Nickel iron molybdate oxygen evolution catalytic electrode and preparation method thereof

By loading nickel-iron mixed molybdate onto a nickel foam substrate and spraying it with FAA-3 ionomer, a nano-flower-shaped catalytic electrode with high specific surface area was prepared, which solved the problem of insufficient activity and stability of existing catalysts and achieved low-cost and high-efficiency water electrolysis catalysis.

CN118895532APending Publication Date: 2024-11-05XI AN JIAOTONG UNIV
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202411145842.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

In existing anion exchange membrane water electrolysis systems, low-cost non-precious metal catalysts have insufficient oxygen evolution activity and poor stability, and the preparation process is complex, resulting in high electrolyzer costs and limiting their application in energy production.

Method used

A high specific surface area nickel-iron-molybdate oxygen evolution catalytic electrode was prepared by loading a specific proportion of nickel-iron molybdate mixture onto a nickel foam substrate using a hydrothermal method, forming a nanoflower-like structure by controlling the hydrothermal reaction parameters, and then spraying FAA-3 ionomer onto the electrode surface.

Benefits of technology

A low-cost, highly active, and stable oxygen evolution catalytic electrode has been developed, which is suitable for anion exchange membrane electrolyzers, reducing the cost of the electrolyzer and improving energy conversion efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118895532A_ABST
    Figure CN118895532A_ABST
Patent Text Reader

Abstract

The invention discloses a nickel iron molybdate oxygen evolution catalytic electrode and a preparation method thereof.The preparation method comprises the following steps that the surface of a foamed nickel sheet is cleaned and dried, and a clean oil-free foamed nickel sheet is obtained; dissolving nickel nitrate, ferric nitrate and ammonium heptamolybdate in deionized water to obtain dispersion liquid; transferring the dispersion liquid into a hydrothermal kettle, putting a foamed nickel sheet into the hydrothermal kettle, carrying out hydrothermal treatment in a drying oven, naturally cooling, washing and drying to obtain foamed nickel loaded with nickel molybdate and iron molybdate catalysts; and preparing an ionomer solution, spraying the ionomer solution onto the electrode precursor, and drying to obtain the oxygen evolution catalytic electrode. The invention provides a preparation scheme of the anion exchange membrane water electrolysis oxygen evolution catalytic electrode which is simple in preparation method, low in synthesis cost, non-toxic and harmless, and the catalyst in the electrode has a microstructure different from that of a common molybdate catalyst and has high electrochemical catalytic activity. The electrolytic bath based on the catalytic electrode can efficiently electrolyze dilute alkali liquor to produce hydrogen, and the energy consumption and the safety of the electrolytic bath are superior to those of a traditional alkaline water electrolysis system.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of energy chemistry, and in particular to a nickel-iron-molybdate oxygen evolution catalytic electrode and a preparation method thereof. Background Art

[0002] With economic development, the problem of ecological environment deterioration caused by the large-scale use of fossil fuels has become increasingly prominent. Using solar and wind power to generate electricity to electrolyze water to produce hydrogen is a promising way to produce clean energy. Among them, anion exchange membrane water electrolysis technology is expected to become the key to reducing the cost of green hydrogen production due to its high system energy conversion efficiency and low cost. However, at this stage, such water electrolysis systems usually use precious metal oxides such as ruthenium and iridium as oxygen evolution catalysts. The lack of low-cost catalysts makes the cost of electrolyzers high, limiting their application in energy production.

[0003] A feasible solution to reduce the manufacturing cost of electrolyzers is to use low-cost transition metals such as cobalt and nickel to prepare catalysts. Currently, non-precious metal catalysts represented by nickel-iron layered double hydroxides are developing rapidly. The oxygen evolution activity of some catalysts is comparable to that of precious metal-based materials, but their stability is generally insufficient and the preparation process is mostly complicated. The stability of the molybdate structure is conducive to improving the catalyst's tolerance to long-term electrolysis. As a low-cost non-metallic material with stable chemical properties, molybdate is currently mostly used in the field of energy storage and is less used in water electrolysis catalysts. The microscopic morphology of molybdate prepared by existing methods is often rod-shaped or linear, and the specific surface area is relatively low. Summary of the invention

[0004] The purpose of the present invention is to provide a nickel-iron-molybdate oxygen evolution catalytic electrode and a preparation method thereof, which can be used for anion exchange membrane water electrolysis to obtain an oxygen evolution catalytic electrode with a simple synthesis method, low cost, high activity and stability. The electrode can be used in anion exchange membrane electrolyzers for efficient electrocatalytic water decomposition.

[0005] To achieve the above object, the present invention provides a method for preparing a nickel-iron-molybdate oxygen evolution catalytic electrode, which comprises:

[0006] The nickel foam sheet is cleaned to obtain a clean and oil-free nickel foam sheet;

[0007] Dissolve nickel nitrate, iron nitrate and ammonium heptamolybdate in deionized water, stir and ultrasonically treat to make them dispersed evenly, to obtain a dispersion;

[0008] Adding clean, oil-free nickel foam sheets into the dispersion to carry out a hydrothermal reaction, and after naturally cooling to room temperature, taking out the obtained nickel foam sheets with molybdate attached, washing and drying them to obtain an electrode precursor;

[0009] Mix isopropanol and deionized water, add a crosslinking agent to the mixture, and perform ultrasonic dispersion to obtain an ionomer solution;

[0010] The ionomer solution is sprayed onto the electrode precursor, and dried to obtain a nickel-iron-molybdate oxygen evolution catalytic electrode for anion exchange membrane water electrolysis.

[0011] As a further improvement of the present invention, the nickel foam sheet is cleaned to obtain a clean oil-free nickel foam sheet, which specifically includes:

[0012] The nickel foam sheet was placed in a hydrochloric acid solution, and the surface was cleaned by ultrasonic treatment at room temperature. Then, the residual solution was washed away with deionized water and ethanol in sequence and dried to obtain a clean and oil-free nickel foam sheet.

[0013] As a further improvement of the present invention, the thickness of the nickel foam sheet is 0.5-1.5 mm; the concentration of the hydrochloric acid used is 2-4 mol·L -1 The specific steps for washing away the residual solution are: rinse with deionized water several times, and then rinse with anhydrous ethanol several times.

[0014] As a further improvement of the present invention, the amounts of nickel nitrate, iron nitrate and ammonium heptamolybdate are such that the atomic ratio of nickel, iron and molybdenum in the dispersion is 3:2:6.

[0015] As a further improvement of the present invention, clean and oil-free nickel foam sheets are added to the dispersion to satisfy the following requirement: the amount of solution corresponding to each square centimeter of nickel foam is 3.5-4.0 mL.

