Optical crystal, preparation method and application
Through the development of the new inorganic compound AgVSeO5 and hydrothermal preparation technology, the problem of insufficient performance of existing nonlinear optical crystals in laser frequency conversion and frequency doubling applications has been solved, and efficient laser frequency doubling and high transmittance are achieved. Its excellent performance in the field of infrared nonlinear optics.
Patent Information
- Application Number
- CN202310497645.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-05
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2043-05-05
AI Technical Summary
Existing nonlinear optical crystals have insufficient performance in laser frequency conversion and frequency doubling applications, especially under high frequency and high intensity laser conditions, which are difficult to meet the needs of emerging laser technologies.
A new nonlinear optical crystal AgVSeO5 of inorganic compound has a strong frequency multiplication effect, and the powder SHG coefficient is 0.5 to 5 times that of AGS. It is prepared by hydrothermal crystallization to form a red striped crystal with high purity and High crystallinity.
The frequency doubling effect under 1910nm laser reaches 0.5 to 5 times that of AGS, and has a high transmittance in the range of 1000 to 4000nm, showing excellent infrared nonlinear optical performance and has potential application value.
Smart Images

Figure CN118895562A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to an optical crystal, a preparation method and an application thereof, and belongs to the field of inorganic materials. Background Art
[0002] Nonlinear optical crystals refer to functional materials with nonlinear optical effects (SHG effects), which can realize functions such as laser frequency conversion, laser intensity and phase modulation, and holographic storage of laser signals. They are widely used in the fields of military and civilian high-tech optoelectronic materials. Currently, the nonlinear optical crystals in practical use include AgGaS 2 (AGS), LiB 3 O 5 (LBO), β-BaB 2 O 4 (BBO), KH 2 PO 4 (KDP), KTiOPO 4 (KTP), α-LiIO 3 With the development of laser technology and the emergence of tunable lasers, nonlinear optical devices have developed rapidly, including laser frequency doubling, frequency mixing, parametric oscillation and amplification; electro-optic modulation, deflection, Q switch and photorefractive devices. The above research and applications have put forward more and higher requirements for the physical and chemical properties of nonlinear optical materials, and also promoted the rapid development of nonlinear optical materials. Second-order nonlinear optical crystal materials must have a non-centrosymmetric structure. Summary of the invention
[0003] The present application aims to provide an inorganic compound nonlinear optical crystal, which exhibits a strong frequency doubling effect, has a powder SHG coefficient of 0.5 to 5 times that of AGS, and can achieve phase matching, and is a nonlinear optical material with potential application value.
[0004] According to one aspect of the present application, an optical crystal is provided, wherein the chemical formula of the optical crystal is AgVSeO 5 ;
[0005] The optical crystal belongs to the orthorhombic system;
[0006] The space group of the optical crystal is Pca2 1 .
[0007] Optionally, the unit cell parameters of the optical crystal are α=β=γ=90°, Z=8.
[0008] Optionally, the unit cell parameters of the optical crystal are α=β=γ=90°, Z=8.
[0009] Optionally, the unit cell parameters of the optical crystal are α=β=γ=90°, Z=8.
[0010] Optionally, in the optical crystal, V includes V 1 and V 2 Site, V 1 and V 2 All of them coordinate with six O to form VO 6 -I Octahedron and VO 6 -II octahedron.
[0011] Optionally, the VO 6 -I Octahedron and VO 6 -II octahedrons share the same vertex O to form a "V-shaped" zigzag chain. The three adjacent parallel V-shaped zigzag chains are connected by triangular pyramidal SeO 3 The Ag ions are connected to form a "W-shaped" chain through electrostatic interactions with the O ions on the "W-shaped" chain to form a three-dimensional structure.
[0012] Optionally, AgVSeO 5 In V, there are V 1 and V 2 Two sites, V 1 and V 2 All of them coordinate with six O to form VO 6 -I Octahedron and VO 6 -II octahedron, VO 6 -I Octahedron and VO 6 -II octahedra are connected by common vertices O to form an infinitely long V-shaped zigzag chain. The three adjacent parallel "V-shaped" chains are connected by triangular pyramidal SeO 3 The Ag ions are connected to form an infinitely long "W-shaped" chain, and the Ag ions are connected to form a three-dimensional structure through electrostatic interactions with the O on the "W-shaped" chain.
