Electrochromic / capacitive bifunctional thin film material as well as preparation method and application thereof

By preparing a hierarchical layered electrochromic/capacitive dual-functional thin film material on the surface of tungsten trioxide, the problems of low color differentiation and slow reaction speed in the prior art are solved, and a variety of rich color variations and high energy storage performance are achieved.

CN118897426APending Publication Date: 2024-11-05DEZHOU UNIV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411388557.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-08
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

In existing technologies, adding a titanium dioxide layer to the surface of tungsten trioxide materials can only achieve changes in the depth or transparency of a single color, which is not very distinguishable. Furthermore, the reaction speed and cycle stability of the dual-function electrochromic capacitor material are insufficient.

Method used

An electrochromic/capacitive dual-function thin film material with a hierarchical layered structure, comprising a tungsten metal bottom layer, a tungsten trioxide intermediate layer, and a titanium dioxide surface layer, was prepared by magnetron sputtering. The thicknesses are 5–40 nm, 150–210 nm, and 20–40 nm, which are amorphous layers of titanium dioxide, tungsten trioxide, and tungsten metal, respectively, thereby improving electron transport speed and ion diffusion rate.

Benefits of technology

It achieves a rich variety of colors, significantly improves color differentiation and energy storage function, accelerates response speed, enhances cycle stability, has a coloring efficiency of up to 74.2 cm2/C, large capacity, and excellent capacitance rate performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118897426A_ABST
    Figure CN118897426A_ABST
Patent Text Reader

Abstract

The invention discloses an electrochromic / capacitive bifunctional thin film material as well as a preparation method and application thereof, and belongs to the technical field of functional thin film materials. The thin film material comprises a titanium dioxide surface layer with the thickness of 20-40 nm, a tungsten trioxide middle layer with the thickness of 150-210 nm and a metal tungsten bottom layer with the thickness of 20-40 nm. The capacity of the electrochromic / capacitive bifunctional thin film material reaches 20.2-51.5 mF / cm < 2 >, and the capacitance rate capability reaches 58.7%-88.6%; according to the present invention, the visible light can be converted into visible light, the coloring and fading process of various colors can be reversibly performed, the complete coloring and fading time is short, the maximum visible light modulation amplitude can achieve 75%, the coloring efficiency is 42.3-74.2 cm < 2 > / C, and the electric quantity stored by the film can be intuitively and quantitatively determined according to the color variety change of the film during the charging and discharging process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of functional thin film materials, and in particular relates to an electrochromic / capacitive dual-functional thin film material and a preparation method and application thereof. Background Art

[0002] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention, and should not necessarily be regarded as an admission or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art.

[0003] Electrochromic materials have attracted much attention due to their tunable and reversible optical properties (transmittance, absorbance or reflection) under low voltage drive, and are promising materials in many aspects. Pseudocapacitors can store energy by inserting / extracting charges through reversible redox reactions, and are considered to be another promising energy storage technology development direction besides batteries. When a reversible redox reaction with rapid charge transfer occurs in a pseudocapacitor, certain specific electrode materials will undergo an electrochromic process at the same time, including tungsten trioxide materials.

[0004] However, in the prior art, the solution of adding a titanium dioxide layer on the surface of the tungsten trioxide material can only achieve a change in the depth or transparency of a single color, and the distinction is not high. Summary of the invention

[0005] In view of the shortcomings of the prior art, the purpose of the present invention is to provide an electrochromic / capacitive dual-function thin film material and its preparation method and application, which utilizes the inherent properties of inorganic materials tungsten trioxide and titanium dioxide, adds a reflective layer of tungsten material, and prepares a graded layered structure, which can effectively improve the electron transmission speed and ion diffusion rate, accelerate the reaction kinetics process, and not only achieve a rich change in color types and improve color differentiation, but also realize the energy storage function and greatly improve the reaction speed and cycle stability of the electrochromic capacitor dual-function material.