[0016] As a further improvement of the present invention, the hydrothermal reaction conditions are: keeping warm at 150-170° C. for 5-7 hours.

[0017] As a further improvement of the present invention, isopropanol and deionized water are mixed in a volume ratio of 1:1; a cross-linking agent is added to the mixed solution, such that 90 μL of 10% FAA-3 cross-linking agent is added to every 1 mL of the mixed solution.

[0018] As a further improvement of the present invention, the spraying temperature is 80-100° C.; and the spraying amount of the ionomer solution is 250 μL per square centimeter of electrode precursor.

[0019] As a further improvement of the present invention, the ultrasonic dispersion time is 20 to 40 minutes, and the temperature during ultrasound does not exceed 50°C.

[0020] The present invention also provides a nickel-iron-molybdate oxygen evolution catalytic electrode, which is prepared by the method for preparing a nickel-iron-molybdate oxygen evolution catalytic electrode. The prepared electrode is a porous composite electrode with a nickel foam as a substrate, nickel-iron mixed molybdate nanoflowers with a particle size of less than 10 μm uniformly attached to the surface and covered with FAA-3 ionomer.

[0021] As a further improvement of the present invention, the concentration of hydrochloric acid is 2 to 4 mol·L -1 .

[0022] As a further improvement of the present invention, the specific steps of washing away the residual solution are: rinsing with deionized water for 3 times, and then rinsing with anhydrous ethanol for 3 times.

[0023] As a further improvement of the present invention, the recommended amounts of nickel nitrate, iron nitrate and ammonium heptamolybdate dissolved in 50 mL of deionized water are 1.25 mmol, 0.84 mmol and 0.36 mmol respectively, so that the atomic ratio of nickel, iron and molybdenum in the dispersion is 3:2:6, wherein the concentration of molybdate and its ratio relative to nitrate should not be higher than this value.

[0024] Compared with the prior art, the present invention has the following advantages:

[0025] The present invention uses a hydrothermal method to load a specific proportion of nickel and iron mixed molybdate on the surface of nickel foam. By controlling the hydrothermal reaction parameters, the catalyst grown on the nickel foam substrate has a nano-flower-like microscopic morphology, and its high specific surface area is conducive to the electrochemical reaction. Compared with the existing molybdate catalyst preparation method, the present invention mainly controls the morphology by adjusting the elements in the finished catalyst, without the need for additional additives and buffers. By spraying ionomers on the electrode surface, the mass transfer of the catalytic electrode in the membrane electrolysis system is further improved. The present invention constructs a high-activity oxygen evolution electrode based on a specific transition metal composition and morphology suitable for anion exchange membrane water electrolysis. Compared with the traditional water electrolysis anode, the catalytic electrode is simple to prepare, low in cost, and excellent in activity, and is suitable for large-scale anion exchange membrane water electrolysis system. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 The invention discloses a method for preparing a nickel-iron-molybdate oxygen evolution catalytic electrode.

[0027] Figure 2 a, Figure 2 c is a low-magnification scanning electron microscope image of the nickel-iron mixed molybdate catalytic electrode precursor prepared by the present invention when the ionomer is not sprayed; Figure 2 b are high magnification scanning electron microscope images of the nickel-iron mixed molybdate catalytic electrode prepared by the present invention; Figure 2 d are the element distribution diagrams corresponding to oxygen, molybdenum, nickel and iron in the area of ​​Figure c.

[0028] Figure 3 The X-ray diffraction image of the unsprayed ionomer electrode precursor obtained in the present invention;

[0029] Figure 4 a is a wide spectrum X-ray photoelectron spectroscopy image of an unsprayed ionomer electrode precursor obtained in the present invention; Figure 4b, Figure 4 c, Figure 4 d is a high-resolution X-ray photoelectron spectroscopy image of Ni 2p, Mo 2d and Fe2p of the unsprayed ionomer electrode precursor obtained in the present invention.

[0030] Figure 5 The nickel-iron mixed molybdate catalytic electrode and pure nickel foam obtained by the present invention are heated to 25°C and 1 mol·L -1 Linear voltammetric scan curve obtained in a three-electrode system with potassium hydroxide solution as the electrolyte.

[0031] Figure 6 The nickel-iron mixed molybdate catalytic electrode obtained by the present invention is 25°C, 1 mol·L -1 Tafel curve measured in a three-electrode system with potassium hydroxide solution as the electrolyte.

[0032] Figure 7 The nickel-iron mixed molybdate catalytic electrode obtained by the present invention is 25°C, 1 mol·L -1 Potassium hydroxide solution was used as the electrolyte, and the electrolysis current density was 250 mA cm -2 Stability test results of continuous electrolysis under different conditions.

[0033] Figure 8 The anion exchange membrane electrolytic cell assembled using the nickel-iron mixed molybdate catalytic electrode obtained by the present invention is heated to 50°C and 1 mol·L -1 Linear voltammetric scanning curve obtained under the condition of potassium hydroxide solution as electrolyte. The control group used unloaded nickel foam instead of catalytic electrode.

[0034] Fig. 9 This is a schematic diagram of the structure and working principle of an anion exchange membrane electrolytic cell assembled from the nickel-iron mixed molybdate catalytic electrode obtained by the present invention. DETAILED DESCRIPTION

[0035] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the accompanying drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the accompanying drawings in the following description are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.

[0036] By controlling the preparation conditions and composition of molybdate, a morphology with a higher specific surface area can be obtained, which is conducive to the electrochemical reaction. On this basis, selecting suitable transition metal atoms as active catalytic sites can further improve the catalyst activity. Applying such catalysts to anion exchange membrane electrolyzers can improve the energy conversion efficiency of the electrolysis system, improve its stability and reduce costs.

[0037] The present invention uses nickel-iron mixed molybdate as anion exchange membrane water electrolysis anode catalyst, and prepares a catalytic electrode with a nano-flower-like morphology on a nickel foam substrate. The catalytic electrode is low in cost, simple to prepare, has good catalytic activity and stability, and can obtain a nano-flower-like morphology without special additives compared to other molybdate catalyst preparation processes, and is suitable for anion exchange membrane electrolyzers.

[0038] Combination Figure 1 The present invention provides a method for preparing a nickel-iron-molybdate oxygen evolution catalytic electrode, comprising the following steps:

[0039] S1. The nickel foam sheet is placed in a hydrochloric acid solution, the surface is cleaned by ultrasonic treatment at room temperature, and then the residual solution is washed away with deionized water and ethanol and dried to obtain a clean oil-free nickel foam sheet A;

[0040] Optionally, in step S1, the concentration of hydrochloric acid is 2 to 4 mol·L -1 The specific concentration can be selected as needed, for example, 2 mol·L -1 , 2.5 mol·L -1 , 3 mol·L -1 , 3.5 mol·L -1 , 4 mol·L -1 ,wait.

