Photosensitive insulating paste and electronic component
By using reasonable proportions of glass frit and inorganic fillers in photosensitive insulating paste, the resolution, dielectric constant and linear expansion coefficient are balanced, and the problems of cracks and dielectric constants of the insulation layer in the prior art are solved, and the problems of high dielectric constants are improved. Reliability and inductance value of inductor components.
Patent Information
- Application Number
- CN202410235073.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-05-01
- Filing Date
- 2024-03-01
- Publication Date
- 2024-11-05
AI Technical Summary
When the existing photosensitive insulating paste forms an insulating layer, the linear expansion coefficient and the linear expansion coefficient of the coil wiring are large, resulting in cracks, and the high dielectric constant leads to an increase in the thickness of the insulating layer, which limits the increase in the number of coil wirings.
Using a photosensitive insulating paste containing glass frit, a first inorganic filler (such as silicon oxide) and a second inorganic filler (such as alumina, zirconia), the first inorganic filler ratio (10 volume % to 40 volume % is used. Filler, 0 volume % to 30 volume % of the second inorganic filler) is used to balance the resolution, dielectric constant and linear expansion coefficient, and to reduce the softening point of the glass frit to improve adhesion.
The balance of resolution, dielectric constant and linear expansion coefficient is achieved, the reliability and inductance value of inductor components are improved, and the generation of cracks is suppressed and the number of coil wiring is increased.
Smart Images

Figure CN118897437A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to a photosensitive insulating paste and an electronic component. Background Art
[0002] Conventionally, photosensitive insulating pastes are used to form inductor components. For example, Japanese Patent Application Laid-Open No. 2012-246176 (Patent Document 1) describes a photosensitive insulating paste containing 50% to 90% by mass of silicon oxide, bismuth oxide, boron oxide, aluminum oxide, and zirconium oxide as glass frit.
[0003] Prior art literature
[0004] Patent Literature
[0005] Patent Document 1: Japanese Patent Application Publication No. 2012-246176 Summary of the invention
[0006] The use of the photosensitive insulating paste described in the above-mentioned gazette results in a higher resolution. However, the difference between the linear expansion coefficient of the insulating layer formed by the photosensitive insulating paste and the linear expansion coefficient of the coil wiring becomes larger, resulting in cracks and the like. In addition, the dielectric constant of the insulating layer becomes higher, resulting in the need to increase the thickness of the insulating layer. In this case, it is not easy to increase the number of coil wirings.
[0007] Therefore, an object of the present disclosure is to provide a photosensitive insulating paste having a good balance among resolution, dielectric constant, and linear expansion coefficient, and an electronic component using the photosensitive insulating paste.
[0008] In order to solve the above-mentioned problems, a photosensitive insulating paste as one embodiment of the present disclosure includes glass frit, a first inorganic filler, a second inorganic filler, an alkali-soluble polymer, a photosensitive monomer, a photopolymerization initiator and a solvent, wherein the glass frit includes SiO2 and B2O3 as main components and includes at least one of aluminum element, sodium element and phosphorus element as a subcomponent, the first inorganic filler is crystalline silicon oxide, the second inorganic filler is at least one of aluminum oxide, titanium dioxide, zirconium oxide, cerium dioxide, forsterite and an inorganic oxide pigment, and the first inorganic filler is contained in an amount of 10 volume % to 40 volume % and 0 volume % to 30 volume % of the second inorganic filler relative to 100 volume % of the total of the glass frit, the first inorganic filler and the second inorganic filler.
[0009] By including the glass frit, the first filler, and the second filler in the above-mentioned ranges, a photosensitive insulating paste having a good balance among resolution, dielectric constant, and linear expansion coefficient can be formed.
[0010] In one embodiment of the photosensitive insulating paste, the glass frit has a softening point of 700°C or higher and lower than 900°C.
[0011] With the above configuration, the glass frit melts at a temperature lower than the sintering temperature of the metal material of the coil wiring included in the inductor component, and the adhesion between the main body formed of the photosensitive insulating paste containing the glass frit and the coil wiring is improved.
