A method for determining the content of boric acid in epoxy resin
By mixing the epoxy resin with a solvent and extracting it with a polyol aqueous solution, combined with sodium hydroxide titration method, the problems of cumbersome and large deviations in the boric acid determination process in the prior art are solved, and the boric acid content in the epoxy resin is accurate and efficient. Test.
Patent Information
- Application Number
- CN202411396843.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-09
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-10-09
AI Technical Summary
In the prior art, when determining the boric acid content in epoxy resin, the sample is cumbersome to process the sample, and the high temperature leads to the loss of boron element during the digestion process, which has a problem of large deviations in the test results, and it is difficult to accurately determine the resin insoluble in the alcohol-water system.
The solvent is mixed with epoxy resin to dissolve it, and the boric acid is extracted into the aqueous phase with a polyol aqueous solution. The boric acid content is determined by titration of sodium hydroxide standard solution. The blank test is performed using epoxy resin without boric acid to eliminate errors and improve detection. Accuracy.
It realizes accurate, efficient and simple measurement of boric acid content in epoxy resin at room temperature, reduces measurement deviations, and improves the repeatability and accuracy of detection.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of chemical detection, and in particular relates to a method for determining the content of boric acid in epoxy resin. Background Art
[0002] The acid value of the resin is used to characterize the total amount of free acid in the sample. The determination of the acid value can quantitatively characterize the structural properties of the resin, which is of great significance. Boric acid, as an acidic catalyst, can react with active groups such as hydroxyl and amine in epoxy resin to generate ester bonds and condensation products, forming a network structure, thereby promoting the curing reaction of epoxy resin.
[0003] In the prior art, ICP or the national standard method (GB / T 538-2018) is often used to determine the boric acid content. When ICP is used to determine the boric acid content, the sample pretreatment process is cumbersome and time-consuming, and the high temperature causes the loss of boron in the digestion process, resulting in a large deviation in the test results. The national standard method uses an alcohol-water system as the solvent, and epoxy resin has an insolubility problem, so an organic extraction system test method needs to be constructed, which also has the problem of cumbersome methods and large test deviations. Summary of the invention
[0004] The invention provides a method for determining the content of boric acid in an epoxy resin. The determination method provided by the invention can determine the content of boric acid in an epoxy resin that is insoluble in an alcohol-water system, and the detection is accurate, efficient, simple, safe and has good repeatability.
[0005] In order to achieve the above object, the present invention provides a method for determining the content of boric acid in epoxy resin, comprising the following steps:
[0006] 1) Mix the epoxy resin to be tested and the solvent to dissolve the epoxy resin in the solvent to obtain an organic solution containing the resin;
[0007] The solvent is chloroform, tetrahydrofuran, acetone, butanone, methyl ethyl ketone, dioxane, toluene, diethylene glycol dimethyl ether or dimethylformamide;
[0008] 2) Mix the polyol aqueous solution with the resin-containing organic solution, extract the boric acid into the aqueous phase, separate the phases, and obtain the product to be tested;
[0009] 3) Add indicator to the sample to be tested and titrate with sodium hydroxide standard solution until the solution turns pink, which is the titration end point. Record the volume of sodium hydroxide standard solution consumed in the titration, which is recorded as V1;
[0010] 4) Calculate the content of solid boric acid in epoxy resin. The specific formula is:
[0011] W=[(61.83*c*V1) / 1000m / s]*100%;
[0012] Where: W is the content of solid boric acid in epoxy resin, unit is %;
[0013] c is the concentration of sodium hydroxide standard solution, in mol / L;
[0014] m is the mass of the epoxy resin sample to be tested, in g;
[0015] s is the solid content of epoxy resin, unit is %;
[0016] 61.83 is the molar mass of boric acid in g / mol.
[0017] Preferably, a blank test is performed using an epoxy resin without boric acid, and the specific operation is the same as steps 1) to 3) in the above scheme. After the titration is completed, the volume of the sodium hydroxide standard solution consumed in the titration is recorded as V0;
[0018] Combined with the blank test, the content of solid boric acid in the epoxy resin is calculated. The specific formula is:
[0019] W=[(61.83*c*(V1-V0)) / 1000m / s]*100%;
[0020] Wherein: V0 is the volume of sodium hydroxide standard solution consumed in titration of epoxy resin without boric acid.
