Method for evaluating hydrophobic homogeneity of hydrophobic concrete
Through the methods of soaking, cutting, spraying and image processing of the chloride ion solution, the simplicity and accuracy of the evaluation of hydrophobic homogeneity of hydrophobic concrete is solved, and the construction quality is effectively controlled.
Patent Information
- Application Number
- CN202410818623.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-24
- Publication Date
- 2024-11-05
AI Technical Summary
The prior art is difficult to evaluate the hydrophobic homogeneity of hydrophobic concrete in a simple and accurate manner, resulting in difficulty in controlling construction quality.
The hydrophobic homogeneity is determined by measuring and analyzing the chloride ion permeability area of hydrophobic concrete by soaking, cutting, spraying of silver ion salt solution, image processing and statistical analysis.
It provides a simple, highly operable and highly accurate hydrophobic homogeneity evaluation method for hydrophobic concrete, which can effectively judge the hydrophobic homogeneity between construction sections and batches, and realize quantitative evaluation and control of construction quality.
Smart Images

Figure CN118896880A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of building materials, and in particular to a method for evaluating the hydrophobic homogeneity of hydrophobic concrete. Background Art
[0002] Concrete is widely used in engineering construction due to its wide range of material sources, low price, and strong plasticity. Since the service environment of concrete is relatively complex, in order to extend the service life of reinforced concrete structures in harsh service environments, technicians proposed the concept of hydrophobic concrete and applied it in actual projects.
[0003] Hydrophobic concrete can significantly improve the waterproof performance and surface self-cleaning performance of concrete, prevent the accumulation of corrosive substances on the concrete surface, and significantly extend the service life of reinforced concrete structures.
[0004] Hydrophobic concrete is mainly prepared by surface hydrophobic modification and overall hydrophobic modification.
[0005] Surface hydrophobic modification is to spray or brush the hydrophobic agent on the concrete surface to form a hydrophobic layer on the concrete surface to achieve the purpose of waterproofing. However, when construction workers perform spraying or brushing construction, due to construction technology, operation level, equipment differences, etc., the construction will be uneven, resulting in uneven distribution of hydrophobicity of surface hydrophobic concrete, uneven penetration depth of hydrophobic substances, and the formation of weak areas on the concrete surface, which reduces the durability and service life of the concrete structure in this area.
[0006] Overall hydrophobic modification is to add hydrophobic agent directly to fresh concrete in a certain proportion to make the pore wall structure of concrete hydrophobic and prevent the intrusion of water and harmful substances. When performing overall hydrophobic modification, you may face problems such as raw material condensation agglomeration and raw material floating, which may lead to hydrophobic unevenness.
[0007] At present, the contact angle of the concrete surface is usually used to evaluate the hydrophobicity and hydrophobic homogeneity of concrete. However, the measurement of the contact angle requires the use of professional instruments and equipment, has high requirements on the roughness of the sample surface, the operation process is relatively cumbersome, and testing multiple points takes a long time.
[0008] In summary, there is an urgent need for a simple and operational evaluation method for judging the hydrophobic homogeneity of hydrophobic concrete, which can be used for the evaluation and quality control of the hydrophobic homogeneity of cast-in-place hydrophobic concrete at construction sites or the concrete after surface hydrophobic treatment of completed structures. Summary of the invention
[0009] The purpose of the present invention is to provide a method for evaluating the hydrophobic homogeneity of concrete which is simple, highly operable and highly accurate.
