Preparation method and application of zinc potassium hexacyanoferrate / carbon cloth composite electrode material
By preparing zinc ferricyanide potassium/carbon cloth composite electrode material, using its open frame structure and high selectivity, the problems of excessive use of chemical reagents and poor selectivity of carbon-based materials during cobalt recovery are solved, and the efficiency of cobalt ions is achieved Electrochemical adsorption and recycling improve recovery efficiency and stability of electrode materials.
Patent Information
- Application Number
- CN202410815089.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-24
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-06-24
AI Technical Summary
The prior art uses a large number of chemical reagents in the cobalt recycling process, which consumes high energy and discharges acid-containing wastewater and toxic gases, resulting in secondary pollution. In addition, traditional carbon-based materials have insufficient ion selectivity and removal rate, which limits the Its application in complex situations.
The zinc ferricyanide potassium/carbon cloth composite electrode material is prepared by electrochemical deposition and hydrothermal reaction, combined with constant current electrode deposition and constant temperature hydrothermal treatment, and prepared an open frame structure and highly selective electrode material for electrochemical recovery. Cobalt ions.
It realizes efficient electrochemical adsorption and selective separation of cobalt ions, and recovers important industrial raw materials such as lithium carbonate and cobalt hydroxide through chemical precipitation, which reduces material losses and improves the mechanical properties and cycle stability of the composite electrodes, achieving Fast and efficient recycling of cobalt elements in waste lithium cobalt oxide batteries.
Smart Images

Figure CN118895539A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of electrochemical technology, and in particular to a preparation method and application of a potassium zinc ferrocyanide / carbon cloth composite electrode material. Background Art
[0002] Since the first commercial use of lithium-ion batteries in the 1990s, the lithium battery industry has developed rapidly and gradually replaced other rechargeable batteries such as zinc-manganese batteries and lead-acid batteries, becoming the mainstream battery in today's new energy and portable electronic devices. It has excellent physical and chemical properties such as light weight, long cycle life, and high energy density per unit weight. Lithium cobalt oxide batteries are the most commonly used positive electrode materials for laptops, mobile phones, digital cameras, etc. However, with the increasingly shorter cycle of iterative upgrades of electronic products in the information age, a large number of obsolete electronic products have become electronic waste and have not been properly recycled. It is reported that by 2025, the total amount of electronic waste worldwide is expected to reach 65.3 million tons, including 464,000 tons of waste lithium battery waste. Considering the growing market demand for important industrial raw materials such as lithium, cobalt and nickel, as well as the human health problems caused by the pollution of waste lithium batteries, the recovery of high-value metals from waste lithium batteries is very important from both economic and environmental perspectives.
[0003] The recovery of cobalt from waste lithium batteries usually starts with a pretreatment process to obtain metal parts through physical separation, including mechanical, mechanochemical and thermal dissolution methods. Subsequently, traditional metal recovery technologies can be divided into two methods: physical calcination and chemical purification. Chemical purification treatments include acid leaching and chemical precipitation. Inorganic acids and organic acids are used together with reducing agents (such as hydrogen peroxide) to dissolve electrode material powders and leach metals, and then the metals are directly recovered by chemical precipitation. Physical calcination technology involves high-temperature treatment of melting and reduction of metal parts. However, these technologies use large amounts of chemical reagents, have high energy consumption, and also emit acidic wastewater and toxic gases, causing secondary pollution. Therefore, there is an urgent need to find an economical and environmentally friendly alternative method to recover cobalt.
[0004] Electrochemical adsorption, or capacitive deionization technology, is an advanced technology for removing salt ions from water that was first proposed in the 1990s. This technology replaces traditional ion separation technologies such as adsorption, chemical precipitation, ion exchange, and membrane separation. The target ions can be adsorbed when the electrode is charged, or they can be released from the electrode material into the bulk solution by short circuit or voltage reversal treatment. With the rapid development of capacitive deionization technology, the target ions have expanded from the initial alkali metal ions (potassium, calcium, sodium, magnesium) to some heavy metals (chromium, cadmium, lead, mercury) and rare metals (lithium, cesium, beryllium, titanium). Traditional carbon-based materials, such as activated carbon, graphene, carbon aerogel, etc., are selected as traditional capacitive deionization electrode materials because of their good conductivity and large specific surface area. However, due to the mechanism of carbon materials storing ions in the electrical double layer at the interface, the selectivity is poor and the removal rate is low, which limits the application of carbon materials in complex situations. Therefore, designing new electrode materials with high selectivity and excellent adsorption / desorption cycle performance is the focus of current capacitive deionization technology research.