[0021] Preferably, in step 1), the mass volume ratio of the epoxy resin to be tested and the solvent is 0.1-0.5 g: 5-40 mL.
[0022] Preferably, the mass volume ratio of the epoxy resin to be tested to the polyol is 1 g:40-60 mL.
[0023] Preferably, in step 2), the volume ratio of polyol to water in the aqueous solution of polyol is 1:1-5.
[0024] Preferably, the polyol in step 2) is glycerol or mannitol.
[0025] Preferably, the polyol in step 2) is glycerol.
[0026] Preferably, the indicator in step 3) is one of phenolphthalein, a mixed indicator of thymol blue and cresol red, and a mixed indicator of thymol blue and phenolphthalein.
[0027] Preferably, the concentration of the sodium hydroxide standard solution in step 3) is 0.01-1 mol / L;
[0028] The calibration method of the sodium hydroxide standard solution is:
[0029] a. Mix 0.15-0.2g potassium hydrogen phthalate with 50-100mL deionized water, add 3-5 drops of phenolphthalein indicator, and titrate with the sodium hydroxide solution to be calibrated until the solution turns pink, which is the titration endpoint;
[0030] b. After the titration is terminated, calculate the concentration of the sodium hydroxide solution. The specific formula is:
[0031] c=1000m / 204.2V;
[0032] in:
[0033] m is the weight of potassium hydrogen phthalate, in g;
[0034] V is the volume of the sodium hydroxide solution to be calibrated consumed in the titration, in mL;
[0035] 204.2 is the molar mass of potassium hydrogen phthalate, in g / moL.
[0036] Preferably, the epoxy resin to be detected is a liquid epoxy resin.
[0037] Compared with the prior art, the advantages and positive effects of the present invention are:
[0038] The present invention provides a method for determining the content of boric acid in an epoxy resin. The present invention firstly mixes a solvent with the epoxy resin to be measured, so that the epoxy resin is dissolved in the solvent. Then, an alcohol-water mixture is added to extract boric acid into the water system, and the boric acid content in the water phase is tested. The determination method provided by the present invention performs the measurement at room temperature, thereby avoiding the measurement deviation caused by the thermal digestion of boric acid and improving the accuracy of the measurement. Moreover, the method is efficient and simple, and fills the gap in the determination method of the boric acid content of the resin that is insoluble in the alcohol-water system.
[0039] The present invention further adopts an epoxy resin without boric acid as a blank test. By setting up a blank test, the reaction of epoxy groups with alkali can be excluded, the consumption volume of sodium hydroxide is increased, and the influence of the test result being biased high can be increased, thereby further improving the accuracy. DETAILED DESCRIPTION
[0040] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0041] The present invention provides a method for determining the content of boric acid in epoxy resin, comprising the following steps:
[0042] 1) Mix the epoxy resin to be tested and the solvent to dissolve the epoxy resin in the solvent to obtain an organic solution containing the resin;
[0043] The solvent is chloroform, tetrahydrofuran, acetone, butanone, methyl ethyl ketone, dioxane, toluene, diethylene glycol dimethyl ether or dimethylformamide;
[0044] 2) Mixing the aqueous solution of the polyol with the organic solution containing the resin, extracting the boric acid into the aqueous phase, and separating the phases to obtain the product to be tested;
[0045] 3) Add indicator to the sample to be tested and titrate with sodium hydroxide standard solution until the solution turns pink, which is the titration end point. Record the volume of sodium hydroxide standard solution consumed in the titration, which is recorded as V1;
[0046] 4) Calculate the content of solid boric acid in epoxy resin. The specific formula is:
[0047] W=[(61.83*c*V1) / 1000m / s]*100%;
[0048] Where: W is the content of solid boric acid in epoxy resin, unit is %;
[0049] c is the concentration of sodium hydroxide standard solution, in mol / L;
[0050] m is the mass of the epoxy resin sample to be tested, in g;
[0051] s is the solid content of epoxy resin, unit is %;
[0052] 61.83 is the molar mass of boric acid in g / mol.