[0012] In one embodiment of the photosensitive insulating paste, the first inorganic filler accounts for 20 to 40% by volume and the second inorganic filler accounts for 0 to 20% by volume, based on 100% by volume of the total of the glass frit, the first inorganic filler, and the second inorganic filler.
[0013] By including the first inorganic filler and the second inorganic filler in the above range, the strength of the main body can be improved, and the difference in linear expansion coefficient between the main body and the metal material is reduced, thereby improving the reliability of the inductor component. In addition, the dielectric constant of the main body can also be reduced. Therefore, the balance between resolution, dielectric constant and linear expansion coefficient becomes better.
[0014] In one embodiment of the photosensitive insulating paste, the first inorganic filler accounts for 30 to 40 volume % and the second inorganic filler accounts for 100 volume % of the total of the glass frit, the first inorganic filler and the second inorganic filler.
[0015] By including the first inorganic filler in the above range, the linear expansion coefficient of the body formed by the photosensitive insulating paste becomes larger, the difference in linear expansion coefficient between the body and the metal material can be reduced, and the generation of cracks can be suppressed. By including the second inorganic filler in the above range, the strength of the body becomes higher. As a result, the reliability of the inductor component is further improved.
[0016] In one embodiment of the photosensitive insulating paste, the glass frit includes phosphorus as a secondary component.
[0017] By having the above structure, the melting point of the glass material becomes lower and the linear expansion coefficient becomes larger. As a result, the difference in linear expansion coefficient between the coil wiring and the body can be reduced. Furthermore, the generation of stress caused by the difference in linear expansion coefficient can be suppressed, and the generation of cracks can be suppressed.
[0018] In one embodiment of the photosensitive insulating paste, the phosphorus element is contained in an amount of 0.1 mass % to 10 mass %.
[0019] With the above configuration, the difference in linear expansion coefficient between the coil wiring and the body can be further reduced, and the generation of stress due to the difference in linear expansion coefficient can be further suppressed, thereby further suppressing the generation of cracks.
[0020] In order to solve the above-mentioned problems, an electronic component as one embodiment of the present invention includes a main body and a coil arranged in the above-mentioned main body and wound along an axis, the above-mentioned coil has multiple coil wirings, the above-mentioned main body contains a glass material, a first inorganic filler and a second inorganic filler, the above-mentioned glass material contains SiO2 and B2O3 as main components, and contains at least one of aluminum element, sodium element and phosphorus element as a minor component, the above-mentioned first inorganic filler is a crystalline silicon oxide, the above-mentioned second inorganic filler contains at least one of aluminum oxide, titanium dioxide, zirconium oxide, cerium dioxide, forsterite and an inorganic oxide pigment, and relative to 100 volume% of the total of the above-mentioned glass material, the above-mentioned first inorganic filler and the above-mentioned second inorganic filler, the above-mentioned first inorganic filler is contained in 10 volume% to 40 volume%, and the above-mentioned second inorganic filler is contained in 0 volume% to 30 volume%.
[0021] By including the glass material, the first inorganic filler, and the second inorganic filler in the above-mentioned ranges, a body having a well-balanced resolution, dielectric constant, and linear expansion coefficient can be formed.
[0022] In one aspect of the electronic component, a ratio of a thickness of the coil wire in the axial direction to a thickness of a portion of the main body between adjacent coil wires in the axial direction is in a range of 1.0 to 3.0.
[0023] By having the above-mentioned structure, the thickness of the portion between adjacent coil wirings in the main body becomes smaller, and as a result, the number of coil wirings can be increased, and the inductance value can be increased. If the above-mentioned ratio becomes too small, the thickness of the portion between adjacent coil wirings in the main body becomes larger, the number of coil wirings decreases, and the number of coil turns decreases. As a result, the inductance value (L value) of the electronic component decreases. If the above-mentioned ratio becomes too large, there is the following risk: the thickness of the portion between adjacent coil wirings in the main body becomes too small, the distance between the coil wirings is close, the stray capacitance increases, and the Q value decreases.
[0024] Here, the axial thickness of the portion between adjacent coil wirings in the body is the value of the shortest distance between adjacent coil wirings in a cross section passing through the center of the body and orthogonal to the extension direction of the coil wiring. The axial thickness of the coil wiring is the maximum value of the axial thickness of the coil wiring in a cross section passing through the center of the body and orthogonal to the extension direction of the coil wiring.
