotriazole derivative;
[0010] The synthetic route of benzotriazole derivatives is as follows:
[0011]
[0012] Benzotriazole is a highly efficient organic corrosion inhibitor. It has a good corrosion inhibition effect in the pH range of 5.5-10, but its corrosion inhibition effect is reduced in a medium with a low pH value. In order to ensure that the corrosion inhibition effect of benzotriazole in a low pH environment is not disturbed, the present invention uses benzotriazole and methylthiopropylene oxide as starting materials, and an epoxy compound ring-opening reaction occurs under the catalysis of N,N-dimethylcyclohexylamine to obtain an intermediate; then, the intermediate and acrylic acid are used as raw materials, and an esterification reaction occurs under the catalysis of p-toluenesulfonic acid to obtain a benzotriazole derivative. The two-step method is used to modify the benzotriazole molecule, and sulfur atoms, ester groups, double bonds and alkyl chains are introduced into the molecular structure, thereby achieving the regulation of the properties and functions of the compound.
[0013] In order to obtain benzotriazole derivatives and ensure product consistency, the molar ratio of benzotriazole, methylthiopropylene oxide and N,N-dimethylcyclohexylamine in step S1 is 1:0.7-0.9:0.03-0.05, and the amount of benzotriazole added in 2-methyltetrahydrofuran is 0.1-0.3 g / mL; the molar ratio of the intermediate, acrylic acid and p-toluenesulfonic acid in step S2 is 1.2:0.8-1.0:0.04-0.07, the mass ratio of p-toluenesulfonic acid, deionized water and sodium bicarbonate is 4-8:25-35:3-7, and the amount of acrylic acid added in toluene is 0.15-0.25 g / mL.
[0014] Organic corrosion inhibitor molecules usually have both polar groups and non-polar groups. The polar groups contain nitrogen, oxygen, phosphorus, sulfur and other elements, all of which contain lone pairs of electrons and have high electronegativity. Organic corrosion inhibitors are firmly adsorbed on the metal surface through polar groups, while non-polar groups are arranged in the medium. This effectively isolates the contact between the metal and the corrosive medium, hinders the diffusion of corrosion reaction products, and also changes the double electric layer structure, increases the activation energy of the corrosion reaction, and ultimately inhibits the corrosion reaction. The corrosion inhibition performance of organic corrosion inhibitors depends on the strength of the adsorption of its polar groups on the metal surface, and the adsorption of polar groups can be physical adsorption or chemical adsorption. In most cases, the two adsorptions work together. Physical adsorption is very fast, a reversible process, and easy to desorb. The thermal effect of the adsorption process is small and is less affected by temperature. Physical adsorption will be significantly affected by the excess charge on the metal surface. Most organic corrosion inhibitors exist in the form of cations in acidic media. If the metal surface carries excess negative charge, there will be a strong electrostatic attraction between the metal surface and the corrosion inhibitor, making it easier for the corrosion inhibitor to adsorb on the metal surface, and the adsorption force is also stronger; on the contrary, if there is excess positive charge on the metal surface, it will inhibit the adsorption of the corrosion inhibitor to the metal surface to a certain extent. In the actual application of corrosion inhibitors, the physical adsorption of corrosion inhibitors can be promoted by changing the amount of excess charge carried on the metal surface. For example, in an acidic medium, after adding a small amount of iodide, the corrosion inhibition performance of organic amines will be significantly improved. This is mainly because after iodide is adsorbed on the metal surface, the metal surface carries more excess negative charge, which promotes the adsorption of organic amine corrosion inhibitors on the metal surface; similarly, the reason why organic amine corrosion inhibitors have excellent corrosion inhibition performance in hydrochloric acid media is also partly attributed to the fact that chloride ions make the metal surface carry more excess charge. Compared with physical adsorption, chemical adsorption has a stronger force and is more stable. Therefore, the interaction between most organic corrosion inhibitors and metal surfaces is mainly achieved through chemical adsorption, and the essence of chemical adsorption is the formation of coordination bonds between corrosion inhibitor molecules or ions and metal surface atoms. The central atoms of corrosion inhibitors such as nitrogen, oxygen, sulfur, and phosphorus have lone pairs of electrons. The lone pairs of electrons of the central atoms of corrosion inhibitors will form coordination bonds with the atoms on the metal surface. Through the strong force of the chemical bond such as coordination bonds, the corrosion inhibitor molecules or ions are firmly adsorbed on the metal surface; in addition, the double bonds or triple bonds in the π bonds can also combine with the empty d orbitals of metal atoms to form coordination bonds, so that the corrosion inhibitor molecules are adsorbed on the metal surface.