[0053] The present invention mixes the epoxy resin to be tested and a solvent, dissolves the epoxy resin in the solvent, and obtains an organic solution containing the resin; the solvent is chloroform, tetrahydrofuran, acetone, butanone, methyl ethyl ketone, dioxane, toluene, diethylene glycol dimethyl ether or dimethylformamide, more preferably chloroform. In the present invention, the mass volume ratio of the epoxy resin to be tested and the solvent is preferably 0.1~0.5g:2.5~40mL. In the present invention, the epoxy resin to be tested is preferably a liquid epoxy resin.
[0054] After obtaining the organic solution containing the resin, the present invention mixes the aqueous solution of the polyol with the organic solution containing the resin, extracts the boric acid into the aqueous phase, separates the phases, and obtains the product to be tested. In the present invention, the polyol is preferably glycerol or mannitol, more preferably glycerol; the volume ratio of the polyol to water in the aqueous solution of the polyol is preferably 1:1~5. In the present invention, the mass volume ratio of the epoxy resin to be tested and the polyol is preferably 1g:40~60mL. In the present invention, adding the aqueous solution of the polyol to the organic solution containing the resin can strengthen the boric acid and improve the accuracy of the detection.
[0055] After obtaining the product to be detected, the present invention drips an indicator into the product to be detected, and titrates with a sodium hydroxide standard solution until the solution turns pink, which is the titration end point, and records the volume of the sodium hydroxide standard solution consumed by the titration, which is recorded as V1. In the present invention, the indicator is preferably one of phenolphthalein, a mixed indicator of thymol blue and cresol red, and a mixed indicator of thymol blue and phenolphthalein, and is more preferably a phenolphthalein indicator. In the present invention, the concentration of the sodium hydroxide standard solution is 0.1~1mol / L. In the present invention, the calibration method of the sodium hydroxide standard solution is preferably:
[0056] a. Mix 0.15-0.2g potassium hydrogen phthalate with 50-100mL deionized water, add 3-5 drops of phenolphthalein indicator, and titrate with the sodium hydroxide solution to be calibrated until the solution turns pink, which is the titration endpoint;
[0057] b. After the titration is terminated, calculate the concentration of the sodium hydroxide solution. The specific formula is:
[0058] c=1000m / 204.2V;
[0059] in:
[0060] m is the weight of potassium hydrogen phthalate, in g;
[0061] V is the volume of the sodium hydroxide solution to be calibrated consumed in the titration, in mL;
[0062] 204.2 is the molar mass of potassium hydrogen phthalate, in g / moL.
[0063] In the present invention, in order to further improve the accuracy of detection, it is preferred to use an epoxy resin without boric acid for a blank test for comparison. The specific dissolution, mixing, and titration methods are the same as the steps 1) to 3) of the epoxy resin to be tested containing boric acid. After the titration is completed, the volume of the sodium hydroxide standard solution consumed in the titration is recorded and recorded as V0;
[0064] Combined with the blank test, the content of solid boric acid in the epoxy resin is calculated. The specific formula is:
[0065] W=[(61.83*c*(V1-V0)) / 1000m / s]*100%;
[0066] Wherein: V0 is the volume of sodium hydroxide standard solution consumed in titration of epoxy resin without boric acid.
[0067] In order to further illustrate the present invention, the technical solutions provided by the present invention are described in detail below in conjunction with embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0068] Example 1
[0069] Weigh 2.0000g of liquid MDI modified resin (containing 0.4% boric acid) and place it in a beaker. Use a pipette to transfer 10mL of chloroform into the beaker and stir to dissolve to obtain an organic solution containing the resin. Measure 100mL of glycerol and 100mL of water and mix to obtain an aqueous solution of polyols. Pour the aqueous solution of polyols into the beaker containing the organic solution of the resin, stir, let stand to separate, extract the boric acid into the aqueous phase, add 5 drops of phenolphthalein indicator to the separated aqueous phase, and titrate with 0.01mol / L sodium hydroxide standard solution until the solution turns pink, which is the titration endpoint. Record the volume as V1.