[0025] In one aspect of the electronic component, an average value of the thickness of the coil wire in the axial direction is 3 μm to 15 μm.
[0026] By having the above structure, the DC resistance (Rdc) can be suppressed, the number of coil wirings can be increased, and the inductance value can be increased. If the above average value becomes too small, the DC resistance becomes large. If the above average value becomes too large, the number of coil wirings becomes small, that is, the number of coil turns becomes small, and the inductance value decreases.
[0027] In one aspect of the electronic component, the number of turns of the coil wiring is one or more.
[0028] By having the above configuration, the inductance value can be increased. In particular, by suppressing the dielectric constant of the main body, even if the coil wiring has one or more turns and a parallel portion is generated, an increase in stray capacitance can be suppressed, and the characteristics of the electronic component can be improved.
[0029] According to the present disclosure, it is possible to provide a photosensitive insulating paste having a good balance among resolution, dielectric constant, and linear expansion coefficient, and an electronic component using the photosensitive insulating paste. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 It is a top perspective view schematically showing the inductor component according to the first embodiment.
[0031] Figure 2 It is an exploded perspective view of the inductor component according to the first embodiment.
[0032] Figure 3 It is an XY cross-sectional view of the inductor component according to the first embodiment.
[0033] Figure 4A This is an explanatory diagram for explaining a method for manufacturing an inductor component.
[0034] Figure 4B This is an explanatory diagram for explaining a method for manufacturing an inductor component.
[0035] Figure 4C This is an explanatory diagram for explaining a method for manufacturing an inductor component.
[0036] Figure 4D This is an explanatory diagram for explaining a method for manufacturing an inductor component.
[0037] Figure 4E This is an explanatory diagram for explaining a method for manufacturing an inductor component.
[0038] Explanation of symbols
[0039] 1 Inductor components
[0040] 10 Main Body
[0041] 13 First side
[0042] 14 Second side
[0043] 15 First end face
[0044] 16 Second end face
[0045] 17 Bottom
[0046] 18 Top
[0047] 20 Coils
[0048] 25 Coil wiring
[0049] 26 Via wiring
[0050] 30 first external electrode
[0051] 33 first external electrode conductor layer
[0052] 40 second external electrode
[0053] 43 Second external electrode conductor layer
[0054] L Axial
[0055] D1 Thickness of the coil wiring body
[0056] D2 Coil wiring thickness DETAILED DESCRIPTION
[0057] The electronic component as one embodiment of the present disclosure is described in more detail below through the illustrated embodiments. It should be noted that the drawings include some schematic drawings, which sometimes do not reflect actual dimensions and proportions. In addition, an inductor component is described below as an example of an electronic component, but the electronic component may also be an electronic component other than an inductor component.
[0058] (First Embodiment)
[0059] Figure 1 It is a top perspective view schematically showing the inductor component according to the first embodiment. Figure 2 This is an exploded perspective view of the inductor components. Figure 3 is an XY cross-sectional view of the inductor component. Figure 1 In the figure, in order to make the structure easier to understand, the main body 10 is depicted as transparent, but it may also be translucent or opaque. Figure 3 In order to facilitate understanding of the structure, the description of the via wiring is omitted.
[0060] The inductor component 1 is electrically connected to wiring of a circuit substrate (not shown) via the first external electrode 30 and the second external electrode 40. The inductor component 1 is used, for example, as an impedance matching coil for a high-frequency circuit, and is used in electronic devices such as personal computers, DVD players, digital cameras, TVs, mobile phones, automotive electronics, and medical and industrial machinery. However, the use of the inductor component 1 is not limited thereto, and it can also be used, for example, in a tuning circuit, a filter circuit, a rectifier smoothing circuit, etc.