[0006] In order to achieve the above object, the technical solution of the present invention is: In the first aspect, an electrochromic / capacitive dual-function thin film material includes: a titanium dioxide surface layer with a thickness of 5 to 40 nm, a tungsten trioxide middle layer with a thickness of 150 to 210 nm, and a metal tungsten bottom layer with a thickness of 20 to 40 nm; and the metal tungsten, tungsten trioxide and titanium dioxide are all amorphous.

[0007] Optionally, the metal tungsten bottom layer is located on a conductive substrate, and the conductive substrate is ITO conductive glass.

[0008] In a second aspect, the method for preparing the above-mentioned electrochromic / capacitive dual-function thin film material comprises the following steps: S1. Using metal tungsten as a target, DC deposition sputtering is performed on the surface of a conductive substrate to obtain a metal tungsten bottom layer of a set thickness; S2, using metal tungsten as a target, in an oxygen-containing atmosphere, performing DC reactive deposition sputtering on the surface of the metal tungsten bottom layer to obtain a tungsten trioxide intermediate layer of a set thickness; S3. Using titanium dioxide as a target, radio frequency deposition sputtering is performed on the surface of the tungsten trioxide intermediate layer to obtain a titanium dioxide surface layer of a set thickness.

[0009] Optionally, in S1, W with a purity of 99.99% or more is used as the target material.

[0010] Optional, S1, vacuum degree is 6×10 -4 In a chamber below 100 Å / min, DC deposition sputtering is performed in an argon atmosphere.

[0011] Optionally, in S1, during the DC deposition sputtering process, the gas flow rate of argon is 15-25 sccm, the sputtering power is 80-120 W, the sputtering pressure is 0.2-0.25 Pa, the sputtering time is 3-5 min, and the working distance is 10-12 cm.

[0012] Optionally, in S2, W with a purity of 99.99% or more is used as the target material.

[0013] Optional, S2, vacuum degree is 6×10 -4 In a chamber below Pa, DC reactive deposition sputtering is carried out in a mixed atmosphere of oxygen and argon with a volume ratio of 1: (2.5-3).

[0014] Optionally, in S2, during the DC reactive deposition sputtering process, the gas flow rate of argon is 25-30 sccm, the gas flow rate of oxygen is 10-12 sccm, the sputtering power is 80-120 W, the sputtering gas pressure is 0.3-0.35 Pa, the sputtering time is 15-18 min, and the working distance is 10-12 cm.

[0015] Optional, S3, vacuum degree is 6×10 -4 In a chamber below 1.5 Å, RF deposition sputtering is performed in an argon atmosphere.

[0016] Optionally, in S3, TiO2 with a purity of 99.99% or more is used as the target material.

[0017] Optionally, in S3, during the RF deposition sputtering process, the gas flow rate of argon is 15 to 25 sccm, the sputtering power is 80 to 120 W, the sputtering pressure is 0.2 to 0.25 Pa, the sputtering time is 8 to 10 min, and the working distance is 10 to 12 cm.

[0018] In a third aspect, the application of the above-mentioned electrochromic / capacitive dual-function thin film material includes: application in color-changing energy storage devices.

[0019] During the charging and discharging process, the amount of electricity stored in the film material can be intuitively and quantitatively judged by the change in the color type of the film. Compared with the change in color depth or transparency, the color distinction is significantly improved.

[0020] The beneficial effects of the present invention are: 1. The electrochromic / capacitive dual-function thin film material provided by the present invention has a layered structure. On a conductive substrate such as ITO conductive glass, three layers are deposited in sequence, with metal tungsten as the reflective layer, tungsten trioxide as the middle color-changing layer, and titanium dioxide as the surface layer. It can reversibly transform from the initial purple to brown, dark brown, green, dark green and other colors during the reversible storage and release of electricity. It has excellent electrochromic performance, short complete coloring and fading time, visible light modulation amplitude of up to 75%, and coloring efficiency of 42.3~74.2cm 2 / C, during the charging and discharging process, the amount of electricity stored in the film material can be intuitively and quantitatively judged by the change in the color type of the film, which significantly improves the color distinction compared to the change in color depth or transparency.