[0010] In order to achieve the above object, the present invention provides a method for evaluating the hydrophobic homogeneity of hydrophobic concrete, the method comprising:
[0011] (1) using a chloride ion-containing solution I to immerse any hydrophobic surface of n hydrophobic concrete cubic blocks of test samples P to obtain an intermediate sample I;
[0012] Wherein, n≥6 and n is an integer;
[0013] (2) cutting the intermediate sample I in a direction perpendicular to the soaking surface so that the chloride ion permeation surface is completely exposed, thereby obtaining an intermediate sample II;
[0014] (3) spraying the cut surface of the intermediate sample II with a salt solution containing silver ions to obtain an intermediate sample III;
[0015] (4) photographing the sprayed surface of the intermediate sample III with a camera to obtain a first image for recording;
[0016] Controlling the magnification of the camera and the distance between the camera and the sprayed surface so that the sprayed surface is completely photographed in the first image, and the area of the sprayed surface in the first image is not less than 75% of the total area of the first image, and the shooting conditions of the n hydrophobic concrete cubic block samples P to be tested are the same;
[0017] (5) using image processing software to analyze and process the first image to determine the chloride ion penetration area; dividing the chloride ion penetration area into four equal parts along the second direction, taking the middle two equal parts as the analysis area; dividing the analysis area into at least 10 test areas of equal width along the first direction, and the width of any test area is 0.5 mm-1.5 mm, and measuring to obtain the area of each test area;
[0018] The first direction is a vertical direction from the chloride ion penetration area in the first image to the non-chloride ion penetration area; the second direction is a direction perpendicular to the first direction;
[0019] (6) Using SPSS software to determine whether the area distribution of the test area in each hydrophobic concrete cubic block sample P conforms to the normal distribution and whether the area of the test area in n hydrophobic concrete cubic block samples P conforms to the homogeneity of variance;
[0020] When the area distribution of all the test areas conforms to the normal distribution and the homogeneity of variance, a one-way ANOVA test is performed to obtain a p value; if the p value is ≥ 0.05, the hydrophobic homogeneity of the hydrophobic concrete cube sample P to be tested is evaluated to be good; if the p value is < 0.05, the hydrophobic homogeneity of the hydrophobic concrete cube sample P to be tested is evaluated to be poor;
[0021] When the area distribution of all the test areas does not conform to the normal distribution and / or does not conform to the homogeneity of variance, the Kruskal-Wallis test is used to calculate the Kruskal-Wallis statistic and obtain the p-value; if the p-value is ≥ 0.05, the hydrophobic homogeneity of the hydrophobic concrete cube sample P to be tested is evaluated to be good; if the p-value is < 0.05, the hydrophobic homogeneity of the hydrophobic concrete cube sample P to be tested is evaluated to be poor.
[0022] The method for evaluating the hydrophobic homogeneity of hydrophobic concrete provided by the present invention is simple to operate and has high accuracy, and can judge the hydrophobic homogeneity of hydrophobic concrete from different construction sections and different batches of cast-in-place hydrophobic concrete, thereby achieving the purpose of quantitative evaluation and quality control of construction quality. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 is a schematic diagram of an image obtained after the first image is analyzed and processed by Image J software in the present invention;
[0024] Figure 2 It is a flow chart of the present invention using SPSS software inspection. DETAILED DESCRIPTION
[0025] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0026] As mentioned above, the present invention provides a method for evaluating the hydrophobic homogeneity of hydrophobic concrete, the method comprising:
[0027] (1) using a chloride ion-containing solution I to immerse any hydrophobic surface of n hydrophobic concrete cubic blocks of test samples P to obtain an intermediate sample I;
[0028] Wherein, n≥6 and n is an integer;
[0029] (2) cutting the intermediate sample I in a direction perpendicular to the soaking surface so that the chloride ion permeation surface is completely exposed, thereby obtaining an intermediate sample II;
[0030] (3) spraying the cut surface of the intermediate sample II with a salt solution containing silver ions to obtain an intermediate sample III;
[0031] (4) photographing the sprayed surface of the intermediate sample III with a camera to obtain a first image for recording;