[0061] The main body 10 is formed by stacking a plurality of insulating layers 11. The insulating layer 11 is obtained, for example, by repeatedly applying a photosensitive insulating paste and drying it as needed to form a stacked body, and then calcining it. The main body 10 is formed into a roughly rectangular parallelepiped shape. The surface of the main body 10 has a first side surface 13, a second side surface 14 opposite to the first side surface, a first end surface 15, a second end surface 16 opposite to the first end surface 15, a bottom surface 17 connected between the first end surface 15 and the second end surface 16, and a top surface 18 opposite to the bottom surface 17. The first end surface 15, the second end surface 16, the bottom surface 17 and the top surface 18 are parallel to the stacking direction of the insulating layer 11. Here, the "parallel" in this application is not limited to an exact parallel relationship, and also includes a substantially parallel relationship in consideration of the range of actual deviations. It should be noted that the main body 10 sometimes becomes unclear due to calcination, etc., and the interfaces between the plurality of insulating layers 11 become unclear.
[0062] It should be noted that, as shown in the drawings, for the sake of convenience of description, the direction from the first end surface 15 toward the second end surface 16 is set as the X direction. The direction from the second side surface 14 toward the first side surface 13 is set as the Y direction. The direction from the bottom surface 17 toward the top surface 18 is set as the Z direction. The X direction, the Y direction, and the Z direction are mutually orthogonal directions, and when arranged in the order of X, Y, and Z, a left-hand coordinate system is formed.
[0063] The first external electrode 30 and the second external electrode 40 are composed of, for example, a conductive material such as Ag or Cu and glass particles. The first external electrode 30 is arranged across the first end surface 15 and the bottom surface 17 and is L-shaped. The second external electrode 40 is arranged across the second end surface 16 and the bottom surface 17 and is L-shaped. It should be noted that in the first embodiment, the first external electrode 30 and the second external electrode 40 have an L-shape, but may also have other shapes. For example, the first external electrode 30 and the second external electrode 40 may have a shape that is only arranged on the bottom surface. Alternatively, the first external electrode 30 may be arranged on the first end surface 15 of the main body 10 and a portion of the first side surface 13, the second side surface 14, the bottom surface 17 and the top surface 18 adjacent to the first end surface 15, and the second external electrode 40 may be arranged on the second end surface 16 and a portion of the first side surface 13, the second side surface 14, the bottom surface 17 and the top surface 18 adjacent to the second end surface 16.
[0064] The coil 20 is composed of, for example, the same conductive material and glass particles as the first external electrode 30 and the second external electrode 40. The coil 20 is wound in a spiral shape along the stacking direction of the insulating layer 11. The first end of the coil 20 is connected to the first external electrode 30, and the second end of the coil 20 is connected to the second external electrode 40. It should be noted that in the present embodiment, the coil 20 is integrated with the first external electrode 30 and the second external electrode 40, and there is no clear boundary, but it is not limited to this, and the coil and the external electrode can also be formed by different types of materials and different types of methods, thereby having a boundary.
[0065] The coil 20 is formed into a substantially oblong shape when viewed from the axial direction L, but is not limited to this shape. The shape of the coil 20 may be, for example, circular, elliptical, rectangular, or other polygonal shapes. The axial direction L of the coil 20 refers to a direction parallel to the central axis of the spiral in which the coil 20 is wound. The axial direction L of the coil 20 and the stacking direction of the insulating layer 11 refer to the same direction (Y direction).
[0066] The coil 20 includes a plurality of coil wirings 25 wound on the insulating layer 11. The coil wirings 25 adjacent to each other in the stacking direction are electrically connected in series via the through-hole wirings 26 that penetrate the insulating layer 11 in the thickness direction. In this way, the plurality of coil wirings 25 are electrically connected in series with each other and form a spiral. Specifically, the coil 20 has a structure in which a plurality of coil wirings 25 are stacked and electrically connected in series with each other and the number of windings is less than 1 turn, and the coil 20 is in a helical shape. It should be noted that the number of windings of the coil 20 can be more than 1 turn, or a combination of less than 1 turn and more than 1 turn.
[0067] Preferably, the ratio of the thickness D2 of the coil wiring 25 in the axial direction L to the thickness D1 of the portion between adjacent coil wirings 25 in the main body 10 in the axial direction L is in the range of 1.0 to 3.0. By having the above-mentioned structure, the thickness D1 becomes smaller, and as a result, the number of coil wirings 25 can be increased, and the inductance value can be increased. If the above-mentioned ratio becomes too small, the thickness D1 becomes larger, the number of coil wirings 25 becomes smaller, and the number of turns of the coil 20 becomes smaller. As a result, the inductance value of the inductor component 1 becomes smaller. If the above-mentioned ratio becomes too large, there is a risk that the thickness D1 becomes too small, the distance between the coil wirings 25 becomes close, the stray capacitance becomes larger, and the Q value decreases.