[0015] When the concentration of sulfuric acid, hydrochloric acid and citric acid in the deplating solution provided by the present invention is low, the deplating time is long and the deplating efficiency is also low; when the concentration of sulfuric acid, hydrochloric acid and citric acid is high, the deplating speed is accelerated, but when the concentration is too high and exceeds the process range, the deplating speed will decrease. Under acidic conditions, nickel is decomposed under the combined action of thiourea and electric field, precipitated on the cathode plate, and the benzotriazole derivative is adsorbed on the surface of the substrate to protect the substrate from corrosion.
[0016] The present invention also provides a method for preparing a deplating solution for nickel-plated automobile parts with a copper alloy as a substrate, comprising the following steps:
[0017] (1) Weigh out the formulated amounts of sulfuric acid, hydrochloric acid, citric acid, thiourea, benzotriazole derivatives, and water and set aside;
[0018] (2) dissolving the sulfuric acid, hydrochloric acid and citric acid weighed in step (1) in part of the water weighed in step (1), stirring and mixing to obtain a mixed solution 1;
[0019] (3) Add the thiourea and benzotriazole derivatives weighed in step (1) to the mixed solution 1 obtained in step (2) in sequence, stir until completely dissolved, and make up to volume with the remaining amount of water to obtain the product.
[0020] Furthermore, the portion of water in step (2) accounts for 1 / 2-2 / 3 of the total mass of water.
[0021] The present invention has the following beneficial effects:
[0022] The present invention utilizes two-step reaction to introduce sulfur atom, ester group, double bond and alkyl chain into the molecular structure of benzotriazole to obtain benzotriazole derivatives; there are lone pair electrons in the sulfur atom, which will form coordination bonds with metal surface atoms, and the double bond can also be combined with the d empty orbit of the metal atom to form a coordination bond, and when the ester group is close to the double bond as a polar group, a large π bond is formed due to the conjugation effect, which enhances the adsorption force of the benzotriazole derivative on the metal surface, so that the prepared organic corrosion inhibitor has a variety of adsorption centers, and the corrosion inhibition performance is more excellent; the introduction of the alkyl chain can not only increase the electron cloud density on the central atom of the corrosion inhibitor, thereby increasing the coordination ability of the central atom and the metal atom, but also effectively isolate the contact between the metal and the corrosive medium, hinder the diffusion of the corrosive medium, and further improve its corrosion inhibition performance. The present invention compounds thiourea with benzotriazole derivatives, and in a corrosive medium containing hydrochloric acid, the thickness and compactness of the protective layer can be increased, the transmission of corrosive ions is effectively blocked, and excellent synergistic corrosion inhibition is shown.
[0023] The deplating solution provided by the present invention does not generate harmful gas during the deplating process and does not need to be heated. After the electrolytic deplating is completed, the electrolytic current is automatically reduced to zero, and the deplating is completed. The deplating process hardly corrodes the copper alloy, and the copper alloy substrate can be well protected from corrosion. DETAILED DESCRIPTION
[0024] The following will be combined with the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of this application. The raw materials used in the following embodiments are all common commercially available products.