[0041] Further optionally, in step S1, the nickel foam sheet used has a thickness of 0.5-1.5 mm. The specific thickness can be selected as needed, for example, 0.5 mm, 0.8 mm, 1.0 mm, 1.2 mm, 1.3 mm, 1.5 mm, etc.

[0042] Optionally, in step S1, ultrasonic treatment is performed at room temperature for 25 to 40 minutes to wash away the residual solution. The specific steps are: rinsing with deionized water for multiple times, and then rinsing with anhydrous ethanol for multiple times, for example, three times. Drying in an oven at 55 to 70° C. for 1.5 to 3 hours.

[0043] S2. nickel nitrate, iron nitrate and ammonium heptamolybdate were dissolved in deionized water and uniformly dispersed by ultrasonic treatment at room temperature to obtain a dispersion B;

[0044] Optionally, in step S2, the ultrasonic time is 5 to 15 minutes. The appropriate ultrasonic time is selected according to the dispersion conditions, for example, 5 minutes, 7 minutes, 9 minutes, 10 minutes, 12 minutes, 15 minutes, etc.

[0045] Further optionally, in step S2, the recommended amounts of nickel nitrate, iron nitrate and ammonium heptamolybdate dissolved in every 50 mL of deionized water are 1.25 mmol, 0.84 mmol and 0.36 mmol respectively, so that the atomic ratio of nickel, iron and molybdenum in the dispersion is 3:2:6, wherein the concentration of molybdate and its ratio to nitrate should not be higher than this value.

[0046] Among them, ultrasonic treatment can effectively break up the agglomeration between solute particles and make them more evenly dispersed in the solvent. This uniform dispersion not only improves the solubility and stability of the solute, but also facilitates the reaction or interaction between the solute and other substances in the subsequent steps.

[0047] By accurately calculating and adding the amounts of nickel nitrate, iron nitrate and ammonium heptamolybdate, the ratio of nickel, iron and molybdenum atoms in the dispersion can be ensured to be 3:2:6. This precise ratio control is crucial for preparing composite materials or catalysts with specific composition and properties.

[0048] The amount of solute dissolved in every 50 mL of deionized water is controlled within a certain range, which helps to avoid precipitation or crystallization caused by excessive solute concentration, while ensuring effective dispersion of the solute in the solvent. In addition, limiting the concentration of molybdate and its relative ratio to nitrate can prevent side reactions or adverse effects caused by excessive concentration. A uniformly dispersed solute system is conducive to the subsequent chemical reactions. In the process of preparing composite materials or catalysts, sufficient contact and reaction between solutes are key factors in improving product quality and performance.

[0049] S3. Transfer the dispersion B obtained in S2 to a hydrothermal reactor, add the nickel foam sheet A obtained in S1, close the hydrothermal reactor, and keep it in an oven at 150-170°C for 5-7h. After cooling naturally to room temperature, take out the obtained nickel foam sheet with molybdate, wash and dry it to obtain an electrode precursor C. The obtained electrode precursor C is a nickel foam loaded with nickel molybdate and iron molybdate catalysts;

[0050] Optionally, in step S3, the amount of solution corresponding to each square centimeter of nickel foam is 3.5-4.0 mL. The hydrothermal reaction conditions are: keeping warm at 150-170°C for 5-7 hours. Preferably, keeping warm at 160°C for 6 hours. Drying: drying in an oven at 60-80°C for 6-12 hours.

[0051] S4. Mix isopropanol and deionized water in a volume ratio of 1:1, add 10% FAA-3 membrane solution to the mixture, and fully disperse it by ultrasonication at room temperature to obtain ionomer solution D.

[0052] Optionally, in step S4, 90 μL of 10% FAA-3 membrane solution is added to every 1 mL of the mixed solution. The specific amount can be adjusted in proportion according to the actual amount.

[0053] Further optionally, in step S4, the ultrasonic time is 20 to 40 minutes, and the temperature during ultrasonication does not exceed 50° C. The appropriate ultrasonic time is selected according to the dispersion conditions, for example, 20 minutes, 25 minutes, 30 minutes, 35 minutes, 36 minutes, 40 minutes, etc.

[0054] S5. Spray the ionomer solution D obtained in S4 onto the electrode precursor C obtained in S3 at 80-100° C., then place the electrode into a vacuum oven and dry it at 70-90° C. for 10-14 h to obtain a non-precious metal catalytic electrode.

[0055] Optionally, in step S5, the spraying amount of the ionomer solution is 250 μL per square centimeter of the electrode precursor.

[0056] Further optionally, the spraying temperature is 80-100°C, preferably 90°C.

[0057] The present invention provides a method for preparing an anion exchange membrane water electrolysis oxygen evolution catalytic electrode with simple preparation method, low synthesis cost, non-toxic and harmless, and the catalyst in the electrode has a microstructure different from that of the common molybdate catalyst and has high electrochemical catalytic activity. The electrolyzer based on the catalytic electrode can efficiently electrolyze dilute alkali solution to produce hydrogen, and its energy consumption and safety are better than those of the traditional alkaline water electrolysis system. The advantages of each step are as follows:

[0058] Among them, S1. Cleaning and preparation of nickel foam sheets; cleaning the nickel foam sheets to remove oil stains, oxides and other impurities on the surface to ensure that the subsequent catalyst can be firmly attached to the nickel foam.

[0059] Using hydrochloric acid solution and ultrasonic treatment can more effectively remove stubborn stains.

[0060] Rinsing with deionized water and then ethanol ensures that residues are completely removed, while the volatility of ethanol facilitates rapid drying. The drying process prevents moisture from remaining, further ensuring surface cleanliness.

[0061] S2. Preparation of dispersion: Nickel nitrate, iron nitrate and ammonium heptamolybdate are dissolved in deionized water and dispersed uniformly by ultrasonic treatment to form a catalyst precursor solution. Ultrasonic treatment promotes uniform dispersion of solutes, avoids precipitation or agglomeration, and improves the uniformity and activity of the catalyst. The concentration and ratio of the solutes are precisely controlled to ensure the accuracy and consistency of the catalyst components.

[0062] S3. Hydrothermal reaction and formation of electrode precursor: Under hydrothermal conditions, the nickel foam sheet reacts with the metal salt in the dispersion to form a nickel foam electrode precursor loaded with nickel molybdate and iron molybdate catalysts. The hydrothermal reaction provides a high temperature and high pressure environment, which is conducive to the uniform deposition and crystallization of the catalyst on the surface of the nickel foam. By controlling the hydrothermal temperature and time, the crystal structure and morphology of the catalyst can be precisely controlled, thereby affecting its catalytic performance.