[0021] 2. In the preparation method of the electrochromic / capacitive dual-function thin film material provided by the present invention, each layer is prepared by magnetron sputtering. The method is simple, stable, and has controllable size and thickness. It is compatible with the existing commercial standard electrochromic process and is conducive to large-scale industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] The accompanying drawings in the specification, which constitute a part of the present invention, are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.

[0023] Figure 1 This is a scanning electron microscope image in Example 1.

[0024] Figure 2 This is the XRD analysis result diagram in Example 1.

[0025] Figure 3 This is the HRTEM analysis result diagram in Example 1.

[0026] Figure 4 This is the reflection spectrum of the thin film material in Example 1.

[0027] Figure 5 Graph showing the reflection spectra of the thin film material at different voltages in Example 1.

[0028] Figure 6 : These are color diagrams of the thin film materials at different voltages in Example 1; (a) is the color change diagram corresponding to 0.1V, (b) is the color change diagram corresponding to 0.0V, (c) is the color change diagram corresponding to -0.1V, (d) is the color change diagram corresponding to -0.2V, (e) is the color change diagram corresponding to -0.3V, (f) is the color change diagram corresponding to -0.4V, (g) is the color change diagram corresponding to -0.5V, and (h) is the CIE color coordinate diagram.

[0029] Figure 7 This is the electrochromic coloring efficiency curve in Example 1.

[0030] Figure 8 This is a chrono current curve diagram in Example 1.

[0031] Fig. 9 This is a graph of the surface capacitance corresponding to different current densities in Example 1.

[0032] Fig.10 This is the charge and discharge curve diagram in Example 1.

[0033] Fig.11 This is a graph of the surface capacitance corresponding to different current densities in Example 2.

[0034] Fig.12 This is the electrochromic coloring efficiency curve in Comparative Example 1.

[0035] Fig.13 This is a graph of the surface capacitance corresponding to different current densities in Comparative Example 1.

[0036] Fig.14 These are the color change diagrams of the thin film materials under different voltages in Comparative Example 2; (a) is the color change diagram corresponding to 0.0V, (b) is the color change diagram corresponding to -0.1V, (c) is the color change diagram corresponding to -0.2V, (d) is the color change diagram corresponding to -0.3V, (e) is the color change diagram corresponding to -0.4V, and (f) is the color change diagram corresponding to -0.5V. DETAILED DESCRIPTION

[0037] It should be noted that the following detailed descriptions are exemplary and are intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.

[0038] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit exemplary embodiments according to the present invention. As used herein, unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. In addition, it should be understood that when the terms "comprising" and / or "including" are used in this specification, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof.

[0039] Example 1 An electrochromic / capacitive dual-function thin film material, the preparation method of which comprises: S1, using W with a purity of more than 99.99% as the target material and ITO conductive glass as the conductive substrate, in a vacuum of 6×10 -4 DC deposition sputtering was carried out in a chamber below 400 Å / s Pa. During the DC deposition sputtering process, the gas flow rate of argon was 20 sccm, the sputtering power was 100 W, the sputtering pressure was 0.2 Pa, the sputtering time was 5 min, and the working distance was 10 cm to obtain a metal tungsten bottom layer.

[0040] S2, using W with a purity of more than 99.99% as the target material, DC reactive deposition sputtering was performed on the metal tungsten substrate. The DC reactive deposition sputtering was performed at a vacuum degree of 6×10 -4 Pa, using an oxygen-argon mixed atmosphere, with an argon gas flow rate of 30sccm, an oxygen gas flow rate of 10sccm, a sputtering power of 100W, a sputtering pressure of 0.3Pa, a sputtering time of 18min, and a working distance of 10cm to obtain a tungsten trioxide intermediate layer.