[0013] Optionally, the ultraviolet absorption cutoff wavelength of the optical crystal is 620-660 nm.
[0014] Optionally, the ultraviolet absorption cut-off wavelength of the optical crystal is selected from any value among 620nm, 625nm, 630nm, 640nm, 650nm, 660nm or a range value between any two of the above points.
[0015] Optionally, the frequency doubling effect of the optical crystal under 1910nm laser irradiation is AgGaS 2 0.5 to 5 times of.
[0016] Optionally, the optical crystal has a second-order nonlinear optical SHG effect.
[0017] Optionally, the transmittance of the optical crystal in the wavelength range of 1000-4000 nm is ≥83%.
[0018] According to another aspect of the present application, a method for preparing the optical crystal described above is provided, the method comprising:
[0019] In a sealed container, a mixture containing Ag source, V source, Se source and water is reacted and cooled to obtain an optical crystal.
[0020] Optionally, the Ag source is selected from at least one of Ag oxide, Ag halide, silver salt and silver ion standard solution.
[0021] Optionally, the Ag source is selected from at least one of silver oxide, silver fluoride, silver chloride, silver bromide, silver iodide, silver carbonate, silver acetate, silver phosphate, silver tetrafluoroborate, silver perchlorate, silver benzoate, silver iodate, silver nitrate, silver metavanadate, silver perchlorate hydrate, silver chromate, silver tungstate, silver trifluoroacetate, silver selenide, silver telluride, silver hexafluorophosphate, silver nitrate concentrate, silver sulfate, and silver ion standard solution.
[0022] Optionally, the V source is selected from at least one of V oxide, vanadium powder, vanadium halide and vanadate.
[0023] Optionally, the V source is selected from vanadium oxide (V 2 O 4 ), vanadium oxide (V 2 O 3 ), vanadium oxide (V 6 O 13 ), vanadium pentoxide, vanadium powder, vanadium trichloride, vanadium chloride, vanadium fluoride (F 3 OV), vanadium fluoride (VF 3 ), at least one of vanadium boride, vanadium sulfide, gallium vanadate, vanadium oxysulfate, sodium orthovanadate, sodium metavanadate, sodium metavanadate hydrate, ammonium metavanadate, potassium metavanadate, silver metavanadate, potassium orthovanadate, cesium orthovanadate, cesium metavanadate, lead metavanadate, and bismuth vanadate.
[0024] Optionally, the Se source is selected from at least one of selenium dioxide, selenium disulfide, selenide, selenous acid, selenite, selenous acid hydrate, and a selenium standard solution.
[0025] Optionally, the Se source is selected from selenium dioxide, selenium disulfide, nickel selenide, zinc selenide, molybdenum selenide, gallium selenide, iron selenide, copper selenide, cadmium selenide, aluminum selenide, tungsten selenide, indium selenide, sodium selenide, selenium tetrachloride, selenium chloride (Cl 2 Se 2), selenium bromide (SeBr 4 ), at least one of tin dichloride oxide, potassium selenite, selenous acid, sodium selenite, zinc selenite, selenite, selenite hydrate, and selenium standard solution.
[0026] Optionally, the pH adjuster is selected from at least one of a strong base and a weak acid salt, a strong acid and a weak base salt, a strong acid solution, a medium-strong acid solution, a weak acid solution, a strong base and its solution, and a weak base and its solution.
[0027] Optionally, the pH adjuster is selected from at least one of ammonium carbonate, ammonium bicarbonate, sodium carbonate, potassium carbonate, potassium bicarbonate, sodium bicarbonate, acetic acid solution, potassium acetate, sodium acetate, hydrochloric acid, ammonium chloride, phosphoric acid, ammonium phosphate, diammonium hydrogen phosphate, diammonium dihydrogen phosphate, potassium phosphate, potassium hydrogen phosphate, potassium dihydrogen phosphate, sodium phosphate, sodium hydrogen phosphate, sodium dihydrogen phosphate, nitric acid, ammonium nitrate, sulfuric acid, ammonium sulfate, diammonium dihydrogen sulfate, ammonium hydrogen sulfate, ammonia solution, potassium hydroxide, and sodium hydroxide.