[0032] Controlling the magnification of the camera and the distance between the camera and the sprayed surface so that the sprayed surface is completely photographed in the first image, and the area of the sprayed surface in the first image is not less than 75% of the total area of the first image, and the shooting conditions of the n hydrophobic concrete cubic block samples P to be tested are the same;
[0033] (5) using image processing software to analyze and process the first image to determine the chloride ion penetration area; dividing the chloride ion penetration area into four equal parts along the second direction, taking the middle two equal parts as the analysis area; dividing the analysis area into at least 10 test areas of equal width along the first direction, and the width of any test area is 0.5 mm-1.5 mm, and measuring to obtain the area of each test area;
[0034] The first direction is a vertical direction from the chloride ion penetration area in the first image to the non-chloride ion penetration area; the second direction is a direction perpendicular to the first direction;
[0035] (6) Using SPSS software to determine whether the area distribution of the test area in each hydrophobic concrete cubic block sample P conforms to the normal distribution and whether the area of the test area in n hydrophobic concrete cubic block samples P conforms to the homogeneity of variance;
[0036] When the area distribution of all the test areas conforms to the normal distribution and the homogeneity of variance, a one-way ANOVA test is performed to obtain a p value; if the p value is ≥ 0.05, the hydrophobic homogeneity of the hydrophobic concrete cube sample P to be tested is evaluated to be good; if the p value is < 0.05, the hydrophobic homogeneity of the hydrophobic concrete cube sample P to be tested is evaluated to be poor;
[0037] When the area distribution of all the test areas does not conform to the normal distribution and / or does not conform to the homogeneity of variance, the Kruskal-Wallis test is used to calculate the Kruskal-Wallis statistic and obtain the p-value; if the p-value is ≥ 0.05, the hydrophobic homogeneity of the hydrophobic concrete cube sample P to be tested is evaluated to be good; if the p-value is < 0.05, the hydrophobic homogeneity of the hydrophobic concrete cube sample P to be tested is evaluated to be poor.
[0038] In the present invention, the p value obtained for the one-way ANOVA test is the value corresponding to the "significance value" line in the SPSS software output results; the p value obtained for the Kruskal-Wallis test is the value corresponding to the "asymptotic significance" line in the SPSS software output results.
[0039] The present invention Figure 1 A schematic diagram of an image obtained after analyzing and processing the first image using Image J software is provided.
[0040] The present invention Figure 2 A flowchart of the test using SPSS software is provided in .
[0041] Preferably, in step (1), the length, width and height of the hydrophobic concrete cube sample P to be tested are independently 30 mm to 50 mm.
[0042] Preferably, when the sample P to be tested is a hydrophobic concrete with overall hydrophobic modification, before the immersion treatment, epoxy resin is first used to mask any five surfaces of the sample P to be tested. The inventors of the present invention have found that in this preferred case, the method provided by the present invention is more accurate in determining the hydrophobic homogeneity of the hydrophobic concrete.
[0043] It should be noted that, in the present invention, when the sample P to be tested is a hydrophobic concrete with surface hydrophobic modification, only one surface is a hydrophobic surface, and there is no need to shield the non-hydrophobic surface before the immersion treatment.
[0044] In the present invention, the “area distribution of all the test areas conforms to both normal distribution and homogeneity of variance” in step (6) means that the area of the test area of each hydrophobic concrete cubic block sample P to be tested conforms to normal distribution, and the areas of the test areas of the n hydrophobic concrete cubic blocks sample P to be tested conform to homogeneity of variance as a whole.
[0045] Preferably, in step (1), the concentration of chloride ions in the solution I is 0.513-0.856 mol / L.
[0046] Preferably, in step (1), the solution I is a sodium chloride solution and / or a potassium chloride solution.
[0047] Preferably, in step (1), the soaking treatment is carried out at a temperature of 20-25°C and for a time of 24h-168h.
[0048] Preferably, in step (3), the concentration of silver ions in the silver ion-containing salt solution is 0.01-0.1 mol / L.
[0049] According to a preferred specific implementation manner, the spraying process is completed within 5 minutes after the cutting process.
[0050] In step (3), the amount of the salt solution is controlled so that the chloride ions on the cut surface of the intermediate sample II are completely precipitated.
[0051] Preferably, in step (3), the sample after the spraying treatment is left to stand to obtain an intermediate sample III.