[0063] S4. Preparation of ionomer solution: Mix isopropanol, deionized water and FAA-3 membrane solution to form an ionomer solution with bonding and conductive properties, which is used to fix the catalyst on the electrode. As a binder, the FAA-3 membrane solution can enhance the bonding force between the catalyst and the nickel foam and prevent the catalyst from falling off. The mixed solvent of isopropanol and deionized water helps to evenly disperse the FAA-3 membrane solution and improve the coating effect.

[0064] S5. Spraying and drying: Spray the ionomer solution onto the electrode precursor and dry it in a vacuum oven to form the final catalytic electrode. The spraying method can ensure uniform coverage of the ionomer solution on the electrode surface, improving the uniformity and consistency of the catalytic electrode. The low-temperature drying process in the vacuum oven avoids the damage to the catalyst structure and performance by high temperature, while ensuring the complete curing of the ionomer. The performance of the catalytic electrode can be further optimized by controlling the spraying amount and drying conditions.

[0065] In order to make the purpose, technical solutions and advantages of the present invention more clear, the specific implementation of the present invention is further described below in conjunction with the accompanying drawings and embodiments, which are intended to explain the present invention rather than limit it.

[0066] Example 1

[0067] The method for preparing a nickel-iron-molybdate oxygen evolution catalytic electrode for anion exchange membrane water electrolysis of the present invention comprises the following steps:

[0068] S1. Take 3×4.5cm 1.5mm thick nickel foam sheets and place them in a beaker. Add 3mol·L -1 The nickel foam sheet A was completely immersed in a hydrochloric acid solution, ultrasonically treated at room temperature for 30 min, then rinsed with deionized water and anhydrous ethanol three times to remove the residual solution, and dried in an oven at 60 ° C for 2 h to obtain a clean oil-free nickel foam sheet A;

[0069] S2. 1.25mmol nickel nitrate, 0.84mmol iron nitrate, and 0.36mmol ammonium heptamolybdate were dissolved in 50ml of deionized water and ultrasonically treated at room temperature for 10min to disperse them uniformly to obtain dispersion B;

[0070] S3. The dispersion B obtained in S2 was transferred to a 100 ml hydrothermal reactor, and the nickel foam sheet A obtained in S1 was added. The hydrothermal reactor was closed and heated in an oven at 160°C for 6 h. After naturally cooling to room temperature, the obtained nickel foam sheet with molybdate was taken out and gently rinsed with deionized water, and dried in an oven at 80°C for 6 h to obtain an electrode precursor C.

[0071] S4. Take 0.5 ml of isopropanol and deionized water and mix them evenly, add 90 μL of 10% FAA-3 membrane solution to the mixture, and ultrasonically disperse it at room temperature for 30 minutes to obtain ionomer solution D;

[0072] S5. Cut a 2×2 cm piece of electrode precursor C obtained in S3 with uniform adhesion, and evenly spray the ionomer solution D prepared in S4 onto the cut electrode precursor on an adsorption heating table at 90°C. Then put it into a vacuum oven and dry it at 80°C for 12 hours to obtain a non-precious metal catalytic electrode.

[0073] Example 2

[0074] The method for preparing a nickel-iron-molybdate oxygen evolution catalytic electrode for anion exchange membrane water electrolysis of the present invention comprises the following steps:

[0075] S1. Take 3×4.5cm 0.5mm thick nickel foam sheets and place them in a beaker. Add 3mol·L -1 The nickel foam sheet A was completely immersed in a hydrochloric acid solution and ultrasonically treated at room temperature for 30 min, and then rinsed with deionized water and anhydrous ethanol for 3 times to remove the residual solution, and a clean, oil-free nickel foam sheet A was obtained and stored in anhydrous ethanol and fully air-dried with hot air before further use;

[0076] S2. 1.25mmol nickel nitrate, 0.84mmol iron nitrate, and 0.36mmol ammonium heptamolybdate were dissolved in 50ml of deionized water and ultrasonically treated at room temperature for 10min to disperse them uniformly to obtain dispersion B;

[0077] S3. The dispersion B obtained in S2 was transferred to a 100 ml hydrothermal reactor, and the nickel foam sheet A obtained in S1 was added. The hydrothermal reactor was closed and heated in an oven at 160°C for 6 h. After cooling naturally to room temperature, the obtained nickel foam sheet with molybdate was taken out and gently rinsed with deionized water, and dried in an oven at 60°C for 12 h to obtain an electrode precursor C.

[0078] S4. Take 0.5 ml of isopropanol and deionized water and mix them evenly, add 90 μL of 10% FAA-3 membrane solution to the mixture, and ultrasonically disperse it at room temperature for 30 minutes to obtain ionomer solution D;

[0079] S5. Cut a 2×2 cm piece of electrode precursor C obtained in S3 with uniform adhesion, and evenly spray the ionomer solution D prepared in S4 onto the cut electrode precursor on an adsorption heating table at 90°C. Then put it into a vacuum oven and dry it at 80°C for 18 hours to obtain a non-precious metal catalytic electrode.

[0080] Example 3

[0081] The method for preparing a nickel-iron-molybdate oxygen evolution catalytic electrode for anion exchange membrane water electrolysis of the present invention comprises the following steps:

[0082] S1. Take a 1.5 mm thick nickel foam sheet of 3×3 cm in size and place it in a beaker. Add 3 mol·L -1 The nickel foam sheet A was completely immersed in a hydrochloric acid solution, ultrasonically treated at room temperature for 30 min, then rinsed with deionized water and anhydrous ethanol three times to remove the residual solution, and dried in an oven at 60 ° C for 2 h to obtain a clean oil-free nickel foam sheet A;

[0083] S2. 1.25mmol nickel nitrate, 0.84mmol iron nitrate, and 0.36mmol ammonium heptamolybdate were dissolved in 50ml of deionized water and ultrasonically treated at room temperature for 10min to disperse them uniformly to obtain dispersion B;

[0084] S3. Take 35 ml of the dispersion B obtained in S2 and transfer it to a 100 ml hydrothermal kettle, put in the nickel foam sheet A obtained in S1, close the hydrothermal kettle, and heat it in an oven at 160°C for 6 hours. After cooling naturally to room temperature, take out the obtained nickel foam sheet with molybdate and rinse it with deionized water, and dry it in an oven at 80°C for 6 hours to obtain an electrode precursor C;

[0085] S4. Take 1 ml of isopropanol and deionized water and mix them evenly, add 200 μL of 10% FAA-3 membrane solution to the mixture, and ultrasonically disperse it at room temperature for 30 minutes to obtain ionomer solution D;

[0086] S5. On an adsorption heating table at 90°C, take the ionomer solution D prepared in S4 and evenly spray it onto the electrode precursor obtained in S3, then send it into a vacuum oven and dry it at 80°C for 12 hours to obtain a non-precious metal catalytic electrode.