[0005] Compared with traditional carbon-based materials that rely on the electric double layer mechanism to adsorb ions, the Faraday system with redox-active materials as electrodes has the advantages of strong ion selectivity and high specific capacitance, and is a very promising electrode material that can be used for environmental remediation. Transition metal ferrocyanide, also known as Prussian blue and its derivatives, is a typical class of redox-active materials, usually with a face-centered cubic lattice structure and an open framework, which is conducive to the rapid insertion and extraction of cations in aqueous solutions. Potassium zinc ferrocyanide, as one of the Prussian blue-like materials with the best chemical stability and the lowest toxicity, has been widely used in the field of aqueous rechargeable batteries. Given that there are few reports on the application of potassium zinc ferrocyanide in cobalt recovery and its high cation adsorption capacity, it is of great significance to use potassium zinc ferrocyanide to recover cobalt from waste lithium cobalt oxide batteries. Summary of the invention
[0006] Based on the technical problems existing in the background technology, the present invention proposes a preparation method and application of potassium zinc ferrocyanide / carbon cloth composite electrode material.
[0007] The present invention provides a method for preparing a potassium zinc ferrocyanide / carbon cloth composite electrode material, comprising the following steps:
[0008] S1, performing hydrophilic treatment on the carbon cloth to obtain a hydrophilic carbon cloth;
[0009] S2, using the hydrophilic carbon cloth as a working electrode and the zinc salt solution as an electrodeposition precursor solution, electrochemically depositing elemental zinc on the surface of the hydrophilic carbon cloth under constant current conditions;
[0010] S3. After the reaction is completed, the carbon cloth is taken out, washed with deionized water, and vacuum dried to obtain a single zinc / carbon cloth composite material;
[0011] S4. Place the elemental zinc / carbon cloth composite material in a potassium ferrocyanide aqueous solution, perform a constant temperature hydrothermal reaction, wash with deionized water, and vacuum dry to obtain a potassium zinc ferrocyanide / carbon cloth composite electrode material.
[0012] Preferably, in S1, the hydrophilic treatment comprises: in a polytetrafluoroethylene reactor, immersing the carbon cloth in a 1-5 mol / L nitric acid solution and heating at 60-120° C. for 6-8 hours, cooling to room temperature, washing with deionized water until neutral, and then storing in deionized water.
[0013] Preferably, in S2, the zinc salt solution is selected from one or more of zinc sulfate solution, zinc chloride solution and zinc nitrate solution.
[0014] More preferably, in S2, the method for preparing the zinc salt solution comprises the following steps: dissolving zinc salt, anhydrous sodium sulfate and boric acid in water, and mixing them uniformly to obtain the zinc salt solution.
[0015] More preferably, in the S2, the mass ratio of zinc salt, anhydrous sodium sulfate, boric acid and water is (3-10):(3-10):(1-5):50.
[0016] Preferably, in S2, the constant current used for electrochemical deposition is -100 to -20 mA·cm -2 , the time is 500 to 1000 seconds.
[0017] Preferably, in S3, the vacuum drying temperature is 40 to 80° C. and the time is 6 to 18 hours.
[0018] Preferably, in said S4, the method for preparing the potassium ferrocyanide aqueous solution comprises the following steps: dissolving potassium ferrocyanide in water to obtain a potassium ferrocyanide solution.
[0019] More preferably, in said S4, the mass ratio of potassium ferrocyanide to water is (5-20):50.
[0020] Preferably, in S4, the temperature of the isothermal hydrothermal reaction is 60-100° C. and the time is 5-11 hours.
[0021] Preferably, in S4, the vacuum drying is carried out at a temperature of 40 to 80° C. and for a time of 6 to 18 hours.
[0022] The present invention also proposes an application of the potassium zinc ferrocyanide / carbon cloth composite electrode material prepared by the above preparation method in electrochemical recovery of cobalt elements in discarded lithium cobalt oxide batteries.
[0023] Preferably, in the electrochemical recovery of cobalt from discarded lithium cobalt oxide batteries, the potassium zinc ferrocyanide / carbon cloth composite electrode material prepared by the above method is used as the working electrode, the hydrophilic carbon cloth is used as the counter electrode, and the silver / silver chloride electrode is used as the reference electrode.