[0052] Preferably, the static treatment time is 10-20 minutes.
[0053] Preferably, in step (4), the camera is a fixed camera.
[0054] In the present invention, the shooting is to make the sprayed surface of the intermediate sample III completely fall into the screen of the camera.
[0055] Preferably, in step (5), the image is analyzed and processed by Image J software to determine the chloride ion penetration area.
[0056] In the present invention, the analysis process refers to distinguishing the chloride ion permeation area and the non-permeation area according to the difference in color.
[0057] According to a preferred specific implementation, in step (6), the single-sample Kolmogorov-Smirnov test in the SPSS software is used to test whether the distribution of the area of the test area conforms to the normal distribution, and the Levene test in the SPSS software is used to test whether the distribution of the area of the test area conforms to the homogeneity of variance.
[0058] Preferably, the hydrophobic concrete cube sample P to be tested is an overall hydrophobic modified hydrophobic concrete.
[0059] According to a preferred embodiment, the overall hydrophobic modified hydrophobic concrete is prepared by a method comprising the following steps:
[0060] S1: In the presence of water, cement, river sand and hydrophobic modified liquid are mixed and stirred to obtain slurry I;
[0061] S2: The slurry I is vibrated, coated, demolded and cured in a mold in sequence to obtain an overall hydrophobic modified hydrophobic concrete.
[0062] The present invention has no special requirements on the type of water. For example, the water may be deionized water or ultrapure water, and those skilled in the art may select the water according to their needs.
[0063] Preferably, in step S1, the hydrophobic modification liquid is a stearic acid hydrophobic modification liquid.
[0064] Preferably, the stearic acid hydrophobically modified liquid is octadecanoic acid (stearic acid) emulsion.
[0065] The present invention has no special requirements for the mixing and stirring conditions. It only requires that the water, cement, river sand and hydrophobic modified liquid be completely and evenly stirred. Those skilled in the art can make the selections as needed.
[0066] Preferably, in step S1, the weight ratio of the cement to the river sand is 1:1.8-2.2.
[0067] Preferably, in step S2, the demoulding is performed 24h-48h after the lamination.
[0068] Preferably, in step S2, the curing treatment conditions include: temperature of 18-22°C, humidity of 95-100%, and time of 624h-720h.
[0069] The present invention has no special requirements for the selection of the mold, and those skilled in the art can select it according to needs.
[0070] It should be noted that in step S2, there is no special requirement for the vibration, and it is only necessary to remove the bubbles in the slurry I in the mold. Those skilled in the art can make a choice according to needs.
[0071] It should be noted that, in step S2, the coating refers to covering the slurry I with a layer of plastic film to prevent the water in the slurry I from volatilizing.
[0072] The present invention will be described in detail below by way of examples. In the following examples, unless otherwise specified, the instruments, reagents, materials, etc. involved are all conventional instruments, reagents, materials, etc., which can be obtained through regular commercial channels. Among them, unless otherwise specified, the reagents used are all commercially available analytically pure products.
[0073] Cement: purchased from China Building Materials Science Research Institute Co., Ltd., brand P.I.42.5.
[0074] River sand: purchased from Xiamen Aceo Standard Sand Co., Ltd., brand name is standard sand.
[0075] Stearic acid hydrophobic modified liquid: Octadecanoic acid (stearic acid) emulsion was purchased from Luoyang Yefang New Material Technology Co., Ltd. with the brand name PETS.
[0076] Sodium chloride solution: concentration is 0.856 mol / L.
[0077] Silver nitrate solution: concentration is 0.01mol / L.
[0078] Preparation Example A:
[0079] The method for preparing the overall hydrophobic modified hydrophobic concrete comprises the following steps:
[0080] S1: In the presence of 48.14 g of deionized water, 100 g of cement, 200 g of river sand and 2.86 g of hydrophobic modification liquid were mixed and stirred to obtain slurry I;
[0081] S2: The slurry I was vibrated and coated (covered with a layer of plastic film) in a mold of 40 mm×40 mm×160 mm in sequence, and then demolded and cured (temperature of 20° C., humidity of 98%, time of 672 h) after 24 hours to obtain an overall hydrophobic modified hydrophobic concrete, named hydrophobic concrete T1.