[0070] Weigh 2.0000g of liquid MDI modified resin (without boric acid) as a blank, place it in a beaker, pipette 10mL of chloroform into the beaker, stir and dissolve to obtain a blank control solution. Measure 100mL of glycerol and 100mL of water to mix to obtain a polyol aqueous solution, inject the polyol aqueous solution into the beaker containing the blank control solution, stir, stand and separate, add 5 drops of phenolphthalein indicator to the separated aqueous phase, and titrate with 0.01mol / L sodium hydroxide standard solution until the solution turns pink, which is the titration endpoint, and record the volume as V0.
[0071] Example 2
[0072] Weigh 2.0000g of liquid MDI modified resin (containing 0.3% boric acid) and place it in a beaker. Use a pipette to transfer 20mL of tetrahydrofuran into the beaker and stir to dissolve to obtain an organic solution containing the resin. Measure 100mL of mannitol and mix with 500mL of water to obtain an aqueous solution of polyols. Inject the aqueous solution of polyols into the beaker containing the organic solution of the resin, stir, let stand to separate, extract the boric acid into the aqueous phase, add 5 drops of phenolphthalein indicator to the separated aqueous phase, and titrate with 0.01mol / L sodium hydroxide standard solution until the solution turns pink, which is the titration endpoint. Record the volume as V1.
[0073] Weigh 2.0000g of liquid MDI modified resin (without boric acid) as a blank, place it in a beaker, pipette 20mL of tetrahydrofuran into the beaker, stir and dissolve to obtain a blank control solution. Measure 100mL of mannitol and 500mL of water to mix to obtain a polyol aqueous solution, inject the polyol aqueous solution into the beaker containing the blank control solution, stir, stand and separate, add 5 drops of phenolphthalein indicator to the separated aqueous phase, and titrate with 0.01mol / L sodium hydroxide standard solution until the solution turns pink, which is the titration endpoint, and record the volume as V0.
[0074] Example 3
[0075] Weigh 2.0000g of liquid MDI modified resin (containing 0.2% boric acid) and place it in a beaker. Use a pipette to transfer 40mL of dimethylformamide into the beaker and stir to dissolve to obtain an organic solution containing the resin. Measure 100mL of glycerol and 100mL of water and mix them to obtain an aqueous solution of polyols. Inject the aqueous solution of polyols into the beaker containing the organic solution of the resin, stir, let stand to separate, extract the boric acid into the aqueous phase, add 5 drops of thymol blue and cresol red mixed indicator to the separated aqueous phase, and titrate with 0.01mol / L sodium hydroxide standard solution until the solution turns pink, which is the titration end point. Record the volume as V1.
[0076] Weigh 2.0000g of liquid MDI modified resin (without boric acid) as a blank, place it in a beaker, pipette 40mL of dimethylformamide into the beaker, stir to dissolve, and obtain a blank control solution. Measure 100mL of glycerol and 100mL of water to mix to obtain a polyol aqueous solution, inject the polyol aqueous solution into the beaker containing the blank control solution, stir, and stand to separate. Add 5 drops of thymol blue and cresol red mixed indicator to the separated aqueous phase, and titrate with 0.01mol / L sodium hydroxide standard solution until the solution turns pink, which is the titration endpoint, and record the volume as V0.
[0077] The boric acid content in the epoxy resins of Examples 1 to 3 is specifically shown in Table 1.
[0078] Table 1
[0079]
[0080] Among them, solid boric acid content = average value of liquid boric acid content / resin solid content
[0081] It can be seen from Table 1 that the method provided by the present invention has good repeatability and high accuracy.