[0024] Preferably, before the electrochemical recovery of cobalt from waste lithium cobalt oxide batteries, the potassium zinc ferrocyanide / carbon cloth composite electrode material is placed in a 1 mg / L potassium nitrate solution and pretreated with an oxidation potential of +1.5 V (vs. Ag / AgCl) for 30 minutes to expel potassium ions from the potassium zinc ferrocyanide / carbon cloth composite electrode material.
[0025] The beneficial effects of the present invention are:
[0026] The present invention provides a method for preparing a potassium zinc ferrocyanide / carbon cloth composite electrode material. A self-supporting electrode loaded with potassium zinc ferrocyanide cubic blocks based on carbon cloth is prepared by a process combining electrochemical deposition of elemental zinc and hydrothermal reaction of potassium ferrocyanide, and is suitable for the recovery of cobalt elements in discarded lithium cobalt oxide batteries. The potassium zinc ferrocyanide prepared by the present invention has an open framework structure and a specific selective pseudocapacitive behavior. The potassium zinc ferrocyanide / carbon cloth composite electrode material has a high efficiency electrochemical adsorption capacity and selectivity for cobalt ions. With the help of this characteristic, the separation of cobalt ions and lithium ions is achieved, and important industrial raw materials such as lithium carbonate and cobalt hydroxide are recovered by chemical precipitation. A method for preparing a potassium zinc ferrocyanide / carbon cloth composite electrode material and its application not only solve the problem of material loss of potassium zinc ferrocyanide materials during use, but also improve the mechanical properties and cycle stability of the composite electrode material, and realize the rapid, efficient and selective recovery of cobalt elements in the leachate of discarded lithium cobalt oxide batteries. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 This is a scanning electron microscope photograph of the potassium zinc ferrocyanide / carbon cloth composite electrode material prepared in an embodiment of the present invention.
[0028] Figure 2 The following are scanning electron microscope photos of the hydrophilic carbon cloth electrode material (a) prepared in Comparative Example 1 and the elemental zinc / carbon cloth composite material (b) prepared in Comparative Example 2.
[0029] Figure 3 The X-ray diffraction spectra of the electrode materials prepared in Example 1, Comparative Example 1 and Comparative Example 2 of the present invention.
[0030] Figure 4 The potassium zinc ferrocyanide / carbon cloth composite electrode material prepared in the embodiment of the present invention is in the presence of 50 mM Co 2+ Cyclic voltammogram in solution.
[0031] Figure 5Co of the electrode material prepared in the examples and comparative examples of the present invention 2+ Schematic diagram of electroadsorption kinetic performance.
[0032] Figure 6 The Co of the potassium zinc ferrocyanide / carbon cloth composite electrode material of Example 1 of the present invention 2+ Schematic diagram of the adsorption / desorption cycle performance. DETAILED DESCRIPTION
[0033] The technical solution of the present invention is described in detail through specific embodiments.
[0034] In the following examples and comparative examples, the specific information of the raw materials used is as follows:
[0035] Carbon cloth: Manufacturer: Shanghai Hesen Electric Co., Ltd.
[0036] Unless otherwise specified, the materials, reagents, etc. used in the following examples and comparative examples can be obtained from commercial sources.
[0037] Example 1
[0038] A method for preparing a potassium zinc ferrocyanide / carbon cloth composite electrode material comprises the following steps:
[0039] S1. Soak a 2 cm (length) × 2 cm (width) carbon cloth in a polytetrafluoroethylene reactor containing 50 mL of 3 mol / L nitric acid solution and heat at 100°C for 6 h. After cooling to room temperature, take it out and wash it with deionized water until it is neutral, and then store it in deionized water;
[0040] S2. Take 5 g of zinc sulfate heptahydrate, 5 g of anhydrous sodium sulfate and 1.6 g of boric acid and dissolve them in 50 mL of deionized water to obtain a zinc sulfate solution. The hydrophilic carbon cloth is used as the working electrode and the zinc sulfate solution is used as the electrodeposition precursor solution. The constant current used for electrochemical deposition is -50 mA cm -2 , time is 600s;
[0041] S3. After the reaction is completed, the carbon cloth is taken out, washed with deionized water, and vacuum dried at 60° C. for 12 h to obtain a single zinc / carbon cloth composite material;
[0042] S4. Take 10 mg of potassium ferrocyanide and dissolve it in 50 mL of deionized water to obtain a potassium ferrocyanide aqueous solution. Place the elemental zinc / carbon cloth composite material in the potassium ferrocyanide aqueous solution, and perform hydrothermal reaction at 60°C for 7 hours. Wash with deionized water and dry in vacuum at 60°C for 12 hours to obtain a potassium zinc ferrocyanide / carbon cloth composite electrode material. The composite material is KZHCF / CC-1.