[0025] Example 1
[0026] A method for preparing a benzotriazole derivative comprises the following steps:
[0027] S1. Under stirring at 200 rpm, benzotriazole was dispersed in 2-methyltetrahydrofuran, and after complete dissolution, methylthiopropylene oxide and N,N-dimethylcyclohexylamine were added in sequence, and the mixture was reacted at 90°C for 6 hours, cooled to room temperature, filtered, and the filtrate was taken. 2-methyltetrahydrofuran was removed by vacuum distillation under reduced pressure, and vacuum dried at 50°C for 12 hours to obtain an intermediate, wherein the molar ratio of benzotriazole, methylthiopropylene oxide and N,N-dimethylcyclohexylamine was 1:0.8:0.04, and the amount of benzotriazole added in 2-methyltetrahydrofuran was 0.2 g / mL;
[0028] S2. Under stirring at 200 rpm, disperse the intermediate obtained in step S1 and acrylic acid in toluene, add p-toluenesulfonic acid, react at 80°C for 7h, cool to 35-40°C, then add deionized water and sodium bicarbonate in sequence, continue to react for 1h, filter, take the filtrate, add ethyl acetate for extraction, take the organic phase and distill under reduced pressure, and vacuum dry at 60°C for 24h to obtain a benzotriazole derivative, wherein the molar ratio of the intermediate, acrylic acid, and p-toluenesulfonic acid is 1.2:0.9:0.05, the mass ratio of p-toluenesulfonic acid, deionized water, and sodium bicarbonate is 5:30:4, and the amount of acrylic acid added to toluene is 0.19 g / mL;
[0029] The NMR results of benzotriazole derivatives are: 1 H NMR (300MHz, DMSO-d6) δ 8.07 (d, 1H), 7.97 (d, 1H), 7.58 (t, 1H), 7.36 (t, 1H), 6.41 (d, 1H), 6.10-6.14 (m, 1H), 5.82 ( d, 1H), 4.90-4.95 (m, 1H), 4.08-4.11 (m, 1H), 3.80-3.84 (m, 1H), 2.79-2.84 (m, 1H), 2.50-2.54 (m, 1H), 2.07 (s, 3H).
[0030] A method for preparing a deplating solution for nickel-plated automobile parts with a copper alloy as a substrate comprises the following steps:
[0031] (1) Weighing the formula amount of sulfuric acid (concentration>98%), hydrochloric acid, citric acid, thiourea, benzotriazole derivatives, and water for use; wherein each liter of the deplating solution is composed of the following components: 150 mL of sulfuric acid, 8 mL of hydrochloric acid, 65 g of citric acid, 25 g of thiourea, and 0.3 g of benzotriazole derivatives, and the solvent is water; wherein the mass fraction of hydrochloric acid is 37.5%;
[0032] (2) dissolving the sulfuric acid, hydrochloric acid and citric acid weighed in step (1) in part of the water weighed in step (1) (the part of the water accounts for 2 / 3 of the total mass of the water), stirring and mixing to obtain a mixed solution 1;
[0033] (3) Add the thiourea and benzotriazole derivatives weighed in step (1) to the mixed solution 1 obtained in step (2) in sequence, stir until completely dissolved, and make up to volume with the remaining amount of water to obtain the product.
[0034] Example 2
[0035] A method for preparing a deplating solution for nickel-plated automobile parts with a copper alloy as a substrate comprises the following steps:
[0036] (1) Weigh out the formula amount of sulfuric acid (concentration>98%), hydrochloric acid, citric acid, thiourea, the benzotriazole derivative prepared in Example 1, and water for use; wherein each liter of the deplating solution is composed of the following components: 100 mL of sulfuric acid, 10 mL of hydrochloric acid, 80 g of citric acid, 15 g of thiourea, and 0.2 g of the benzotriazole derivative, and the solvent is water; wherein the mass fraction of hydrochloric acid is 37.5%;
[0037] (2) dissolving the sulfuric acid, hydrochloric acid and citric acid weighed in step (1) in part of the water weighed in step (1) (the part of the water accounts for 1 / 2 of the total mass of the water), stirring and mixing to obtain a mixed solution 1;
[0038] (3) Add the thiourea and benzotriazole derivatives weighed in step (1) to the mixed solution 1 obtained in step (2) in sequence, stir until completely dissolved, and make up to volume with the remaining amount of water to obtain the product.