[0082] Preparation Example B:
[0083] The hydrophobic concrete T1 obtained in the above preparation example A was cut into 40 mm × 40 mm × 40 mm cubic blocks (a total of 24 were prepared for standby use) using a cutting machine, and placed in an oven at 60°C to dry to constant weight, and then any five faces of each cubic block were masked with epoxy resin. After the epoxy resin hardened, the hydrophobic concrete cubic block sample P to be tested was obtained (and numbered as P1-P12).
[0084] Example 1
[0085] In this embodiment, 12 hydrophobic concrete cubic block test samples P (numbered P1-P12) in Preparation Example B are used for evaluation, specifically including:
[0086] (1) Sodium chloride solution was used to immerse the hydrophobic surfaces (unshielded sides) of 12 hydrophobic concrete cubes (samples P) for 72 hours at a temperature of 23° C. to obtain intermediate samples I;
[0087] (2) cutting the intermediate sample I in a direction perpendicular to the soaking surface so that the chloride ion permeation surface is completely exposed, thereby obtaining an intermediate sample II;
[0088] (3) spraying and standing the cut surface of the intermediate sample II with a silver nitrate solution (15 min) to obtain an intermediate sample III;
[0089] (4) photographing the sprayed surface of the intermediate sample III with a fixed camera to obtain a first image for recording;
[0090] Controlling the magnification of the camera and the distance between the camera and the sprayed surface so that the sprayed surface is completely photographed in the first image, and the area of the sprayed surface in the first image is 80% of the total area of the first image, and the shooting conditions of the 12 hydrophobic concrete cubic block samples P to be tested are the same;
[0091] (5) Using Image J software to analyze and process the first image to determine the chloride ion penetration area; dividing the chloride ion penetration area into four equal parts along the second direction (see Figure 1 , each divided into L / 4), take the middle two equal parts ( Figure 1 The analysis area is divided into 20 test areas of equal width along the first direction, and the width of any test area is 1 mm, and the area X of each test area is obtained by measuring. ij (i is the specimen number, j is the area of the jth trapezoid of specimen i) The areas of the 20 test areas in all the hydrophobic concrete cubic blocks to be tested samples P are shown in Table 1 below;
[0092] Figure 1 This is a schematic diagram of an image obtained after analyzing and processing the first image using Image J software. Figure 1 The medium dark grey part represents the non-permeable area, and the light grey part represents the chloride ion permeable area; Figure 1 The area with vertical lines in the middle is the analysis area.