[0043] Example 2
[0044] A method for preparing a potassium zinc ferrocyanide / carbon cloth composite electrode material comprises the following steps:
[0045] S1. Soak a 2 cm (length) × 2 cm (width) carbon cloth in a polytetrafluoroethylene reactor containing 50 mL of 3 mol / L nitric acid solution and heat at 100°C for 6 h. After cooling to room temperature, take it out and wash it with deionized water until it is neutral, and then store it in deionized water;
[0046] S2. Take 5 g of zinc sulfate heptahydrate, 5 g of anhydrous sodium sulfate and 1.6 g of boric acid and dissolve them in 50 mL of deionized water to obtain a zinc sulfate solution. The hydrophilic carbon cloth is used as the working electrode and the zinc sulfate solution is used as the electrodeposition precursor solution. The constant current used for electrochemical deposition is -50 mA cm -2 , time is 800s;
[0047] S3. After the reaction is completed, the carbon cloth is taken out, washed with deionized water, and vacuum dried at 60° C. for 12 h to obtain a single zinc / carbon cloth composite material;
[0048] S4. Take 10 mg of potassium ferrocyanide and dissolve it in 50 mL of deionized water to obtain a potassium ferrocyanide aqueous solution. Place the elemental zinc / carbon cloth composite material in the potassium ferrocyanide aqueous solution, and perform hydrothermal reaction at 60°C for 7 hours. Wash with deionized water and vacuum dry at 60°C for 12 hours to obtain a potassium zinc ferrocyanide / carbon cloth composite electrode material. The composite material is KZHCF / CC-2.
[0049] Example 3
[0050] A method for preparing a potassium zinc ferrocyanide / carbon cloth composite electrode material comprises the following steps:
[0051] S1. Soak a 2 cm (length) × 2 cm (width) carbon cloth in a polytetrafluoroethylene reactor containing 50 mL of 3 mol / L nitric acid solution and heat at 100°C for 6 h. After cooling to room temperature, take it out and wash it with deionized water until it is neutral, and then store it in deionized water;
[0052] S2. Take 5 g of zinc sulfate heptahydrate, 5 g of anhydrous sodium sulfate and 1.6 g of boric acid and dissolve them in 50 mL of deionized water to obtain a zinc sulfate solution. The hydrophilic carbon cloth is used as the working electrode and the zinc sulfate solution is used as the electrodeposition precursor solution. The constant current used for electrochemical deposition is -50 mA cm -2 , time is 1000s;
[0053] S3. After the reaction is completed, the carbon cloth is taken out, washed with deionized water, and vacuum dried at 60° C. for 12 h to obtain a single zinc / carbon cloth composite material;
[0054] S4. Take 10 mg of potassium ferrocyanide and dissolve it in 50 mL of deionized water to obtain a potassium ferrocyanide aqueous solution. Place the elemental zinc / carbon cloth composite material in the potassium ferrocyanide aqueous solution, and perform hydrothermal reaction at 60°C for 7 hours. Wash with deionized water and vacuum dry at 60°C for 12 hours to obtain a potassium zinc ferrocyanide / carbon cloth composite electrode material. The composite material is KZHCF / CC-3.
[0055] Comparative Example 1
[0056] A method for preparing a hydrophilic carbon cloth electrode material comprises the following steps:
[0057] S1. Soak a 2 cm (length) × 2 cm (width) carbon cloth in a polytetrafluoroethylene reactor containing 50 mL of 3 mol / L nitric acid solution and heat at 100 °C for 6 h;
[0058] S2. After the reaction is completed, the carbon cloth is taken out, washed with deionized water until neutral, and then vacuum dried at 60°C for 12 hours to obtain the hydrophilic carbon cloth electrode material CC.