[0068] Here, thickness D1 is the value of the shortest distance between adjacent coil wirings 25 in a cross section passing through the center of the body 10 and perpendicular to the extension direction of the coil wiring 25. Thickness D2 is the maximum value of the coil wiring 25 in the axial direction L in a cross section passing through the center of the body 10 and perpendicular to the extension direction of the coil wiring 25.
[0069] Preferably, the average value of the thickness of the coil wiring 25 in the axial direction L is 3 μm to 15 μm. By having the above-mentioned structure, the DC resistance (Rdc) can be suppressed, and the number of coil wirings 25 can be increased, and the inductance value (L value) can be increased. If the above-mentioned average value becomes too small, the DC resistance becomes larger. If the above-mentioned average value becomes too large, the number of coil wirings 25 becomes smaller, that is, the number of turns of the coil 20 becomes smaller, and the inductance value decreases.
[0070] Preferably, the number of turns of the coil wiring 25 is one or more. With the above configuration, the inductance value of the inductor component 1 can be increased. In particular, by suppressing the dielectric constant of the body 10, even if the coil wiring 25 has one or more turns and a parallel portion is generated, an increase in stray capacitance can be suppressed, and the characteristics of the inductor component 1 can be improved.
[0071] (Photosensitive insulating paste and insulating layer 11)
[0072] The photosensitive insulating paste and the insulating layer 11 are described.
[0073] The photosensitive insulating paste comprises glass frit, a first inorganic filler, a second inorganic filler, an alkali-soluble polymer, a photosensitive monomer, a photopolymerization initiator and a solvent. The glass frit comprises SiO2 and B2O3 as main components, and comprises at least one of aluminum, sodium and phosphorus as a secondary component. The first inorganic filler is a crystalline silicon oxide. The second inorganic filler comprises at least one of aluminum oxide, titanium dioxide, zirconium oxide, cerium dioxide, forsterite and an inorganic oxide pigment. With respect to the total of 100 volume of the glass frit, the first inorganic filler and the second inorganic filler, 10 volume % to 40 volume % of the first inorganic filler and 0 volume % to 30 volume % of the second inorganic filler are included.
[0074] According to the research of the present inventors, it is found that by including the glass frit, the first inorganic filler and the second inorganic filler in the above range, a photosensitive insulating paste with a good balance of resolution, dielectric constant and linear expansion coefficient can be formed. Specifically, by including the glass frit in the above range, a photosensitive insulating paste with high resolution is obtained, and the photosensitive insulating paste can form a high-precision inductor component 1. If the content of the glass frit increases, the crack extension prevention effect caused by the filler contained in the main body 10 (insulating layer 11) formed by the photosensitive insulating paste cannot be obtained, the strength is reduced, and cracks are sometimes generated in the main body 10. If the content of the glass frit decreases, the glass frit cannot be calcined tightly, and as a result, the main body 10 becomes brittle and easily cracked. By including the first inorganic filler in the above range, the main body 10 can be sintered tightly while reducing the difference in linear expansion coefficient between the main body 10 and the metal material of the coil wiring 25 included in the inductor component 1, and the generation of cracks can be suppressed. Furthermore, the dielectric constant of the main body 10 can be reduced, and the electrical characteristics of the inductor component 1 can be improved. It should be noted that if the content of the first inorganic filler becomes too large, the content of the glass frit decreases and cannot be sintered tightly, resulting in the main body 10 becoming brittle. In addition, if the content of the first filler becomes too small, the above-mentioned linear expansion coefficient difference and dielectric constant reduction effect cannot be obtained. By adding the second inorganic filler, the strength of the main body 10 can be further improved, and the stress generated between the main body 10 and the coil wiring 25 can be withstood. As a result, by including the second inorganic filler in the above range, cracks are not easy to occur. If the content of the second inorganic filler becomes too large, the light transmittance of the photosensitive paste decreases and the resolution deteriorates. Furthermore, in addition to the main body 10 being difficult to sinter tightly and becoming brittle, the dielectric constant of the main body 10 increases, and the electrical characteristics of the inductor component 1 are reduced. In addition, by including the glass frit, the first inorganic filler and the second inorganic filler in the above range, the thickness of the main body 10 can be reduced, and the number of coil wirings 25 can be increased, as a result, the inductance value of the inductor component 1 becomes larger. In addition, by including the glass frit, the first inorganic filler, and the second inorganic filler in the above range, the dielectric constant of the body 10 becomes lower. As a result, the thickness of the portion between the adjacent coil wirings 25 in the body 10 can be reduced, and the number of coil wirings 25 can be increased, resulting in a larger inductance value of the inductor component 1. In summary, by including the glass frit, the first filler, and the second filler in the above range, the body 10 with a good balance of resolution, dielectric constant, and linear expansion coefficient can be formed.