[0093] Table 1
[0094] P1 P2 P3 P4 P5 P6 P7 P8 P9 P10 P11 P12 17.621 19.926 20.749 17.253 18.533 19.354 16.548 19.045 18.487 20.749 17.353 16.531 17.457 20.386 20.941 16.829 16.784 18.961 17.053 20.136 17.632 18.329 16.355 15.684 17.071 18.505 21.172 16.944 17.07 17.75 16.486 18.34 15.485 16.046 17.589 17.138 15.554 16.855 20.903 16.944 15.785 16.653 17.381 17.655 16.303 15.355 16.574 17.908 15.23 16.932 20.403 18.442 15.16 15.893 16.055 16.51 17.335 15.432 14.335 16.355 16.822 15.895 20.403 18.942 16.212 16.335 14.387 15.483 14.321 19.978 16.798 17.256 16.213 13.785 19.75 19.365 16.893 14.356 12.159 16.335 16.534 21.898 15.145 16.253 16.126 14.935 19.174 21.517 18.341 15.478 13.122 15.487 18.785 15.052 13.283 15.388 17.477 14.361 18.098 19.058 19.046 14.354 14.358 14.336 15.658 13.861 15.377 13.212 15.799 17.47 17.842 18.174 20.746 13.832 15.149 13.261 14.353 15.976 16.013 14.941 15.266 17.853 16.302 18.02 18.331 12.861 16.047 12.834 16.478 15.052 17.834 15.835 15.139 15.128 16.177 17.405 15.941 13.628 17.073 14.327 15.388 13.628 18.253 17.034 13.867 14.897 15.612 17.445 13.867 15.487 16.356 15.782 16.241 16.078 18.554 16.041 15.55 14.936 14.026 17.636 14.356 16.48 15.214 16.487 18.335 18.325 19.065 15.891 16.186 15.09 14.759 15.792 16.035 17.384 16.883 17.292 19.358 16.755 20.353 16.654 16.371 15.281 14.179 15.368 17.841 16.689 17.057 16.868 16.839 15.186 18.487 16.879 16.002 16.05 13.794 15.754 18.332 17.316 17.94 17.024 16.577 16.714 17.548 18.363 17.415 17.546 14.755 16.104 19.065 16.046 18.348 17.324 18.352 17.944 16.756 20.457 16.992 20.041 14.755 16.944 17.384 18.052 19.991 18.442 19.52 18.541 16.055 19.483 18.525 17.699 15.677 16.791 16.616 17.35 21.384 19.291 20.403 19.273 15.677 18.355
[0095] (6) According to Figure 2The test flow chart shown in the figure is as follows. The areas of all the test areas of the test samples P of each hydrophobic concrete cube are imported into the SPSS software. The areas are grouped according to the numbers of the test samples P. For example, the 20 areas corresponding to the number P1 are group 1, and the 20 areas corresponding to the number P2 are group 2, for a total of 12 groups. The single-sample Kolmogorov-Smirnov test in the SPSS software is used to test whether the areas of the test areas in each group conform to the normal distribution (specific operation: use the "Analysis" function in the menu bar, select "Nonparametric Test" in the drop-down menu, and select "Single Sample" in the submenu. In the pop-up dialog box, select "Custom Test" under the "Settings" column, and check "Test the measured distribution and the hypothesized distribution (Kolmogorov-Smirnov test)", and in the options Select "normal" as the assumed distribution; enter the area of the test area of the 12 hydrophobic concrete cubes to be tested in Table 1 into the "test field", and click "run" to complete the test. ), and use the Levene test in SPSS software to test whether the area of the test area in all groups meets the variance homogeneity (specific operation: select "analysis" in the SPSS menu bar, select "compare means" in the drop-down menu, and select "single factor ANOVA test" in the submenu, click "options" in the pop-up dialog box, and select the "variance homogeneity test" option, fill the group column into "factor (F)", fill the data of the area of the test area of the hydrophobic concrete cubes to be tested into "dependent variable list (E)", and click OK to complete the analysis.), the results are shown in Table 2.
[0096] Table 2
[0097]
[0098] It can be seen from Table 2 that the area of the test area in each hydrophobic concrete cubic block sample P conforms to the normal distribution, but the area of the test area in the 12 hydrophobic concrete cubic block samples P does not conform to the homogeneity of variance. At this time, the Kruskal-Wallis test is used (specific operation: first propose the null hypothesis and the alternative hypothesis, the null hypothesis: the median penetration depth of all hydrophobic concrete cubic block samples is equal, the alternative hypothesis: the median penetration depth of at least two hydrophobic concrete cubic block samples is not equal, use the "Analyze" in the menu bar of SPSS software, in the drop-down menu Select "Nonparametric Test" in the pop-up menu, select "K Independent Samples" in the "Old Dialog Box" in the sub-dialog box, add the data in the "Group" column to the "Grouping Variable" option, and fill in the minimum value 1 and the maximum value 12 (the serial number of the largest group) in the Define Range box, add the data in the area column to the "Test Variable List", check the "Kruskal-Wallis H (K)" option in the Test Type box, and click "OK" to complete the analysis. ), calculate the Kruskal-Wallis statistic, and obtain the p value corresponding to the "Asymptotic Significance" line in the SPSS software output results;
[0099] The obtained p value is 0.604, that is, the p value>0.05, therefore, it is evaluated that the hydrophobic homogeneity of the hydrophobic concrete cube sample P is good.