[0028] Optionally, the molar ratio of the Ag source: V source: Se source: pH regulator: water is: 1: 0.01-200: 0.01-600: 0.01-500: 1-2000;
[0029] The molar number of the Ag source is calculated by the molar number of the Ag element contained therein, the molar number of the V source is calculated by the molar number of the V element contained therein, the molar number of the Se source is calculated by the molar number of the Se element contained therein, and the pH adjuster is calculated by the molar number of the effective ingredient.
[0030] Optionally, the molar ratio of the Ag source: V source: Se source: pH regulator: water is: 1: 0.01-100: 0.1-400: 0.01-300: 10-1500;
[0031] The molar number of the Ag source is calculated by the molar number of the Ag element contained therein, the molar number of the V source is calculated by the molar number of the V element contained therein, the molar number of the Se source is calculated by the molar number of the Se element contained therein, and the pH adjuster is calculated by the molar number of the effective ingredient.
[0032] Optionally, the molar ratio of the Ag source: V source: Se source: pH regulator: water is: 1: 0.05-80: 0.1-300: 0.1-100: 20-1000;
[0033] The molar number of the Ag source is calculated by the molar number of the Ag element contained therein, the molar number of the V source is calculated by the molar number of the V element contained therein, the molar number of the Se source is calculated by the molar number of the Se element contained therein, and the pH adjuster is calculated by the molar number of the effective ingredient.
[0034] Optionally, in the mixture, the silver ions come from silver nitrate, the vanadium element comes from vanadium trioxide, and the selenium element comes from selenium dioxide; and the pH regulator is an ammonia solution.
[0035] Optionally, the aqueous ammonia solution is selected from 22-25 wt % aqueous ammonia solution.
[0036] Optionally, in the mixture, silver ions come from silver nitrate, vanadium elements come from vanadium trioxide, selenium elements come from selenium dioxide, the pH regulator is an ammonia solution, and the water here comes from water in the ammonia solution and added deionized water.
[0037] Optionally, the reaction temperature is 100° C. to 320° C., and the reaction time is 4 h to 1000 h.
[0038] Optionally, the reaction temperature is independently selected from 100°C, 110°C, 120°C, 130°C, 140°C, 150°C, 160°C, 170°C, 180°C, 190°C, 200°C, 210°C, 220°C, 230°C, 240°C, 250°C, 260°C, 270°C, 280°C, 290°C, 300°C, 310°C, 320°C, or any range between two of them.
[0039] Optionally, the reaction time is independently selected from 4h, 6h, 12h, 24h, 30h, 40h, 50h, 62h, 72h, 80h, 100h, 120h, 140h, 160h, 180h, 210h, 240h, 260h, 280h, 300h, 320h, 340h, 360h, 380h, 400h, 420h, 440h, 460h, 480h, 500h, 520h, 540h, 560h, 580h, 600h, 620h, 640h, 660h, 680h, 700h, 720h, 740h, 760h, 780h, 800h, 1000h, any value or any range value between two of them.
[0040] Optionally, the reaction temperature is 150° C. to 300° C., and the reaction time is 6 h to 800 h.
[0041] Optionally, the cooling rate is 0.01°C / h to 20°C / h.
[0042] Optionally, the cooling rate is independently selected from any value among 0.01℃ / h, 0.05℃ / h, 0.1℃ / h, 1℃ / h, 2℃ / h, 3℃ / h, 4℃ / h, 6℃ / h, 8℃ / h, 10℃ / h, 13℃ / h, 15℃ / h, 18℃ / h, 20℃ / h or any range between two values.
[0043] Optionally, the cooling rate is 0.01°C / h to 15°C / h.
[0044] Optionally, the cooling rate is 0.01°C / h to 10°C / h.
[0045] According to another aspect of the present application, there is provided an application of the optical crystal described above, or an optical crystal prepared by the preparation method described above in a laser frequency converter.
[0046] The present application provides a method for preparing an optical crystal, using a hydrothermal crystallization method to grow a red long strip of AgVSeO 5 The method is simple and can obtain high-purity and high-crystallinity inorganic compound AgVSeO 5 Crystalline material.