[0041] S3. Using TiO2 with a purity of more than 99.99% as the target material, radio frequency deposition sputtering is performed on the tungsten trioxide intermediate layer. The protective atmosphere of the radio frequency deposition sputtering is argon, the gas flow rate of argon is 20sccm, the sputtering power is 100W, the sputtering pressure is 0.2Pa, the sputtering time is 10min, the working distance is 10cm, and a titanium dioxide surface layer is obtained.

[0042] The ITO conductive glass was ultrasonically cleaned in acetone, ethanol and deionized water for 20 minutes in sequence before use, and then dried in a vacuum oven for later use.

[0043] Through the above steps S1 to S3, an electrochromic / capacitive dual-function thin film material is obtained, and the surface of the obtained electrochromic / capacitive dual-function thin film material is scanned by electron microscope, and the obtained image is as follows Figure 1 As shown, the surface is smooth and dense, without obvious defects such as cracks.

[0044] The obtained electrochromic / capacitive dual-function thin film material cross section was subjected to XRD analysis, and the results are as follows: Figure 2As shown, W, WO3 and TiO2 were successfully deposited on the ITO glass surface, and W, WO3 and TiO2 were all amorphous.

[0045] The cross section of the obtained electrochromic / capacitive dual-function thin film material was analyzed by high-resolution transmission electron microscopy (HRTEM). The obtained image is as follows: Figure 3 As shown, the thin film material has layered characteristics, and the thickness of the metal tungsten bottom layer is 30nm, the thickness of the tungsten trioxide middle layer is 180nm, and the thickness of the titanium dioxide surface layer is 10nm.

[0046] The obtained electrochromic / capacitive dual-function film samples were analyzed for visible light reflectance spectrum using an Avantis fiber optic spectrometer. Figure 4 As shown in the figure, the metal layer causes the film sample to produce obvious interference resonance in the wavelength range of 380-780 nm, with two interference peaks and one interference valley. Therefore, it is known that some wavelengths of light are absorbed by the film material, while the rest of the light is selectively reflected to the surface of the film material.

[0047] The obtained electrochromic / capacitive dual-function thin film material was used as the working electrode, the silver / silver chloride electrode was used as the reference electrode, and the platinum sheet electrode was used as the counter electrode. The following detection was performed using an electrochemical workstation.

[0048] Using the constant potential polarization method, the prepared electrochromic / capacitive dual-function film samples were subjected to voltages of 0.1 to -0.5 V, including 0.1, 0.0, -0.1, -0.2, -0.3, -0.4 and -0.5 V, and the color of the film material was observed to change. During the color change process, the reflectance spectrum of the material is as follows Figure 5 As shown in Figure 1, the reflectance spectrum shows a significant red shift at the peak position, from 740 nm to 550 nm, thus achieving a very large modulation range (amplitude up to 190 nm). Figure 6 As shown in (a) to (g) in the figure, the sample color changes from the initial purple to brown, dark brown, green, dark green and other colors, showing a rich variety of color types. The corresponding color CIE coordinate diagram is shown in Figure 6 The scatter plots in (h) are shown. Figure 6 The arrow in (h) shows the color change trend during the application of 0.1 to -0.5 V voltage; the scattered points and Figure 5 The voltage values ​​of 0.1, 0.0, -0.1, -0.2, -0.3, -0.4 and -0.5 V correspond one to one. It can be seen that the color of the sample changes from the initial lavender to pink, rose red, light yellow, light green and other colors, showing a rich change in color types.

[0049] (a) to (g) in 6 are photos of real objects, showing the colors under diffuse reflection conditions. The colors are similar to those observed with the naked eye. Figure 6 (h) in the figure is the CIE coordinate diagram. The reflected light is stronger during the test, so the test results are different from the color observed by the naked eye, but both reflect the changes in multiple color types.