[0100] In the present invention, the contact angle of the surface of each hydrophobic concrete cube sample P is compared with the above evaluation results to determine the accuracy of the evaluation method provided by the present invention in determining the homogeneity of the hydrophobic concrete, which specifically includes the following steps:
[0101] (i) Twelve hydrophobic concrete cubic blocks of test samples P (numbered P13-P24) obtained in the above-mentioned Preparation Example B were taken and placed in an oven at 60° C. to dry to constant weight, and any one side of each test sample P was polished using 200 mesh (75 μm), 400 mesh (38 μm), 800 mesh (18 μm) and 1200 mesh (5 μm) sandpaper in sequence (the same side was polished each time) to make the polished surface roughness consistent;
[0102] (ii) The contact angle of the polished surface was measured using a JC2000 contact angle meter (Powereach). Twelve points were measured on the polished surface of each test block. The results are shown in Table 3.
[0103] Table 3
[0104]
[0105]
[0106] All contact angle data of the hydrophobic concrete cube test samples P13-P24 were imported into SPSS software, and grouped according to the serial numbers of the test samples P13-P24. The single-sample Kolmogorov-Smirnov test in SPSS software was used to test whether all contact angles of each test sample conformed to the normal distribution (specific operation: use the "Analysis" function in the menu bar, select "Nonparametric Test" in the drop-down menu, and select "Single Sample" in the submenu. In the pop-up dialog box, select "Custom Test" under the "Settings" column, and check "Test Measured Distribution and Hypothesized Distribution (Kolmogorov-Smirnov Test)", and select "Normal" as the assumed distribution in the options; Table The contact angles of the 12 hydrophobic concrete cubes to be tested are marked in the "Test Field", and the test can be completed by clicking "Run". ), and the Levene test in the SPSS software is used to test whether the contact angles of all the samples to be tested meet the variance homogeneity (specific operation: select "Analysis" in the SPSS menu bar, select "Compare Means" in the drop-down menu, and select "Single-factor ANOVA Test" in the submenu, click "Options" in the pop-up dialog box, and select the "Variance Homogeneity Test" option, fill the group column into "Factor (F)", fill the data of the contact angles of all the samples to be tested into "Dependent Variable List (E)", and click OK to complete the analysis), the results are shown in Table 4.
[0107] Table 4
[0108]
[0109]
[0110] According to the results in Table 4, the "one-way ANOVA test" was used to test the hydrophobic homogeneity of the hydrophobic concrete cube test samples P13-P24.
[0111] Specific operation: Select "Analysis" in the SPSS menu bar, select "Compare Means" in the drop-down menu, and select "One-Way ANOVA Test" in the submenu, fill the group column into "Factor (F)", fill the data of the contact angle of the hydrophobic concrete cube sample to be tested into "Dependent Variable List (E)", and click OK to complete the analysis.
[0112] The p value corresponding to the "Significance Value" line in the SPSS software output result obtained by the "One-Way ANOVA Test" is 0.592>0.05. Therefore, it is determined that the mean values of the contact angles of the tested hydrophobic concrete have no significant changes, that is, the hydrophobic homogeneity is good. This is consistent with the results determined by the evaluation method provided by the present invention.
[0113] It can be seen from the above results that the method for evaluating the hydrophobic homogeneity of hydrophobic concrete provided by the present invention is simple, highly operable and highly accurate, and provides a more intuitive way to judge the hydrophobic uniformity of hydrophobic concrete in the construction field.