[0087] Example 4

[0088] The method for preparing a nickel-iron-molybdate oxygen evolution catalytic electrode for anion exchange membrane water electrolysis of the present invention comprises the following steps:

[0089] S1. Take 3×4.5cm 1.5mm thick nickel foam sheets and place them in a beaker. Add 3mol·L -1The nickel foam sheet A was completely immersed in a hydrochloric acid solution, ultrasonically treated at room temperature for 30 min, then rinsed with deionized water and anhydrous ethanol three times to remove the residual solution, and dried in an oven at 60 ° C for 2 h to obtain a clean oil-free nickel foam sheet A;

[0090] S2. 1.25mmol nickel nitrate, 0.84mmol iron nitrate, and 0.36mmol ammonium heptamolybdate were dissolved in 50ml of deionized water and ultrasonically treated at room temperature for 10min to disperse them uniformly to obtain dispersion B;

[0091] S3. The dispersion B obtained in S2 was transferred to a 100 ml hydrothermal reactor, and the nickel foam sheet A obtained in S1 was added. The hydrothermal reactor was closed and heated in an oven at 160°C for 6 h. After cooling naturally to room temperature, the obtained nickel foam sheet with molybdate was taken out and rinsed with deionized water, and dried in an oven at 80°C for 6 h to obtain an electrode precursor C.

[0092] S4. Take 0.5 ml of isopropanol and deionized water and mix them evenly, add 90 μL of 10% FAA-3 membrane solution to the mixture, and ultrasonically disperse it at room temperature for 30 minutes to obtain ionomer solution D;

[0093] S5. Cut a 2×2 cm piece of electrode precursor C obtained in S3 with uniform adhesion, spray half of the ionomer solution D prepared in S4 evenly onto the cut electrode precursor on a 90°C adsorption heating table, and then put it into a vacuum oven and dry it at 80°C for 12h to obtain a non-precious metal catalytic electrode E;

[0094] S6. In order to protect the anion exchange membrane from being punctured, the catalytic electrode E was flattened using a pressure of about 1 MPa, and then the remaining half of the ionomer solution was evenly sprayed onto the electrode on an adsorption heating table at 90°C. The electrode was then placed in a vacuum oven and dried at 80°C for 12 hours to obtain a flattened non-precious metal catalytic electrode with a thickness of about 0.15 mm.

[0095] Example 5

[0096] The method for preparing a nickel-iron-molybdate oxygen evolution catalytic electrode for anion exchange membrane water electrolysis of the present invention comprises the following steps:

[0097] S1. Take 3×4.5cm 1.5mm thick nickel foam sheets and place them in a beaker. Add 3mol·L -1 The nickel foam sheet A was completely immersed in a hydrochloric acid solution, ultrasonically treated at room temperature for 30 min, then rinsed with deionized water and anhydrous ethanol three times to remove the residual solution, and dried in an oven at 60 ° C for 2 h to obtain a clean oil-free nickel foam sheet A;

[0098] S2. 1.25mmol nickel nitrate, 0.84mmol iron nitrate, and 0.35mmol ammonium heptamolybdate were dissolved in 50ml of deionized water and ultrasonically treated at room temperature for 10min to disperse them uniformly to obtain dispersion B;

[0099] S3. The dispersion B obtained in S2 was transferred to a 100 ml hydrothermal reactor, and the nickel foam sheet A obtained in S1 was added. The hydrothermal reactor was closed and heated in an oven at 160°C for 6 h. After cooling naturally to room temperature, the obtained nickel foam sheet with molybdate was taken out and gently rinsed with deionized water, and dried in an oven at 80°C for 6 h to obtain an electrode precursor C.

[0100] S4. Take 0.5 ml of ethanol and deionized water and mix them evenly, add 180 μL of FAA-3-EtOH-5 membrane solution to the mixture, and ultrasonically disperse it at room temperature for 30 minutes to obtain ionomer solution D;

[0101] S5. Cut a 2×2 cm piece of electrode precursor C obtained in S3 with uniform adhesion, and evenly spray the ionomer solution D prepared in S4 onto the cut electrode precursor on an adsorption heating table at 80°C. Then put it into a vacuum oven and dry it at 60°C for 18 hours to obtain a non-precious metal catalytic electrode.

[0102] Example 6

[0103] The method for preparing a nickel-iron-molybdate oxygen evolution catalytic electrode for anion exchange membrane water electrolysis of the present invention comprises the following steps:

[0104] S1. Take a 2×2cm nickel foam sheet with a thickness of 1.5mm and place it in a beaker. Add 3mol·L -1 The nickel foam sheet A was completely immersed in a hydrochloric acid solution, ultrasonically treated at room temperature for 30 min, then rinsed with deionized water and anhydrous ethanol three times to remove the residual solution, and dried in an oven at 60 ° C for 2 h to obtain a clean oil-free nickel foam sheet A;

[0105] S2. 0.66mmol nickel nitrate, 0.40mmol iron nitrate, and 0.34mmol ammonium heptamolybdate were dissolved in 50ml of deionized water and ultrasonically treated at room temperature for 10min to disperse them uniformly to obtain dispersion B;

[0106] S3. Transfer the dispersion B obtained in S2 to a 50 ml hydrothermal kettle, seal the hydrothermal kettle and keep it in an oven at 160°C for 6 hours. After cooling naturally to room temperature, separate the solid in the hydrothermal product using a centrifuge, ultrasonically disperse it in 30 mL of deionized water and centrifuge it again, repeat 3 times, dry it in a vacuum oven at 60°C for 12 hours, and gently crush it to obtain a powdered catalyst C;

[0107] S4. Take 0.5 ml of isopropanol and deionized water and mix them evenly. Add 30 μL of 10% FAA-3 membrane solution and 48 mg of powdered catalyst C to the mixture. Ultrasonic dispersion is performed at room temperature for 30 min to obtain catalyst ink D.

[0108] S5. On an adsorption heating table at 90°C, the catalyst ink D prepared in S4 is evenly sprayed onto the clean oil-free nickel foam sheet A obtained from S1, and then sent into a vacuum oven and dried at 80°C for 12 hours to obtain a non-precious metal catalytic electrode.