[0050] The electrochromic coloring efficiency of the prepared electrochromic / capacitive dual-function film sample was tested, and the electrochromic coloring efficiency (CE) was calculated as follows: ; Where ΔQ is the amount of charge inserted or extracted per unit area of ​​electrochromic material, ΔOD is the change in optical density, and R b is the reflectance in the bleached state, R c is the reflectivity in the colored state. CE can be evaluated by the slope of the ΔOD vs. ΔQ graph. The electrochromic coloring efficiency test results of the electrochromic / capacitive dual-function film sample are shown in Figure 7 As shown, the coloring efficiency is as high as 74.2cm 2 / C.

[0051] The switching dynamics of the electrochromic / capacitive dual-function film sample were studied by chronoamperometry. The initial potential step was set to -0.5 V and the final potential step was set to 0.5 V. The results are shown in Figure 8 As shown in Figure 2, during the period from 0 to 2 s, the current increased from 54.5 mA / cm 2 Down to 0 mA / cm 2 In the time range close to 4 s, the current increases from -27 mA cm −2 Rising to 0 mAcm −2 , indicating that the electrochromic / capacitive dual-function film sample has a higher H + Insertion / uninsertion rate.

[0052] The prepared electrochromic / capacitive dual-function film samples were tested at different current densities by constant current polarization method to obtain the surface capacitance of the electrochromic / capacitive dual-function film samples at different current densities. The results are as follows: Fig. 9 As shown in Figure 2, the surface capacitance gradually decreases with the increase of discharge current density, even at a current density of 1 mA / cm 2 The maximum capacitance is still maintained at 63.1%, further confirming the excellent rate performance of the electrochromic / capacitive dual-function film sample.

[0053] The prepared electrochromic / capacitive dual-function film samples were charged and discharged at 0.1 mA / cm 2 The charge and discharge test results under current density are as follows Fig.10As shown, the discharge surface capacitance obtained reaches 51.5mF / cm 2 .

[0054] The electrochromic / capacitive dual-function thin film material obtained in Example 1 was charged using a constant voltage polarization method to obtain current-time data during the charging process. The charging state (surface charge capacity) of the thin film material was calculated based on the current-time data and the size of the electrochromic / capacitive dual-function thin film material, and the color change was observed with the naked eye: when the electrochromic / capacitive dual-function thin film sample was charged at a voltage of -0.1 V, the surface charge capacity was 0.00117 C / cm 2 , the film sample appears brown; when the electrochromic / capacitive dual-function film sample is charged at a voltage of -0.2 V, the surface charge capacity is 0.00246 C / cm 2 , the film sample appears dark brown; when the electrochromic / capacitive dual-function film sample is charged at a voltage of -0.3 V, the surface charge capacity is 0.00337 C / cm 2 , the film sample appears green; when the electrochromic / capacitive dual-function film sample is charged at a voltage of -0.4 V, the surface charge capacity is 0.00537 C / cm 2 , the film sample appears dark green. That is, as the energy storage increases, the color changes from purple to brown, dark brown, green and dark green. When analyzed using CIE coordinates, the same Figure 6 The corresponding detection result of (g) in .

[0055] It can be seen from the above test results that when the thin film material prepared in the embodiment is applied to energy storage devices (surface capacitance), a fast reaction process can be achieved and for larger ion capacity, the presence of the layered structure is beneficial to the reaction kinetics, and can well buffer the volume change of the electrode during the redox reaction, which is beneficial to the cyclic stability of the material; the thin film material has a wide range of modulation in the visible band, a short reaction time, and a high coloring efficiency; at the same time, it has the characteristics of large capacity and high rate in terms of capacitance; the excellent dual-functional performance is very beneficial to the preparation of energy-saving energy storage devices.

[0056] Example 2 An electrochromic / capacitive dual-function thin film material, the preparation method of which comprises: S1, using W with a purity of more than 99.99% as the target material and ITO conductive glass as the conductive substrate, in a vacuum of 6×10 -4 DC deposition sputtering was carried out in a chamber below 400 Å / s Pa. During the DC deposition sputtering process, the gas flow rate of argon was 20 sccm, the sputtering power was 100 W, the sputtering pressure was 0.2 Pa, the sputtering time was 5 min, and the working distance was 10 cm to obtain a metal tungsten bottom layer.