[0047] As an embodiment of the present application, a method for preparing an inorganic compound crystal comprises the following steps:
[0048] The raw materials containing silver, vanadium, selenium, a pH regulator and water are mixed and placed in a reactor lined with polytetrafluoroethylene, and then sealed and crystallized at a crystallization temperature of 100°C to 320°C for more than 4 hours; after the crystallization is completed, the system is cooled to room temperature at a cooling rate of no more than 20°C per hour, and the solid sample obtained after separation, washing and drying is the inorganic compound crystal.
[0049] The inorganic compound crystals prepared by the hydrothermal method have the morphology of red long strip crystals.
[0050] The beneficial effects of this application include:
[0051] 1) The present application provides an inorganic nonlinear optical crystal, the AgVSeO 5 The powder frequency-doubled effect under 1910nm laser irradiation is 0.5 to 5 times that of AGS, and phase matching can be achieved. 5 Crystals have great potential as nonlinear optical materials.
[0052] 2) The inorganic compound crystal AgVSeO provided in this application 5 It has a high transmittance in the spectral range of 1000-4000nm, and its ultraviolet absorption cut-off wavelength is about 644nm. It is a potential infrared nonlinear optical material with excellent performance.
[0053] 3) The present application provides a method for preparing an inorganic nonlinear optical crystal, which uses a hydrothermal crystallization method to grow a red long strip of AgVSeO 5The method is simple and can obtain high-purity and high-crystallinity inorganic compound AgVSeO 5 Crystalline material. BRIEF DESCRIPTION OF THE DRAWINGS
[0054] Figure 1 The inorganic compound crystal AgVSeO in Example 1 of the present application 5 Schematic diagram of the crystal structure.
[0055] Figure 2 The X-ray diffraction pattern of sample 1# of this application obtained by fitting the crystal structure analyzed by single crystal X-ray diffraction is compared with the diffraction pattern obtained by X-ray diffraction after the sample is ground into powder.
[0056] Figure 3 This is the infrared spectrum of sample 1# of this application.
[0057] Figure 4 This is the UV spectrum of sample 1# of this application.
[0058] Figure 5 This is a comparison chart of the frequency doubling effect of sample 1# in this application and the frequency doubling effect of AGS. DETAILED DESCRIPTION
[0059] The present application is described in detail below with reference to embodiments, but the present application is not limited to these embodiments.
[0060] Unless otherwise specified, the raw materials in the examples of the present application were purchased through commercial channels and used directly without treatment, and the instruments and equipment used adopted the schemes and parameters recommended by the manufacturers.
[0061] In this application, "room temperature" refers to 30±5°C.
[0062] In the present application, single crystal X-ray diffraction was performed using a SuperNova CCD single crystal X-ray diffractometer produced by Agilent Corporation of the United States.
[0063] Powder X-ray diffraction was performed using a Miniflex II X-ray powder diffractometer manufactured by Rigaku Corporation (Japan).
[0064] The UV-visible-near infrared spectrophotometer Lambda-950 from Perkin-Elmer, USA was used.
[0065] Example 1 AgVSeO 5 Hydrothermal synthesis of samples
[0066] The raw materials containing silver, vanadium, selenium, pH regulator and water are mixed and placed in a reactor with a polytetrafluoroethylene lining, and then sealed and crystallized at a crystallization temperature of 100°C to 320°C for more than 4 hours; after the crystallization is completed, the system is cooled to room temperature at a cooling rate of no more than 20°C, and a red long strip solid sample is obtained after separation, washing and drying, which is the sample of the inorganic compound crystal. AgVSeO 5 The crystal structure of Figure 1 As shown, AgVSeO 5 In V, there are V 1 and V 2 Two sites, V 1 and V 2 All of them coordinate with six O to form VO 6 -I Octahedron and VO 6 -II octahedron, VO 6 -I Octahedron and VO 6 -II octahedra are connected by common vertices O to form an infinitely long "V-shaped" zigzag chain. The three adjacent parallel "V-shaped" chains are connected by triangular pyramidal SeO 3 The Ag ions are connected to form an infinitely long "W-shaped" chain, and the Ag ions are connected to form a three-dimensional structure through electrostatic interactions with the O on the "W-shaped" chain.
[0067] The sample number, raw material type and dosage, crystallization temperature and holding time, and cooling rate are shown in Table 1. 3 ·H 2 O (22-25 wt%) refers to an aqueous ammonia solution with a mass fraction of 22-25%.