[0109] Figure 2 a, c are low-magnification scanning electron microscope images of the nickel-iron mixed molybdate catalytic electrode precursor obtained in Example 1 of the present invention when the ionomer is not sprayed; Figure 2 b are high magnification scanning electron microscope images of the nickel-iron mixed molybdate catalytic electrode prepared by the present invention; Figure 2 d is the corresponding Figure 2 Element distribution diagram of oxygen, molybdenum, nickel and iron in the c region. The microstructure of the nickel-iron mixed molybdate attached to the surface of the catalytic electrode precursor prepared by the present invention presents a nanoflower shape. The diameter of the nanoflower is 5-7μm, and the thickness of the layer is less than 300nm. This type of structure has a relatively large specific surface area, which is conducive to the escape of gas during electrolysis. And this structure is obviously different from the rod-shaped microstructure of other molybdate water-splitting catalysts widely reported, and its morphology is innovative. Figure 2 The element distribution diagrams of c and d show that the distribution of transition metal elements molybdenum, nickel and iron in the samples is relatively uniform. Based on the consistency of the catalyst morphology, it is inferred that the hydrothermally generated mixed nickel and iron molybdates are fully mixed during crystallization, which is conducive to the transfer of oxygen-containing adsorbed species on the nickel and iron sites.

[0110] Figure 3 The X-ray diffraction image of the unsprayed ionomer nickel-iron mixed molybdate catalytic electrode precursor obtained by the present invention. As can be seen from the figure, except for the diffraction peaks at 45°, 52°, and 77° introduced by the nickel foam pure nickel substrate, the diffraction peak distribution of the mixed molybdate catalytic electrode sample is similar to the combination of the main diffraction peaks in the diffraction images of the standard samples of nickel molybdate (PDF#45-0142) and iron molybdate (PDF#15-0290), proving the formation of nickel molybdate and iron molybdate on the surface of the catalytic electrode during the hydrothermal process. At the same time, the peak at 13.5° in the sample X-ray diffraction image can be regarded as the result of the peak at 13.06° in the iron molybdate standard sample shifting, indicating that the catalyst on the electrode surface has changed compared to the pure molybdate lattice parameter, corresponding to the solid solution formed by the two molybdates.

[0111] Figure 4 a is a wide spectrum X-ray photoelectron spectrum image of the unsprayed ionomer nickel-iron mixed molybdate catalytic electrode precursor obtained by the present invention; Figure 4b, c, d are high-resolution X-ray photoelectron spectroscopy images of Ni2p, Mo 2d and Fe 2p of the unsprayed ionomer electrode precursor prepared in the present invention. Figure 4 It can be seen from a that the catalyst mainly contains molybdenum, nickel, iron, oxygen, and carbon. Except for the carbon element which may come from the substrate used in the test, the presence of the other elements is consistent with the target composition of the catalytic electrode. For the fine spectra of each element, the binding energies corresponding to the centers of the characteristic peaks of the nickel element were measured to be 880.0, 874.1, 861.8, and 856.2 eV, respectively, corresponding to the nickel components in the 0-valent substrate nickel foam material and nickel molybdate. The peaks of the molybdenum element at 235.3 and 232.3 eV are consistent with the expectation that molybdenum in the catalyst exists in the form of molybdate. The iron signal is weak, indicating that the iron content in the catalyst may be low, which may be related to the hydrolysis of iron ions during the hydrothermal process and the reaction of iron ions with the nickel foam substrate during the hydrothermal process. The ratio of nickel to iron in the molybdate on the surface of the catalytic electrode may be different from the solution prepared in S2.

[0112] Figure 5 The nickel-iron mixed molybdate catalytic electrode and pure nickel foam obtained by the present invention are heated to 25°C and 1 mol·L -1 The linear voltammetric scanning curve obtained in the three-electrode system with potassium hydroxide solution as the electrolyte is obtained, and the curve adopts 90% iR compensation. Compared with the substrate material, the catalytic electrode prepared by the present invention can obtain a significantly higher current density than the control at the same potential, indicating that it has anode catalytic activity far superior to that of pure nickel electrode.

[0113] Figure 6 The nickel-iron mixed molybdate catalytic electrode obtained by the present invention is 25°C, 1 mol·L -1 The partial Tafel curve and its linear fitting results in the three-electrode system with potassium hydroxide solution as the electrolyte, with a current density of about 10 mA cm -2 The Tafel slope of the catalytic electrode prepared by the present invention under this condition is about 93mV·dec -1 , compared with the measured precious metal catalyst 80mV·dec -1 This shows that its catalytic effect in reaction kinetics is close to that of precious metals, and it has the potential to serve as a substitute for the current high-cost anode catalysts.

[0114] Figure 7 The nickel-iron mixed molybdate catalytic electrode obtained by the present invention is 25°C, 1 mol·L -1 Potassium hydroxide solution was used as the electrolyte, and the electrolysis current density was 250 mA cm -2The change of overpotential relative to the initial condition when electrolysis was continued for 12 hours under the condition of , that is, the stability test result. It can be seen that after 12 hours of continuous electrolysis, the catalyst overpotential rise does not exceed 4%, and the rising speed gradually slows down, and the catalyst has good stability.

[0115] Figure 8 The anion exchange membrane electrolytic cell assembled using the nickel-iron mixed molybdate catalytic electrode prepared by the present invention is heated to 50°C and 1 mol·L -1 The linear voltammetric scanning curve obtained under the working condition of potassium hydroxide solution as electrolyte. Under this typical working condition, the membrane water splitting system assembled with the catalytic electrode prepared by the present invention can obtain 200-480mA·cm at a cell voltage of 1.7-1.9V. -2 The current density is significantly better than that of non-catalytic electrode membrane water splitting system and alkaline water electrolysis system (the current density is less than 400mA·cm at 2V). -2 ). Compared with the existing alkaline water electrolysis system, the electrolyte used in the preparation of the electrode of the present invention is more diluted, the working temperature is lower, and the energy input required to obtain the same chemical is less, which has obvious advantages in energy consumption and safety.

[0116] Fig. 9 This is a schematic image of the structure and working principle of an anion exchange membrane electrolyzer assembled with the nickel-iron mixed molybdate catalytic electrode obtained by the present invention. Water diffuses through the porous transport layer on the cathode side to the cathode catalyst layer to react and generate hydrogen and hydroxide. Hydrogen diffuses into the cathode flow channel and is discharged; hydroxide migrates to the anode catalyst layer through the exchange membrane. A reaction occurs on the catalyst layer on the anode side to generate oxygen and water; the products finally diffuse into the flow channel on the anode side and are discharged. The catalytic electrode prepared by the present invention is the red frame part in the figure, which includes a porous nickel foam substrate (light gray) that plays a role in mass transfer and conduction as the anode side transport layer and an ionomer-coated mixed molybdate catalyst layer (light orange) on the electrode surface.