[0057] S2, using W with a purity of more than 99.99% as the target material, DC reactive deposition sputtering was performed on the metal tungsten substrate. The DC reactive deposition sputtering was performed at a vacuum degree of 6×10 -4 Pa, using an oxygen-argon mixed atmosphere, with an argon gas flow rate of 30sccm, an oxygen gas flow rate of 10sccm, a sputtering power of 100W, a sputtering pressure of 0.3Pa, a sputtering time of 18min, and a working distance of 10cm to obtain a tungsten trioxide intermediate layer.

[0058] S3. Using TiO2 with a purity of more than 99.99% as the target material, radio frequency deposition sputtering is performed on the tungsten trioxide intermediate layer. The protective atmosphere of the radio frequency deposition sputtering is argon, the gas flow rate of argon is 20sccm, the sputtering power is 100W, the sputtering pressure is 0.2Pa, the sputtering time is 20min, the working distance is 10cm, and a titanium dioxide surface layer is obtained.

[0059] The ITO conductive glass was ultrasonically cleaned in acetone, ethanol and deionized water for 10 min in sequence before use, and then dried in a vacuum oven for later use.

[0060] The difference between the preparation method of this embodiment and that of Embodiment 1 is that in S3, the sputtering time is 20 minutes, which is twice as long as that of Embodiment 1.

[0061] It was detected that the thin film material prepared in this embodiment has a layered characteristic, and the thickness of the metal tungsten bottom layer is 30nm, the thickness of the tungsten trioxide middle layer is 180nm, and the thickness of the titanium dioxide surface layer is 20nm.

[0062] The thin film material prepared in this embodiment was tested according to the method of embodiment 1. The results showed that the visible light modulation of the thin film material reached 87.5%, the reaction time was short, and the coloring efficiency was high (42.3 cm 2 / C), large capacity (20.2mF / cm 2 ), high capacitance ratio (88.6%).

[0063] In particular, the surface capacitance diagram of the material under different current densities is as follows: Fig.11 As shown in Figure 2, the surface capacitance gradually decreases with the increase of discharge current density, even at a current density of 1 mA / cm 2 The maximum capacitance is still maintained at 88.6%, which further confirms the excellent rate performance of the electrochromic / capacitive dual-function film sample, which is very beneficial for the preparation of energy-saving energy storage devices.

[0064] Comparative Example 1: A thin film material, the preparation method of which comprises: S1, using W with a purity of more than 99.99% as the target material and ITO conductive glass as the conductive substrate, in a vacuum of 6×10 -4 DC deposition sputtering was carried out in a chamber below 400 Å / s Pa. During the DC deposition sputtering process, the gas flow rate of argon was 20 sccm, the sputtering power was 100 W, the sputtering pressure was 0.2 Pa, the sputtering time was 5 min, and the working distance was 10 cm to obtain a metal tungsten bottom layer.

[0065] S2, using W with a purity of more than 99.99% as the target material, DC reactive deposition sputtering was performed on the metal tungsten substrate. The DC reactive deposition sputtering was performed at a vacuum degree of 6×10 -4 Pa, using an oxygen-argon mixed atmosphere, with an argon gas flow rate of 30sccm, an oxygen gas flow rate of 10sccm, a sputtering power of 100W, a sputtering pressure of 0.3Pa, a sputtering time of 18min, and a working distance of 10cm to obtain a tungsten trioxide intermediate layer.

[0066] The ITO conductive glass was ultrasonically cleaned in acetone, ethanol and deionized water for 10 min in sequence before use, and then dried in a vacuum oven for later use.

[0067] The difference between the preparation method of this comparative example and that of Example 1 is that no titanium dioxide layer is prepared.