[0075] As the glass frit, borosilicate glass can be used. It should be noted that, as the glass frit, in addition to borosilicate glass, for example, glass containing SiO2, B2O3, K2O, Li2O, CaO, ZnO, Bi2O3, P2O5 and / or Al2O3, such as SiO2-B2O3-K2O glass, SiO2-B2O3-Li2O-CaO glass, SiO2-B2O3-Li2O-CaO-ZnO glass, SiO2-B2O3-P2O5 glass and Bi2O3-B2O3-SiO2-Al2O3 glass can be used. These inorganic components can be combined into two or more.
[0076] The softening point of the glass frit is 700° C. or higher and lower than 900° C. With the above configuration, the glass frit melts at a temperature lower than the sintering temperature of the metal material of the coil wiring 25 included in the inductor component 1, and the adhesion between the body 10 formed of the photosensitive insulating paste containing the glass frit and the coil wiring 25 becomes good. The softening point is a value measured using a thermomechanical analyzer (TMA).
[0077] As the first inorganic filler, for example, quartz and silicon dioxide can be cited, and quartz can be preferably used. With the above-mentioned structure, the linear expansion coefficient becomes higher, and the difference in linear expansion coefficient between the insulating layer 11 formed by the photosensitive insulating paste and the coil wiring 25 becomes smaller. Thus, it is possible to suppress the generation of cracks between the insulating layer 11 and the coil wiring 25. Quartz is crystalline quartz, and the crystallinity of quartz is not particularly limited.
[0078] Preferably, the second inorganic filler is alumina.
[0079] The average particle size of each of the first inorganic filler and the second inorganic filler is, for example, 0.1 μm to 5.0 μm, specifically 0.3 μm to 3.0 μm. If the average particle size is too small, the photosensitive insulating paste is difficult to disperse. If the average particle size is too large, the smoothness of the insulating layer 11 may be reduced.
[0080] The alkali-soluble polymer includes, for example, an acrylic copolymer having a carboxyl group in a side chain. The above resin including an acrylic copolymer having a carboxyl group in a side chain can be produced by, for example, copolymerizing an unsaturated carboxylic acid with an ethylenically unsaturated compound.
[0081] Examples of the unsaturated carboxylic acid include acrylic acid, methacrylic acid, maleic acid, fumaric acid, vinylacetic acid, and anhydrides thereof. Examples of the ethylenically unsaturated compound include acrylic acid esters such as methyl acrylate and ethyl acrylate, methacrylic acid esters such as methyl methacrylate and ethyl methacrylate, and fumaric acid esters such as monoethyl fumarate.
[0082] As the acrylic copolymer having a carboxyl group in a side chain, an acrylic copolymer into which an unsaturated bond is introduced in the following form can be used.
[0083] (1) An acrylic monomer having a functional group such as an epoxy group that can react with the carboxyl group on the side chain of the acrylic copolymer is added.
[0084] (2) After reacting the acrylic copolymer into which epoxy groups have been introduced instead of carboxyl groups in the side chains with an unsaturated monocarboxylic acid, a saturated or unsaturated polycarboxylic acid anhydride is further introduced.
[0085] As the acrylic copolymer having a carboxyl group in a side chain, an acrylic copolymer having a weight average molecular weight (Mw) of 50,000 or less and an acid value of 30 to 150 can be used.