[0059] Comparative Example 2
[0060] A method for preparing a single-element zinc / carbon cloth composite electrode material comprises the following steps:
[0061] S1. Soak a 2 cm (length) × 2 cm (width) carbon cloth in a polytetrafluoroethylene reactor containing 50 mL of 3 mol / L nitric acid solution and heat at 100°C for 6 h. After cooling to room temperature, take it out and wash it with deionized water until it is neutral, and then store it in deionized water;
[0062] S2. Take 5 g of zinc sulfate heptahydrate, 5 g of anhydrous sodium sulfate and 1.6 g of boric acid and dissolve them in 50 mL of deionized water to obtain a zinc sulfate solution. The hydrophilic carbon cloth is used as the working electrode and the zinc sulfate solution is used as the electrodeposition precursor solution. The constant current used for electrochemical deposition is -50 mA cm -2 , time is 600s;
[0063] S3. After the reaction is completed, the carbon cloth is taken out, washed with deionized water, and vacuum dried at 60°C for 12 hours to obtain the single zinc / carbon cloth composite electrode material Zn / CC.
[0064] An application of a potassium zinc ferrocyanide / carbon cloth composite electrode material: the recovery of cobalt elements in discarded lithium cobalt oxide batteries, specifically including: the lithium cobalt oxide batteries of discarded laptop computers are first completely discharged in a 5% sodium chloride solution, and then manually disassembled in a vacuum glove box to obtain electrode materials, followed by crushing and sieving the lithium cobalt oxide powder material. The ion leaching process is carried out in a 100mL beaker, and 50mL of a mixed solution containing 2.5mol / L hydrochloric acid and 0.6% (v / v) hydrogen peroxide is prepared, and 2.5g of lithium cobalt oxide powder is added thereto, and stirred at room temperature for 48h. Using a potassium zinc ferrocyanide / carbon cloth composite electrode, a carbon cloth of the same area, and a silver / silver chloride electrode as the working electrode, counter electrode, and reference electrode, Co was recovered in a three-electrode system. 2+ Electrosorption kinetics performance test. The lithium cobalt oxide leachate was diluted 1000 times with deionized water to obtain a mixed metal ion solution containing cobalt ions and lithium ions. 50 mL of the mixed solution was taken, and the pH value was adjusted to 9.0 by 0.1 mol / L ammonia water. Before the cobalt ion adsorption experiment, the potassium zinc ferrocyanide / carbon cloth composite electrode was first pretreated in a 1 mg / L potassium nitrate solution at an oxidation potential of +1.5V for 30 min to discharge the potassium ions in the potassium zinc ferrocyanide and the potassium ions remaining in the synthesis process. The potassium zinc ferrocyanide / carbon cloth composite electrode was then transferred to 50 mL of metal leachate, and a constant voltage of -0.6V was applied to the working electrode for 2 hours to reach the adsorption equilibrium state. During the reaction, 0.5 mL of solution was taken out from the reaction vessel at predetermined time intervals, and its metal ion concentration was analyzed and detected. After the reaction, the potassium zinc ferrocyanide / carbon cloth composite electrode material was washed with deionized water and transferred to a 1 mg / L potassium nitrate solution for desorption of cobalt ions and electrode regeneration, and then the concentration of desorbed cobalt ions in the solution was detected. After applying an oxidation potential of +1.5 V to the potassium zinc ferrocyanide / carbon cloth composite electrode for 30 min, it was washed with deionized water and dried in an oven at 60°C overnight for the next cobalt recovery experiment.
[0065] The potassium zinc ferrocyanide / carbon cloth composite electrode material prepared in Examples 1 to 3 was subjected to Co 2+ Electrosorption kinetics performance test; Comparative Example 1 Co 2+ The electrosorption kinetics performance test is as follows: the only difference is that the potassium zinc ferrocyanide / carbon cloth composite electrode material is replaced with the hydrophilic carbon cloth electrode material CC obtained in Comparative Example 1; Comparative Example 2 is subjected to the above application. 2+ The electrosorption kinetic performance test is as follows: the only difference is that the potassium zinc ferrocyanide / carbon cloth composite electrode material is replaced with the elemental zinc / carbon cloth composite electrode material Zn / CC obtained in Comparative Example 2; the test results are as follows Figure 5 shown.