[0117] Example 7

[0118] The method for preparing a nickel-iron-molybdate oxygen evolution catalytic electrode for anion exchange membrane water electrolysis of the present invention comprises the following steps:

[0119] S1. Take 3×4.5cm 0.5mm thick nickel foam sheets and place them in a beaker. Add 2mol·L -1 The nickel foam sheet A was completely immersed in a hydrochloric acid solution, ultrasonically treated at room temperature for 28 min, then rinsed with deionized water and anhydrous ethanol 4 times to remove the residual solution, and dried in an oven at 55 ° C for 3 h to obtain a clean and oil-free nickel foam sheet A;

[0120] S2. 1.25mmol nickel nitrate, 0.84mmol iron nitrate, and 0.36mmol ammonium heptamolybdate were dissolved in 50ml of deionized water and ultrasonically treated at room temperature for 8min to disperse them uniformly to obtain dispersion B;

[0121] S3. Transfer the dispersion B obtained in S2 to a 100 ml hydrothermal kettle, and add the nickel foam sheet A obtained in S1. The amount of solution corresponding to each square centimeter of nickel foam is 4.0 mL. Close the hydrothermal kettle and heat it in an oven at 170°C for 5 hours. After cooling naturally to room temperature, take out the obtained nickel foam sheet with molybdate and gently rinse it with deionized water, and dry it in an oven at 70°C for 11 hours to obtain electrode precursor C;

[0122] S4. Take 0.5 ml of isopropanol and deionized water and mix them evenly, add 90 μL of 10% FAA-3 membrane solution to the mixture, and ultrasonically disperse it at room temperature for 20 minutes to obtain ionomer solution D;

[0123] S5. Cut a 2×2 cm piece of electrode precursor C obtained in S3 with uniform adhesion, and evenly spray the ionomer solution D prepared in S4 onto the cut electrode precursor on an adsorption heating table at 80°C. Then put it into a vacuum oven and dry it at 80°C for 10 hours to obtain a non-precious metal catalytic electrode.

[0124] Example 8

[0125] The method for preparing a nickel-iron-molybdate oxygen evolution catalytic electrode for anion exchange membrane water electrolysis of the present invention comprises the following steps:

[0126] S1. Take 3×4.5cm 0.8mm thick nickel foam sheets and put them in a beaker. Add 3.5mol·L -1 The nickel foam sheet A was completely immersed in a hydrochloric acid solution and ultrasonically treated at room temperature for 40 min, and then rinsed with deionized water and anhydrous ethanol twice to remove the residual solution, and a clean, oil-free nickel foam sheet A was stored in anhydrous ethanol and fully air-dried with hot air before further use;

[0127] S2. 1.25mmol nickel nitrate, 0.84mmol iron nitrate, and 0.36mmol ammonium heptamolybdate were dissolved in 50ml of deionized water and ultrasonically treated at room temperature for 15min to disperse them uniformly to obtain dispersion B;

[0128] S3. Transfer the dispersion B obtained in S2 to a 100 ml hydrothermal kettle, and add the nickel foam sheet A obtained in S1, with the solution volume corresponding to each square centimeter of nickel foam being 3.5 mL. Close the hydrothermal kettle and heat it in an oven at 70°C for 5.5 h. After cooling naturally to room temperature, take out the obtained nickel foam sheet with molybdate and gently rinse it with deionized water, and dry it in an oven at 70°C for 10 h to obtain electrode precursor C;

[0129] S4. Take 0.5 ml of isopropanol and deionized water and mix them evenly, add 90 μL of 10% FAA-3 membrane solution to the mixture, and ultrasonically disperse it at room temperature for 40 min to obtain ionomer solution D;

[0130] S5. Cut a 2×2 cm piece of electrode precursor C obtained in S3 with uniform adhesion, and evenly spray the ionomer solution D prepared in S4 onto the cut electrode precursor on an adsorption heating table at 95°C. Then put it into a vacuum oven and dry it at 85°C for 16 hours to obtain a non-precious metal catalytic electrode.

[0131] Example 9

[0132] The method for preparing a nickel-iron-molybdate oxygen evolution catalytic electrode for anion exchange membrane water electrolysis of the present invention comprises the following steps:

[0133] S1. Take a 1.0 mm thick nickel foam sheet of 3×3 cm in size and place it in a beaker. Add 4 mol·L -1 The nickel foam sheet A was completely immersed in a hydrochloric acid solution, ultrasonically treated at room temperature for 30 min, then rinsed with deionized water and anhydrous ethanol three times to remove the residual solution, and dried in an oven at 63 ° C for 2.5 h to obtain a clean and oil-free nickel foam sheet A;

[0134] S2. 1.25mmol nickel nitrate, 0.84mmol iron nitrate, and 0.36mmol ammonium heptamolybdate were dissolved in 50ml of deionized water and ultrasonically treated at room temperature for 9min to disperse them uniformly to obtain dispersion B;

[0135] S3. Take 35 ml of the dispersion B obtained in S2 and transfer it to a 100 ml hydrothermal kettle, and put in the nickel foam sheet A obtained in S1. The amount of solution corresponding to each square centimeter of nickel foam is 3.6 ml. The hydrothermal kettle is closed and heated in an oven at 155°C for 7 hours. After cooling naturally to room temperature, the obtained nickel foam sheet with molybdate is taken out and rinsed with deionized water, and dried in an oven at 78°C for 6.5 hours to obtain electrode precursor C;

[0136] S4. Take 1 ml of isopropanol and deionized water and mix them evenly. Add 200 μL of 10% FAA-3 membrane solution to the mixture and disperse them ultrasonically at room temperature for 26 min to obtain ionomer solution D.

[0137] S5. On an adsorption heating table at 88°C, take the ionomer solution D prepared in S4 and evenly spray it onto the electrode precursor obtained in S3, then send it into a vacuum oven and dry it at 88°C for 14 hours to obtain a non-precious metal catalytic electrode.