[0068] Table 1
[0069]
[0070] Example 2 Crystal structure analysis
[0071] Single crystal X-ray diffraction was used to analyze the structures of samples 1# to 3#.
[0072] The single crystal X-ray diffraction was performed on a SuperNova CCD X-ray single crystal diffractometer from Agilent, USA. The data collection temperature was 293K, and the diffraction light source was graphite monochromatized Mo-Kα rays. The scanning mode was ω-2θ; the data were processed for absorption correction using the Multi-Scan method. The structure analysis was completed using the SHELXTL-2014 program package; the positions of heavy atoms were determined using the direct method, and the coordinates of the remaining atoms were obtained using the difference Fourier synthesis method; the F-based 2 The full-matrix least-squares method was used to refine the coordinates of all atoms and the anisotropic thermal parameters.
[0073] Powder X-ray diffraction was carried out on a Miniflex II X-ray powder diffractometer produced by RIGAKU Co., Ltd., Japan. The test conditions were a fixed target monochromatic light source Cu-Kα, a wavelength of The voltage and current were 30 kV / 15 A, the scanning range was 10 to 60°, and the scanning step was 0.02°.
[0074] The results show that samples 1# to 3# are all pure phases. Taking sample 1# as an example, the single crystal X-ray diffraction pattern obtained by fitting the crystal structure analyzed by single crystal X-ray diffraction is compared with the diffraction pattern obtained by X-ray diffraction after the sample is ground into powder. Figure 2 As shown, the single crystal X-ray diffraction results show that the chemical formulas of samples 1# to 3# are all AgVSeO 5 , belongs to the orthorhombic system, the space group is Pca2 1 , the unit cell parameters are α=β=γ=90°, Z=8.
[0075] Taking sample 1# as a typical example, Table 2 shows the single crystal X-ray diffraction data. It can be seen that sample 1# belongs to the orthorhombic system and the space group is Pca2. 1 , the unit cell parameters are α=γ=β=90°, Z=8.
[0076] Table 2 AgVSeO 5 Crystal parameters
[0077]
[0078] Take sample 1# as a typical example. Figure 2 As shown, according to the crystal structure analyzed by single crystal X-ray diffraction, the fitted X-ray diffraction pattern is consistent with the pattern obtained by X-ray diffraction test after sample 1# is ground into powder, and the peak position and peak intensity are consistent, indicating that the obtained samples are of high purity.
[0079] Example 3 Diffuse reflection absorption spectrum test
[0080] like Figure 3 As shown, taking sample 1# as an example, the AgVSeO 5 Diffuse reflectance absorption spectroscopy was performed on a Lambda-950 UV-visible-near infrared spectrophotometer from Perkin-Elmer, USA. The crystal samples were ground into powder and BaSO 4 As a reference substrate. Test results are as follows Figure 3 and Figure 4 As shown, it shows that the compound AgVSeO 5The crystal has a wide transmission range and a very high transmittance in the spectral range of 1000-4000nm. The transmittance in the spectral range of 1000-4000nm is not less than 83%, and the ultraviolet absorption cut-off wavelength is about 640nm.
[0081] The diffuse reflection absorption spectrum test results of samples 2# and 3# are consistent with those of sample 1#.
[0082] Example 4 Frequency doubling test experiment and results
[0083] like Figure 5 As shown in the figure, sample 1# is a typical representative of the inorganic compound crystal AgVSeO 5 The specific steps are as follows: a Q-switched Nd:YAG solid laser with a frequency converter is used to generate a wavelength of 1910nm as the fundamental frequency light to irradiate the tested crystal powder, a photomultiplier tube is used to detect the generated second harmonic, and an oscilloscope is used to display the harmonic intensity. The test results show that the compound AgVSeO 5 Under 1910nm laser irradiation, the powder SHG coefficient is 0.5 to 3 times that of AGS.
[0084] The frequency doubling test results of samples 2# and 3# are consistent with those of sample 1#.
[0085] The above are only a few embodiments of the present application and do not constitute any form of limitation to the present application. Although the present application is disclosed as above with preferred embodiments, it is not intended to limit the present application. Any technician familiar with the profession, without departing from the scope of the technical solution of the present application, using the technical content disclosed above to make slight changes or modifications are equivalent to equivalent implementation cases and fall within the scope of the technical solution.