[0068] It was detected that the thin film material prepared in this comparative example had a layered characteristic, and the thickness of the metal tungsten bottom layer was 30 nm, and the thickness of the tungsten trioxide layer was 180 nm.

[0069] The film material prepared by this comparative example was tested according to the method of Example 1, and the results were as follows: the coloring efficiency of the film material was low (40.0 cm 2 / C), large capacity (40.8mF / cm 2 ), but the capacitance ratio can only reach (58.7%).

[0070] The electrochromic coloring efficiency of the electrochromic / capacitive dual-function film sample prepared in this comparative example was tested. The electrochromic coloring efficiency test results of the electrochromic / capacitive dual-function film sample are as follows: Fig.12 As shown, the coloring efficiency CE is 40.0 cm 2 / C.

[0071] By constant current polarization method, the prepared electrochromic / capacitive dual-function film sample was tested at different current densities in this comparative example to obtain the surface capacitance of the electrochromic / capacitive dual-function film sample at different current densities. The results are as follows: Fig.13 As shown in Figure 2, the surface capacitance gradually decreases with the increase of discharge current density. 2The maximum capacitance is maintained at 58.7%.

[0072] Comparative Example 2 A thin film material, the preparation method of which comprises: S1. Using W with a purity of more than 99.99% as the target material and ITO conductive glass as the conductive substrate, direct current reactive deposition sputtering was performed on the ITO conductive glass. The direct current reactive deposition sputtering was performed in a vacuum of 6×10 -4 Pa, using an oxygen-argon mixed atmosphere, with an argon gas flow rate of 30sccm, an oxygen gas flow rate of 10sccm, a sputtering power of 100W, a sputtering pressure of 0.3Pa, a sputtering time of 18min, and a working distance of 10cm to obtain a tungsten trioxide intermediate layer.

[0073] S2. Using TiO2 with a purity of more than 99.99% as the target material, radio frequency deposition sputtering is performed on the tungsten trioxide intermediate layer. The protective atmosphere of the radio frequency deposition sputtering is argon, the gas flow rate of argon is 20sccm, the sputtering power is 100W, the sputtering pressure is 0.2Pa, the sputtering time is 10min, and the working distance is 10cm to obtain a titanium dioxide surface layer.

[0074] The ITO conductive glass was ultrasonically cleaned in acetone, ethanol and deionized water for 10 min in sequence before use, and then dried in a vacuum oven for later use.

[0075] The difference between the preparation method of this comparative example and that of Example 1 is that no metal tungsten bottom layer is prepared.

[0076] It was detected that the thin film material prepared in this comparative example had a layered characteristic, and the thickness of the tungsten trioxide middle layer was 180 nm, and the thickness of the titanium dioxide surface layer was 10 nm.

[0077] like Fig.14 As shown in (a) to (f) in the figure, the lower half of the transparent substrate is provided with the thin film material of this comparative example. The thin film material prepared in this comparative example appears to be transparent in appearance when there is no voltage, and has a very high transmittance in the entire visible light spectrum range, and the thin film material has almost no detectable structural color. Using the constant potential polarization method, a voltage of 0 to -0.5V is applied to the prepared thin film material samples, and the thin film material only changes from a colorless and transparent state to blue and the blue gradually deepens. That is: only the depth of a single color can be changed, and changes in multiple colors cannot be achieved, and the distinction is not high. When applied to energy storage devices, only changes in color depth and transparency can occur. The color richness and distinction are obviously not as good as the technical effects of Example 1.

[0078] Through the above embodiments and comparative examples, it can be seen that: in the technical scheme of the present invention, the thickness of the tungsten bottom layer and the titanium dioxide surface layer can affect the performance of the electrochromic / capacitive dual-function thin film material: if there is no tungsten bottom layer, the electrochromic color can only achieve changes in color depth, and the color of the thin film material can only achieve a transition between colorless and blue; and if there is no titanium dioxide surface layer, the coloring efficiency of the thin film material is low and the capacitance rate performance is poor. The technical scheme of Example 1 can be used to obtain the best technical effect.