[0138] Example 10

[0139] The method for preparing a nickel-iron-molybdate oxygen evolution catalytic electrode for anion exchange membrane water electrolysis of the present invention comprises the following steps:

[0140] S1. Take 3×4.5cm 1.5mm thick nickel foam sheets and place them in a beaker. Add 3mol·L -1 The nickel foam sheet A was completely immersed in a hydrochloric acid solution, ultrasonically treated at room temperature for 25 min, then rinsed with deionized water and anhydrous ethanol three times each to remove the residual solution, and dried in an oven at 65 ° C for 1.5 h to obtain a clean oil-free nickel foam sheet A;

[0141] S2. 1.25mmol nickel nitrate, 0.84mmol iron nitrate, and 0.36mmol ammonium heptamolybdate were dissolved in 50ml of deionized water and ultrasonically treated at room temperature for 5min to disperse them uniformly to obtain dispersion B;

[0142] S3. Transfer the dispersion B obtained in S2 to a 100 ml hydrothermal kettle, and add the nickel foam sheet A obtained in S1, with the solution volume corresponding to each square centimeter of nickel foam being 3.7 mL. Close the hydrothermal kettle and heat it in an oven at 160°C for 7 hours. After cooling naturally to room temperature, take out the obtained nickel foam sheet with molybdate, rinse it with deionized water, and dry it in an oven at 80°C for 6.5 hours to obtain electrode precursor C;

[0143] S4. Take 0.5 ml of isopropanol and deionized water and mix them evenly, add 90 μL of 10% FAA-3 membrane solution to the mixture, and ultrasonically disperse it at room temperature for 32 minutes to obtain ionomer solution D;

[0144] S5. Cut a 2×2 cm piece of electrode precursor C obtained in S3 with uniform adhesion, spray half of the ionomer solution D prepared in S4 evenly onto the cut electrode precursor on an adsorption heating table at 92°C, and then send it into a vacuum oven and dry it at 82°C for 10 hours to obtain a non-precious metal catalytic electrode E.

[0145] Compared with the existing alkaline water electrolysis system, the non-precious metal catalytic electrodes prepared in Examples 7 to 9 use a more dilute electrolyte concentration, a lower operating temperature, and require less energy input to obtain the same chemicals, and have obvious advantages in energy consumption and safety. They can be used for anion exchange membrane water electrolysis.

[0146] The above is only an example of the present invention. Those skilled in the art may make various modifications or additions to the examples described, as long as they do not deviate from the spirit and essence of the present invention and are within the scope defined by the claims of the present invention.

[0147] Although the specific embodiments of the present invention are described above in conjunction with the accompanying drawings, the present invention is not limited to the above specific embodiments, which are merely illustrative, instructive, and not restrictive. Under the guidance of this specification, a person skilled in the art can make many forms without departing from the scope of protection of the claims of the present invention, all of which belong to the scope of protection of the present invention.

Claims

1. A method for preparing a nickel-iron-molybdate oxygen evolution catalytic electrode, characterized in that: include: The nickel foam sheet is cleaned to obtain a clean and oil-free nickel foam sheet; Dissolve nickel nitrate, iron nitrate and ammonium heptamolybdate in deionized water, stir and ultrasonically treat to make them dispersed evenly, to obtain a dispersion; Adding clean, oil-free nickel foam sheets into the dispersion to carry out a hydrothermal reaction, and after naturally cooling to room temperature, taking out the obtained nickel foam sheets with molybdate attached, washing and drying them to obtain an electrode precursor; Mix isopropanol and deionized water, add a crosslinking agent to the mixture, and perform ultrasonic dispersion to obtain an ionomer solution; The ionomer solution is sprayed onto the electrode precursor, and dried to obtain a nickel-iron-molybdate oxygen evolution catalytic electrode for anion exchange membrane water electrolysis.

2. The method for preparing the nickel-iron-molybdate oxygen evolution catalytic electrode according to claim 1, characterized in that: The nickel foam sheet is cleaned to obtain a clean oil-free nickel foam sheet, specifically comprising: The nickel foam sheet was placed in a hydrochloric acid solution, and the surface was cleaned by ultrasonic treatment at room temperature. Then, the residual solution was washed away with deionized water and ethanol in sequence and dried to obtain a clean and oil-free nickel foam sheet.

3. The method for preparing a nickel-iron-molybdate oxygen evolution catalytic electrode according to claim 2, characterized in that: The thickness of the nickel foam sheet is 0.5-1.5 mm; the concentration of hydrochloric acid used is 2-4 mol·L -1 The specific steps for washing away the residual solution are: rinse with deionized water several times, and then rinse with anhydrous ethanol several times.

4. The method for preparing a nickel-iron-molybdate oxygen evolution catalytic electrode according to claim 1, characterized in that: The amounts of nickel nitrate, iron nitrate and ammonium heptamolybdate are such that the atomic ratio of nickel, iron and molybdenum in the dispersion is 3:2:

6.

5. The method for preparing a nickel-iron-molybdate oxygen evolution catalytic electrode according to claim 1, characterized in that: Add clean, oil-free nickel foam sheets into the dispersion to satisfy the following requirement: the amount of solution corresponding to each square centimeter of nickel foam is 3.5-4.0 mL.

6. The method for preparing a nickel-iron-molybdate oxygen evolution catalytic electrode according to claim 1, characterized in that: The hydrothermal reaction conditions are: keeping warm at 150-170°C for 5-7h.

7. The method for preparing a nickel-iron-molybdate oxygen evolution catalytic electrode according to claim 1, characterized in that: Isopropanol and deionized water were mixed in a volume ratio of 1:1; a cross-linking agent was added to the mixture, such that 90 μL of 10% FAA-3 cross-linking agent was added to every 1 mL of the mixture.

8. The method for preparing a nickel-iron-molybdate oxygen evolution catalytic electrode according to claim 1, characterized in that: The spraying temperature is 80-100° C.; the spraying amount of the ionomer solution is 250 μL per square centimeter of electrode precursor.

9. The method for preparing a nickel-iron-molybdate oxygen evolution catalytic electrode according to claim 1, characterized in that: The ultrasonic dispersion time is 20 to 40 minutes, and the temperature during ultrasound does not exceed 50°C.

10. A nickel-iron-molybdate oxygen evolution catalytic electrode, characterized in that: The electrode is prepared by the method for preparing a nickel-iron-molybdate oxygen evolution catalytic electrode as described in any one of claims 1 to 9. The prepared electrode is a porous composite electrode with a nickel foam as a substrate, nickel-iron mixed molybdate nanoflowers with a particle size of less than 10 μm uniformly attached to the surface and covered with FAA-3 ionomer.

Citation Information

Cited By

  • Iron-doped molybdate nano composite material, preparation method thereof and method for oxygen evolution of alkaline salt through electro-catalysis of iron-doped molybdate nano composite material

    CN120026352A

  • Iron-nickel-molybdenum oxyhydroxide and preparation method and application thereof

    CN121627071A

  • Iron-nickel-molybdenum hydroxyl oxide, and preparation method and application thereof

    CN121627071B