[0066] The electrode materials prepared in the examples and comparative examples were tested by scanning electron microscope. The test results are as follows: Figures 1-2 As shown. Figure 1 As shown, Figure 1 a is a scanning electron microscope photo of the potassium zinc ferrocyanide / carbon cloth composite material prepared in Example 1 of the present invention. After the hydrothermal reaction, a layer of dense and uniform potassium zinc ferrocyanide nanocubes is evenly loaded on the entire surface of the carbon cloth substrate. The size of the cubes is about 1 μm. 3 , and well dispersed throughout the carbon cloth fiber skeleton; Figure 1 b is a scanning electron microscope photo of the potassium zinc ferrocyanide / carbon cloth composite material prepared in Example 2 of the present invention. As the electrodeposition time increases, the volume of the cubic block increases to 8 μm 3 Around, the cubes begin to agglomerate; Figure 1 c is a scanning electron microscope photo of the potassium zinc ferrocyanide / carbon cloth composite material prepared in Example 3 of the present invention. As the electrodeposition time continues to increase, the volume of the cubic block increases to 12 μm 3 Left and right, the cubes are tightly packed together. Figure 2 The following are scanning electron microscope photos of the hydrophilic carbon cloth electrode material and the single zinc / carbon cloth composite electrode material prepared in the comparative example. Figure 2 a is the hydrophilic carbon cloth electrode material prepared in Comparative Example 1 of the present invention. The surface of the carbon fiber after the hydrothermal reaction with the nitric acid solution is smooth and free of impurities, which is conducive to the subsequent deposition of elemental zinc; Figure 2 b is the single zinc / carbon cloth composite electrode material prepared in comparative example 2 of the present invention. After electrochemical deposition, the entire surface of the carbon cloth substrate is uniformly loaded with a layer of dense nanosheets, whose lateral size is 1 to 2 μm. The electrode materials prepared in Example 1, comparative example 1 and comparative example 2 were subjected to X-ray diffraction test. The test results are as follows: Figure 3 As shown, the diffraction peak of the hydrophilic carbon cloth electrode material CC at 24.0o corresponds to the (0 0 2) crystal plane of graphite; the diffraction peaks of the elemental zinc / carbon cloth composite electrode material Zn / CC at 36.3o and 39.0o are from the (0 0 2) and (1 0 0) crystal plane reflections of the zinc nanosheets, respectively, indicating the successful deposition of zinc on the carbon cloth surface; the main characteristic diffraction peaks of the potassium zinc ferrocyanide / carbon cloth composite material KZHCF / CC-1 at 16.4o, 19.7o, 21.8o, 24.3o, 24.5o and 28.7o correspond to the (1 1 3), (0 2 4), (1 1 6), (2 1 4), (3 0 0) and (1 1 9) crystal planes of K2Zn3[Fe(CN)6]2·9H2O, respectively, indicating the successful preparation of the potassium zinc ferrocyanide / carbon cloth composite electrode material. Figure 4 The potassium zinc ferrocyanide / carbon cloth composite electrode material prepared in the embodiment of the present invention is in the presence of 50 mM Co 2+Cyclic voltammetry curves in the solution; A group of significant redox peaks appeared on the cyclic voltammetry curves of the potassium zinc cyanide / carbon cloth composite electrode materials of Examples 1 to 3, indicating that the potassium zinc ferrocyanide / carbon cloth composite electrode material can control Co through electrochemical reaction 2+ The KZHCF / CC-1 composite electrode material prepared in Example 1 has a larger specific capacitance than the KZHCF / CC-2 composite electrode material prepared in Example 2 and the KZHCF / CC-3 composite electrode material prepared in Example 3, indicating that its electrosorption of Co 2+ 's ability is stronger. Figure 5 Co of the electrode material prepared in the examples and comparative examples of the present invention 2+ Schematic diagram of electrosorption kinetics; under weak alkaline conditions of pH 9, Co(NH3)6 3+ The hydration radius is Less than Co 2+ Hydration radius The advantage of a small hydration radius makes Co(NH3)6 3+ It is easier to enter the molecular framework of potassium zinc ferrocyanide, thereby improving the recovery rate of cobalt; the KZHCF / CC-1 composite electrode material prepared in Example 1 of the present invention can recover 50mL of 30mg·g -1 Cobalt ions and 1.5 mg g -1 The waste cobalt oxide battery leachate of lithium ions achieves efficient and selective electrochemical adsorption of cobalt (98.6%), which is higher than the KZHCF / CC-2 composite electrode material prepared in Example 2 (74.0%), the KZHCF / CC-3 composite electrode material prepared in Example 3 (66.0%), the CC electrode material prepared in Comparative Example 1 (3.7%) and the Zn / CC composite electrode material prepared in Comparative Example 2 (4.0%), indicating that the Co of the potassium zinc ferrocyanide / carbon cloth composite electrode material prepared under the condition of shorter electrodeposition time is 2+ The adsorption performance is the best, and the carbon cloth substrate and zinc nanosheets are excluded. 2+ The effect of adsorption. Figure 6 The Co of the potassium zinc ferrocyanide / carbon cloth composite electrode material of Example 1 of the present invention 2+ Schematic diagram of the adsorption / desorption cycle performance; after the potassium zinc ferrocyanide / carbon cloth composite electrode material prepared in Example 1 of the present invention was recycled for 5 times, the adsorption and desorption efficiencies of cobalt ions decreased by 16.6% and 16.0%, respectively, indicating that most of the adsorbed cobalt ions can be desorbed from the electrode, and the electrode material itself can be successfully regenerated and recycled by converting to an oxidized state through an electrochemical reaction.