[0039] Example 3
[0040] A method for preparing a deplating solution for nickel-plated automobile parts with a copper alloy as a substrate comprises the following steps:
[0041] (1) Weigh the formula amount of sulfuric acid (concentration>98%), hydrochloric acid, citric acid, thiourea, the benzotriazole derivative prepared in Example 1, and water for use; wherein each liter of the deplating solution is composed of the following components: 120 mL of sulfuric acid, 9 mL of hydrochloric acid, 70 g of citric acid, 20 g of thiourea, and 0.3 g of the benzotriazole derivative, and the solvent is water; wherein the mass fraction of hydrochloric acid is 37.5%;
[0042] (2) dissolving the sulfuric acid, hydrochloric acid and citric acid weighed in step (1) in part of the water weighed in step (1) (the part of the water accounts for 2 / 3 of the total mass of the water), stirring and mixing to obtain a mixed solution 1;
[0043] (3) Add the thiourea and benzotriazole derivatives weighed in step (1) to the mixed solution 1 obtained in step (2) in sequence, stir until completely dissolved, and make up to volume with the remaining amount of water to obtain the product.
[0044] Example 4
[0045] A method for preparing a deplating solution for nickel-plated automobile parts with a copper alloy as a substrate comprises the following steps:
[0046] (1) Weigh out the formula amount of sulfuric acid (concentration>98%), hydrochloric acid, citric acid, thiourea, the benzotriazole derivative prepared in Example 1, and water for use; wherein each liter of the deplating solution is composed of the following components: 200 mL of sulfuric acid, 5 mL of hydrochloric acid, 50 g of citric acid, 30 g of thiourea, and 0.4 g of the benzotriazole derivative, and the solvent is water; wherein the mass fraction of hydrochloric acid is 37.5%;
[0047] (2) dissolving the sulfuric acid, hydrochloric acid and citric acid weighed in step (1) in part of the water weighed in step (1) (the part of the water accounts for 2 / 3 of the total mass of the water), stirring and mixing to obtain a mixed solution 1;
[0048] (3) Add the thiourea and benzotriazole derivatives weighed in step (1) to the mixed solution 1 obtained in step (2) in sequence, stir until completely dissolved, and make up to volume with the remaining amount of water to obtain the product.
[0049] Comparative Example 1
[0050] A method for preparing a deplating solution for nickel-plated automobile parts with a copper alloy as a substrate comprises the following steps:
[0051] (1) Weigh the formula amount of sulfuric acid (concentration>98%), hydrochloric acid, citric acid, thiourea, the benzotriazole derivative prepared in Example 1, and water for use; wherein each liter of the deplating solution is composed of the following components: 150 mL of sulfuric acid, 8 mL of hydrochloric acid, 65 g of citric acid, 25 g of thiourea, and 0.1 g of the benzotriazole derivative, and the solvent is water; wherein the mass fraction of hydrochloric acid is 37.5%;
[0052] (2) dissolving the sulfuric acid, hydrochloric acid and citric acid weighed in step (1) in part of the water weighed in step (1) (the part of the water accounts for 2 / 3 of the total mass of the water), stirring and mixing to obtain a mixed solution 1;
[0053] (3) Add the thiourea and benzotriazole derivatives weighed in step (1) to the mixed solution 1 obtained in step (2) in sequence, stir until completely dissolved, and make up to volume with the remaining amount of water to obtain the product.