[0079] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. An electrochromic / capacitive dual-function thin film material, characterized in that: include: A titanium dioxide surface layer with a thickness of 5 to 40 nm, a tungsten trioxide middle layer with a thickness of 150 to 210 nm, and a metal tungsten bottom layer with a thickness of 20 to 40 nm; and the metal tungsten, tungsten trioxide and titanium dioxide are all in amorphous state.

2. The electrochromic / capacitive dual-function thin film material according to claim 1, characterized in that: The metal tungsten bottom layer is located on a conductive substrate, and the conductive substrate is ITO conductive glass.

3. A method for preparing the electrochromic / capacitive dual-function thin film material according to any one of claims 1 to 2, characterized in that: The following steps are involved: S1. Using metal tungsten as a target, DC deposition sputtering is performed on the surface of a conductive substrate to obtain a metal tungsten bottom layer of a set thickness; S2, using metal tungsten as a target, in an oxygen-containing atmosphere, performing DC reactive deposition sputtering on the surface of the metal tungsten bottom layer to obtain a tungsten trioxide intermediate layer of a set thickness; S3. Using titanium dioxide as a target, radio frequency deposition sputtering is performed on the surface of the tungsten trioxide intermediate layer to obtain a titanium dioxide surface layer of a set thickness.

4. The method for preparing the electrochromic / capacitive dual-function thin film material according to claim 3, characterized in that: In S1, W with a purity of more than 99.99% is used as the target material; in a vacuum of 6×10 -4 In a chamber below 100 Å / min, DC deposition sputtering is performed in an argon atmosphere.

5. The method for preparing the electrochromic / capacitive dual-function thin film material according to claim 4, characterized in that: In S1, during the DC deposition sputtering process, the gas flow rate of argon gas is 15-25 sccm, the sputtering power is 80-120 W, the sputtering pressure is 0.2-0.25 Pa, the sputtering time is 3-5 min, and the working distance is 10-12 cm.

6. The method for preparing the electrochromic / capacitive dual-function thin film material according to claim 3, characterized in that: In S2, W with a purity of more than 99.99% is used as the target material; in a vacuum of 6×10 -4 In a chamber below Pa, DC reactive deposition sputtering is carried out in a mixed atmosphere of oxygen and argon with a volume ratio of 1: (2.5-3).

7. The method for preparing the electrochromic / capacitive dual-function thin film material according to claim 6, characterized in that: In S2, during the DC reactive deposition sputtering process, the gas flow rate of argon is 25-30 sccm, the gas flow rate of oxygen is 10-12 sccm, the sputtering power is 80-120 W, the sputtering pressure is 0.3-0.35 Pa, the sputtering time is 15-18 min, and the working distance is 10-12 cm.

8. The method for preparing the electrochromic / capacitive dual-function thin film material according to claim 3, characterized in that: In S3, TiO2 with a purity of more than 99.99% is used as the target material, and the vacuum degree is 6×10 -4 In a chamber below 1.5 Å, RF deposition sputtering is performed in an argon atmosphere.

9. The method for preparing the electrochromic / capacitive dual-function thin film material according to claim 8, characterized in that: In S3, during the RF deposition sputtering process, the gas flow rate of argon gas is 15-25 sccm, the sputtering power is 80-120 W, the sputtering pressure is 0.2-0.25 Pa, the sputtering time is 8-10 min, and the working distance is 10-12 cm.

10. An application of the electrochromic / capacitive dual-function thin film material according to any one of claims 1 to 2, characterized in that: The applications include: application in color-changing energy storage devices.

Citation Information

Patent Citations

  • Electrochromic glass and fabrication method thereof

    CN109031838A

  • Metal target used for electrochromic glass and preparation method and application method thereof

    CN109825805A

  • Multicolor electrochromic structure as well as preparation method and application thereof

    CN111624829A

  • Multicolor electrochromic structure, fabrication method and application thereof

    US20230367167A1