[0067] In summary, the potassium zinc ferrocyanide / carbon cloth composite electrode material provided by the present invention can achieve efficient and selective electrochemical adsorption of cobalt (98.6%) on the waste lithium cobalt oxide battery leachate and desorb cobalt ions by applying a reverse potential; and can adsorb / desorb cobalt ions multiple times in a cycle.
[0068] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A method for preparing potassium zinc ferrocyanide / carbon cloth composite electrode material, characterized in that: The following steps are involved: S1, performing hydrophilic treatment on the carbon cloth to obtain a hydrophilic carbon cloth; S2, using the hydrophilic carbon cloth as a working electrode and the zinc salt solution as an electrodeposition precursor solution, electrochemically depositing elemental zinc on the surface of the hydrophilic carbon cloth under constant current conditions; S3. After the reaction is completed, the carbon cloth is taken out, washed with deionized water, and vacuum dried to obtain a single zinc / carbon cloth composite material; S4. Place the elemental zinc / carbon cloth composite material in a potassium ferrocyanide aqueous solution, perform a constant temperature hydrothermal reaction, wash with deionized water, and vacuum dry to obtain a potassium zinc ferrocyanide / carbon cloth composite electrode material.
2. The preparation method according to claim 1, characterized in that: In the above S1, the hydrophilic treatment comprises: in a polytetrafluoroethylene reactor, immersing the carbon cloth in a 1-5 mol / L nitric acid solution and heating at 60-120° C. for 6-8 hours, cooling to room temperature, washing with deionized water until neutral, and then storing in deionized water.
3. The preparation method according to claim 1, characterized in that: In the S2, the constant current used for electrochemical deposition is -100 to -20 mA·cm -2 , the time is 500 to 1000 seconds.
4. The preparation method according to claim 1, characterized in that: In the above-mentioned S3, the vacuum drying temperature is 40-80° C. and the time is 6-18 hours.
5. The preparation method according to claim 1, characterized in that: In the above-mentioned S4, the method for preparing the potassium ferrocyanide aqueous solution comprises the following steps: dissolving potassium ferrocyanide in water to obtain a potassium ferrocyanide solution; the mass ratio of potassium ferrocyanide to water is (5-20):
50.
6. The preparation method according to claim 1, characterized in that: In the S4, the temperature of the isothermal hydrothermal reaction is 60-100° C., and the time is 5-11 hours; the temperature of the vacuum drying is 40-80° C., and the time is 6-18 hours.
7. An application of potassium zinc ferrocyanide / carbon cloth composite electrode material obtained by the preparation method according to any one of claims 1 to 6 in electrochemical recovery of cobalt elements from waste lithium cobalt oxide batteries, characterized in that: The potassium zinc ferrocyanide / carbon cloth composite electrode material is used as a working electrode, the hydrophilic carbon cloth is used as a counter electrode, and the silver / silver chloride electrode is used as a reference electrode.
Citation Information
Patent Citations
Carbon-based zinc material and preparation method thereof
CN105742643A
Derivative electrocatalyst for growing Prussian blue or Prussian blue analogues in situ on metal substrate and preparation method of derivative electrocatalyst
CN110449156A
Zinc cobaltate nanosheet / carbon fiber cloth composite material and preparation method and application thereof
CN113035589A
Prussian blue composite material as well as preparation method and application thereof
CN115505939A
Neutral silver-zinc secondary battery based on electrochemical in-situ growth electrode and preparation method thereof
CN116365055A