[0054] Comparative Example 2
[0055] A method for preparing a deplating solution for nickel-plated automobile parts with a copper alloy as a substrate comprises the following steps:
[0056] (1) Weigh the formula amount of sulfuric acid (concentration>98%), hydrochloric acid, citric acid, thiourea, benzotriazole, and water for use; wherein each liter of the deplating solution is composed of the following components: 150 mL of sulfuric acid, 8 mL of hydrochloric acid, 65 g of citric acid, 25 g of thiourea, and 0.3 g of benzotriazole, and the solvent is water; wherein the mass fraction of hydrochloric acid is 37.5%;
[0057] (2) dissolving the sulfuric acid, hydrochloric acid and citric acid weighed in step (1) in part of the water weighed in step (1) (the part of the water accounts for 2 / 3 of the total mass of the water), stirring and mixing to obtain a mixed solution 1;
[0058] (3) Add the thiourea and benzotriazole weighed in step (1) to the mixed solution 1 obtained in step (2) in sequence, stir until completely dissolved, and make up to volume with the remaining amount of water to obtain the product.
[0059] Comparative Example 3
[0060] A method for preparing a deplating solution for nickel-plated automobile parts with a copper alloy as a substrate comprises the following steps:
[0061] (1) Weighing the formula amount of sulfuric acid (concentration>98%), hydrochloric acid, citric acid, thiourea, and water for use; wherein each liter of the deplating solution is composed of the following components: 150 mL of sulfuric acid, 8 mL of hydrochloric acid, 65 g of citric acid, and 35 g of thiourea, and the solvent is water; wherein the mass fraction of hydrochloric acid is 37.5%;
[0062] (2) dissolving the sulfuric acid, hydrochloric acid and citric acid weighed in step (1) in part of the water weighed in step (1) (the part of the water accounts for 2 / 3 of the total mass of the water), stirring and mixing to obtain a mixed solution 1;
[0063] (3) Add the thiourea weighed in step (1) to the mixed solution 1 obtained in step (2), stir until completely dissolved, and make up to volume with the remaining amount of water to obtain the product.
[0064] The deplating solutions prepared in Examples 1-4 and Comparative Examples 1-3 were subjected to relevant performance tests. The deplating solutions prepared in Examples 1-4 and Comparative Examples 1-3 were used to deplating nickel-plated automobile parts based on copper alloys, and the specific process was as follows: the nickel-plated automobile parts were cleaned and used as workpieces to be deplated, and the deplating solution was added to the electrolytic cell, the workpiece to be deplated was used as the anode, the lead plate was used as the cathode, and the parts were placed in the deplating solution at 20-30°C, and the electrolytic current was set to 10A for electrolytic deplating. When the nickel coating was deplated, the electrolytic current automatically decreased to zero, and the deplating was completed. The nickel coating thickness, nickel deplating time, and copper corrosion thickness were recorded, the surface condition of the workpiece substrate was observed, and the surface of the workpiece substrate was evaluated for pitting or pit-shaped corrosion, and the nickel deplating speed and copper corrosion speed were calculated. The calculation formula was: nickel deplating speed = nickel coating thickness / nickel deplating time, copper corrosion speed = copper corrosion thickness / nickel deplating time; each group of tests was repeated three times to take the average value, and the test results are shown in Table 1. It can be seen from Table 1 that compared with Comparative Examples 1-3, the deplating solutions prepared in Examples 1-4 maintain a relatively high nickel stripping rate while also having a relatively low copper corrosion rate. After the electrolytic deplating process is completed, there is no pitting corrosion or pitting corrosion on the surface of the workpiece substrate. The deplating process causes less damage to the substrate, and the product obtained by deplating can be re-electroplated with only ordinary pre-treatment.
[0065] Table 1 Deplating solution related performance test results
[0066] Test items Nickel stripping speed (μm / min) Copper etching speed (μm / min) Surface condition of workpiece substrate Example 1 5.60 0.165 No pitting, no cratering Example 2 5.12 0.214 No pitting, no cratering Example 3 4.95 0.272 No pitting, no cratering Example 4 5.38 0.107 No pitting, no cratering Comparative Example 1 5.25 0.465 There is pitting corrosion, but no pitting corrosion Comparative Example 2 5.06 0.678 Pitting corrosion Comparative Example 3 4.88 0.997 Pitting corrosion
[0067] Although the embodiments of the present application have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present application, and that the scope of the present application is defined by the appended claims and their equivalents.