Claims
1. An optical crystal, It is characterized in that The chemical formula of the optical crystal is AgVSeO 5 ; The optical crystal belongs to the orthorhombic system; The space group of the optical crystal is Pca2 1 .
2. The optical crystal according to claim 1, It is characterized in that The unit cell parameters of the optical crystal are: α=β=γ=90°, Z=8; Preferably, the unit cell parameters of the optical crystal are α=β=γ=90°, Z=8; Preferably, the unit cell parameters of the optical crystal are α=β=γ=90°, Z=8.
3. The optical crystal according to claim 1, It is characterized in that In the optical crystal, V includes V 1 and V 2 Site, V 1 and V 2 All of them coordinate with six O to form VO 6 -I Octahedron and VO 6 -II octahedron; Preferably, the VO 6 -I Octahedron and VO 6 -II octahedrons share the same vertex O to form a V-shaped zigzag chain. The three adjacent parallel V-shaped zigzag chains are connected by triangular pyramidal SeO 3 The Ag ions are connected to form a W-shaped chain through electrostatic interactions with the O atoms on the W-shaped chain to form a three-dimensional structure.
4. The optical crystal according to claim 1, It is characterized in that The ultraviolet absorption cut-off wavelength of the optical crystal is 620-660nm; Preferably, the frequency doubling effect of the optical crystal under 1910nm laser irradiation is AgGaS 2 0.5 to 5 times; Preferably, the optical crystal has a second-order nonlinear optical SHG effect; Preferably, the transmittance of the optical crystal in the wavelength range of 1000-4000 nm is ≥83%.
5. The method for preparing an optical crystal according to any one of claims 1 to 4, It is characterized in that The preparation method comprises: In a sealed container, a mixture containing a Ag source, a V source, a Se source, a pH adjuster and water is reacted and cooled to obtain an optical crystal.
6. The preparation method according to claim 5, It is characterized in that The Ag source is selected from at least one of Ag oxide, Ag halide, silver salt, and silver ion standard solution; Preferably, the V source is selected from at least one of V oxide, vanadium powder, vanadium halide, and vanadate; Preferably, the Se source is selected from at least one of selenium dioxide, selenium disulfide, selenide, selenous acid and selenite.
7. The preparation method according to claim 5, It is characterized in that The molar ratio of the Ag source: V source: Se source: pH regulator: water is: 1: 0.01-200: 0.01-600: 0.01-500: 1-2000; The molar number of the Ag source is calculated by the molar number of the Ag element contained therein, the molar number of the V source is calculated by the molar number of the V element contained therein, and the molar number of the Se source is calculated by the molar number of the Se element contained therein; Preferably, the molar ratio of the Ag source: V source: Se source: pH regulator: water is: 1: 0.01-100: 0.1-400: 0.01-300: 10-1500; The molar number of the Ag source is calculated by the molar number of the Ag element contained therein, the molar number of the V source is calculated by the molar number of the V element contained therein, and the molar number of the Se source is calculated by the molar number of the Se element contained therein; Preferably, the molar ratio of the Ag source: V source: Se source: pH regulator: water is: 1: 0.05-80: 0.1-300: 0.01-100: 20-1000; The molar number of the Ag source is calculated by the molar number of the Ag element contained therein, the molar number of the V source is calculated by the molar number of the V element contained therein, and the molar number of the Se source is calculated by the molar number of the Se element contained therein.
8. The preparation method according to claim 5, It is characterized in that The reaction temperature is 100°C to 320°C, and the reaction time is 4h to 1000h; Preferably, the reaction temperature is 150° C. to 300° C., and the reaction time is 6 h to 800 h.
9. The preparation method according to claim 5, It is characterized in that The cooling rate is 0.01°C / h to 20°C / h; Preferably, the cooling rate is 0.01°C / h to 15°C / h; Preferably, the cooling rate is 0.01°C / h to 10°C / h.
10. Use of the optical crystal according to any one of claims 1 to 4 or the optical crystal prepared by the preparation method according to any one of claims 5 to 9 in a laser frequency converter.
Citation Information
Patent Citations
X-ray detector based on ATe3O8 single crystal and preparation method thereof
CN115274921A
Niobium lithium tellurate compound and preparation method and application of nonlinear optical crystal of niobium lithium tellurate compound
CN115717271A