[0114] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A method for evaluating the hydrophobic homogeneity of hydrophobic concrete, characterized in that: The method includes: (1) using a chloride ion-containing solution I to immerse any hydrophobic surface of n hydrophobic concrete cubic blocks of test samples P to obtain an intermediate sample I; Wherein, n≥6 and n is an integer; (2) cutting the intermediate sample I in a direction perpendicular to the soaking surface so that the chloride ion permeation surface is completely exposed, thereby obtaining an intermediate sample II; (3) spraying the cut surface of the intermediate sample II with a salt solution containing silver ions to obtain an intermediate sample III; (4) photographing the sprayed surface of the intermediate sample III with a camera to obtain a first image for recording; Controlling the magnification of the camera and the distance between the camera and the sprayed surface so that the sprayed surface is completely photographed in the first image, and the area of the sprayed surface in the first image is not less than 75% of the total area of the first image, and the shooting conditions of the n hydrophobic concrete cubic block samples P to be tested are the same; (5) using image processing software to analyze and process the first image to determine the chloride ion penetration area; dividing the chloride ion penetration area into four equal parts along the second direction, taking the middle two equal parts as the analysis area; dividing the analysis area into at least 10 test areas of equal width along the first direction, and the width of any test area is 0.5 mm-1.5 mm, and measuring to obtain the area of each test area; The first direction is a vertical direction from the chloride ion penetration area in the first image to the non-chloride ion penetration area; the second direction is a direction perpendicular to the first direction; (6) Using SPSS software to determine whether the area distribution of the test area in each hydrophobic concrete cubic block sample P conforms to the normal distribution and whether the area of the test area in n hydrophobic concrete cubic block samples P conforms to the homogeneity of variance; When the area distribution of all the test areas conforms to the normal distribution and the homogeneity of variance, a one-way ANOVA test is performed to obtain a p value; if the p value is ≥ 0.05, the hydrophobic homogeneity of the hydrophobic concrete cube sample P to be tested is evaluated to be good; if the p value is < 0.05, the hydrophobic homogeneity of the hydrophobic concrete cube sample P to be tested is evaluated to be poor; When the area distribution of all the test areas does not conform to the normal distribution and / or does not conform to the homogeneity of variance, the Kruskal-Wallis test is used to calculate the Kruskal-Wallis statistic and obtain the p-value; if the p-value is ≥ 0.05, the hydrophobic homogeneity of the hydrophobic concrete cube sample P to be tested is evaluated to be good; if the p-value is < 0.05, the hydrophobic homogeneity of the hydrophobic concrete cube sample P to be tested is evaluated to be poor.
2. The method according to claim 1, wherein: In step (1), the concentration of chloride ions in the solution I is 0.513-0.856 mol / L.
3. The method according to claim 1 or 2, wherein: In step (1), the solution I is a sodium chloride solution and / or a potassium chloride solution.
4. The method according to claim 1 or 2, wherein: In step (1), the soaking treatment is carried out at a temperature of 20-25°C and for a time of 24h-168h.
5. The method according to claim 1 or 2, wherein: In step (3), the concentration of silver ions in the silver ion-containing salt solution is 0.01-0.1 mol / L.
6. The method according to claim 1 or 2, wherein: The hydrophobic concrete cubic block sample P to be tested is a hydrophobic concrete that has been hydrophobically modified as a whole.
7. The method according to claim 6, wherein: The overall hydrophobic modified hydrophobic concrete is prepared by a method comprising the following steps: S1: In the presence of water, cement, river sand and hydrophobic modified liquid are mixed and stirred to obtain slurry I; S2: The slurry I is vibrated, coated, demolded and cured in a mold in sequence to obtain an overall hydrophobic modified hydrophobic concrete.
8. The method according to claim 7, wherein: In step S1, the hydrophobic modification liquid is a stearic acid hydrophobic modification liquid.
9. The method according to claim 7, wherein: In step S1, the weight ratio of the cement to the river sand is 1:1.8-2.
2.
10. The method according to claim 7, wherein: In step S2, the curing treatment conditions include: temperature of 18-22°C, humidity of 95-100%, and time of 624h-720h.