[0082] Comparative Example 1
[0083] The samples to be tested in Examples 1 to 3 (MDI modified epoxy resin (containing 0.4% boric acid), MDI modified epoxy resin (containing 0.3% boric acid), MDI modified epoxy resin (containing 0.2% boric acid)) were sent to a third-party testing company for testing using the ICP method. The specific test results are shown in Table 2:
[0084] Table 2
[0085]
[0086] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for determining the content of boric acid in epoxy resin, characterized in that: The steps include: 1) Mix the epoxy resin to be tested and the solvent to dissolve the epoxy resin in the solvent to obtain an organic solution containing the resin; The solvent is chloroform, tetrahydrofuran, acetone, butanone, methyl ethyl ketone, dioxane, toluene, diethylene glycol dimethyl ether or dimethylformamide; The epoxy resin to be detected is a liquid epoxy resin; 2) Mixing a polyol aqueous solution with an organic solution containing a resin, extracting boric acid into the aqueous phase, and performing phase separation to obtain a sample to be tested; the polyol is glycerol or mannitol; 3) Add indicator to the sample to be tested and titrate with sodium hydroxide standard solution until the solution turns pink, which is the titration end point. Record the volume of sodium hydroxide standard solution consumed in the titration, which is recorded as V1; 4) Calculate the content of solid boric acid in epoxy resin. The specific formula is: W=[(61.83*c*V1) / 1000m / s]*100%; Where: W is the content of solid boric acid in epoxy resin, unit is %; c is the concentration of sodium hydroxide standard solution, in mol / L; m is the mass of the epoxy resin sample to be tested, in g; s is the solid content of epoxy resin, unit is %; 61.83 is the molar mass of boric acid in g / mol.
2. The method for measuring the content of boric acid in epoxy resin according to claim 1, characterized in that: The method further comprises performing a blank test using an epoxy resin that does not contain boric acid, wherein the specific operations are the same as steps 1) to 3) in claim 1, and recording the volume of the sodium hydroxide standard solution consumed in the titration after the titration is completed, which is recorded as V0; Combined with the blank test, the content of solid boric acid in the epoxy resin is calculated. The specific formula is: W=[(61.83*c*(V1-V0)) / 1000m / s]*100%; Wherein: V0 is the volume of sodium hydroxide standard solution consumed in titration of epoxy resin without boric acid.
3. The method for measuring the content of boric acid in epoxy resin according to claim 1, characterized in that: The mass volume ratio of the epoxy resin to be tested and the solvent in step 1) is 0.1-0.5 g: 2.5-40 mL.
4. The method for measuring the content of boric acid in epoxy resin according to claim 1, characterized in that: The mass volume ratio of the epoxy resin to be tested to the polyol is 1 g:40-60 mL.
5. The method for measuring the content of boric acid in epoxy resin according to claim 1, characterized in that: In step 2), the volume ratio of the polyol to water in the aqueous solution of the polyol is 1:1-5.
6. The method for determining the content of boric acid in epoxy resin according to claim 1, characterized in that: The polyol in step 2) is glycerol.
7. The method for determining the content of boric acid in epoxy resin according to claim 1, characterized in that: The indicator in step 3) is one of phenolphthalein, a mixed indicator of thymol blue and cresol red, and a mixed indicator of thymol blue and phenolphthalein.
8. The method for determining the content of boric acid in epoxy resin according to claim 1, characterized in that: The concentration of the sodium hydroxide standard solution in step 3) is 0.01-0.1 mol / L; The calibration method of the sodium hydroxide standard solution is: a. Mix 0.15-0.2g potassium hydrogen phthalate with 50-100mL deionized water, add 3-5 drops of phenolphthalein indicator, and titrate with the sodium hydroxide solution to be calibrated until the solution turns pink, which is the titration endpoint; b. After the titration is terminated, calculate the concentration of the sodium hydroxide solution. The specific formula is: c=1000m / 204.2V; in: m is the weight of potassium hydrogen phthalate, in g; V is the volume of the sodium hydroxide solution to be calibrated consumed in the titration, in mL; 204.2 is the molar mass of potassium hydrogen phthalate, in g / moL.
Citation Information
Patent Citations
Method for detecting benzoic acid content in Kushen compound salicylic acid powder
CN105021752A
Method for determining 22 impurity elements in nuclear-grade phenolic resin
CN106932381A