Claims
1. A stripping solution for nickel-plated automobile parts with copper alloy as the substrate, characterized in that: Each liter of the deplating solution is composed of the following components: 100-200 mL of sulfuric acid, 5-10 mL of hydrochloric acid, 50-80 g of citric acid, 15-30 g of thiourea, and 0.2-0.4 g of a benzotriazole derivative, and the solvent is water; the preparation method of the benzotriazole derivative is as follows: S1. Under stirring conditions, disperse benzotriazole in 2-methyltetrahydrofuran, add methylthiopropylene oxide and N,N-dimethylcyclohexylamine in sequence after complete dissolution, react at 80-100°C for 4-8h, cool to room temperature, filter, take the filtrate, distill under reduced pressure, and dry to obtain an intermediate; S2. Disperse the intermediate obtained in step S1 and acrylic acid in toluene under stirring, add p-toluenesulfonic acid, react at 70-90° C. for 5-9 hours, add deionized water and sodium bicarbonate in sequence after cooling, continue to react for 0.5-1.5 hours, filter, take the filtrate, extract, distill under reduced pressure, and dry to obtain a benzotriazole derivative; The structural formula of the benzotriazole derivative is:
2. The stripping solution for nickel-plated automobile parts with copper alloy as the substrate according to claim 1, characterized in that: The molar ratio of benzotriazole, methylthiopropylene oxide and N,N-dimethylcyclohexylamine in step S1 is 1:0.7-0.9:0.03-0.
05.
3. The deplating solution for nickel-plated automobile parts with copper alloy as the substrate according to claim 1, characterized in that: The added amount of benzotriazole in the 2-methyltetrahydrofuran is 0.1-0.3 g / mL.
4. The deplating solution for nickel-plated automobile parts with copper alloy as the substrate according to claim 1, characterized in that: In step S2, the molar ratio of the intermediate, acrylic acid and p-toluenesulfonic acid is 1.2:0.8-1.0:0.04-0.07, and the mass ratio of p-toluenesulfonic acid, deionized water and sodium bicarbonate is 4-8:25-35:3-7.
5. The deplating solution for nickel-plated automobile parts with copper alloy as the substrate according to claim 1, characterized in that: The amount of acrylic acid added to the toluene is 0.15-0.25 g / mL.
6. The stripping solution for nickel-plated automobile parts with copper alloy as the substrate according to claim 1, characterized in that: The mass fraction of the hydrochloric acid is 37-38%.
7. A method for preparing a deplating solution for nickel-plated automobile parts with a copper alloy as a substrate according to any one of claims 1 to 6, characterized in that: The following steps are involved: (1) Weigh out the formulated amounts of sulfuric acid, hydrochloric acid, citric acid, thiourea, benzotriazole derivatives, and water and set aside; (2) dissolving the sulfuric acid, hydrochloric acid and citric acid weighed in step (1) in part of the water weighed in step (1), stirring and mixing to obtain a mixed solution 1; (3) Add the thiourea and benzotriazole derivatives weighed in step (1) to the mixed solution 1 obtained in step (2) in sequence, stir until completely dissolved, and make up to volume with the remaining amount of water to obtain the product.
8. The method for preparing a deplating solution for nickel-plated automobile parts with a copper alloy as a substrate according to claim 7, characterized in that: The part of water in step (2) accounts for 1 / 2-2 / 3 of the total mass of water.
Citation Information
Patent Citations
Stripping solution for chemical nickel-plated coating of cast aluminum piece
CN103160832A
High-efficiency environment-friendly nickel stripper and preparation method thereof
CN103409755A