[0086] As the photosensitive monomer, dipentaerythritol monohydroxy pentaacrylate can be used. It should be noted that as the photosensitive monomer, in addition to dipentaerythritol monohydroxy pentaacrylate, hexanediol triacrylate, tripropylene glycol triacrylate, trimethylolpropane triacrylate, EO-modified trimethylolpropane triacrylate, stearyl acrylate, tetrahydrofurfuryl acrylate, lauryl acrylate, 2-phenoxyethyl acrylate, isodecyl acrylate, isooctyl acrylate, tridecyl acrylate, caprolactone acrylate, ethoxylated nonylphenol acrylate, 1,3-butylene glycol dipropylene glycol acrylate, Acid ester, 1,4-butanediol diacrylate, diethylene glycol diacrylate, tetraethylene glycol diacrylate, triethylene glycol diacrylate, ethoxylated bisphenol A diacrylate, propoxylated neopentyl glycol diacrylate, tris(2-hydroxyethyl)isocyanurate triacrylate, pentaerythritol triacrylate, propoxylated trimethylolpropane triacrylate, propoxylated glycerol triacrylate, pentaerythritol tetraacrylate, ditrimethylolpropane tetraacrylate, ethoxylated pentaerythritol tetraacrylate, etc. In addition, compounds obtained by converting part or all of the acrylate in the molecule of the above-mentioned compound into methacrylate can be used.
[0087] As the photopolymerization initiator, an acetophenone compound, a benzophenone compound, an acylphosphine compound, or an oxime ester compound can be used.
[0088] The solvent is not particularly limited, and examples thereof include ethylene glycol monobutyl ether, ethylene glycol monohexyl ether, ethylene glycol monoethylhexyl ether, propylene glycol monobutyl ether, dipropylene glycol monoethyl ether, dipropylene glycol monobutyl ether, propylene glycol monophenyl ether, ethyl acetate, butyl acetate, amyl acetate, hexyl acetate, and cyclohexyl acetate.
[0089] The photosensitive insulating paste may further contain an organic dye. As the organic dye, an azo compound may be used. When the photosensitive insulating paste is used for photolithography patterning, the organic dye functions as an ultraviolet absorber for finely adjusting the ultraviolet transmittance.
[0090] Preferably, the first inorganic filler is contained in an amount of 20% to 40% by volume and the second inorganic filler is contained in an amount of 0% to 20% by volume relative to 100% by volume of the total of the glass frit, the first inorganic filler and the second inorganic filler. By containing the first inorganic filler and the second inorganic filler in the above range, the strength of the main body 10 can be improved, and the difference in linear expansion coefficient between the main body 10 and the metal material becomes smaller, thereby improving the reliability of the inductor component 1. In addition, the dielectric constant of the main body 10 can also be reduced. Therefore, the balance among the resolution, dielectric constant and linear expansion coefficient becomes better.
[0091] Preferably, the first inorganic filler is contained in an amount of 30% to 40% by volume and the second inorganic filler is contained in an amount of 100% by volume relative to the total of the glass frit, the first inorganic filler and the second inorganic filler. By containing the first inorganic filler in the above range, the linear expansion coefficient of the main body 10 formed by the photosensitive insulating paste becomes larger, the difference in linear expansion coefficient between the main body 10 and the metal material can be reduced, and the generation of cracks can be suppressed. By containing the second inorganic filler in the above range, the strength of the main body 10 becomes higher. As a result, the reliability of the inductor component 1 is further improved.
[0092] It should be noted that, relative to 100 volume % of the total of the glass frit, the first inorganic filler and the second inorganic filler, the first inorganic filler may be contained at 10 volume % to 40 volume % and the second inorganic filler at 0 volume %, or the first inorganic filler may be contained at 20 volume % to 40 volume % and the second inorganic filler at 0 volume %.
[0093] Preferably, the glass frit contains phosphorus as a secondary component. By having the above-mentioned structure, the melting point of the glass frit becomes lower and the linear expansion coefficient becomes larger. As a result, the difference in linear expansion coefficient between the coil wiring 25 and the main body 10 can be reduced. Furthermore, the generation of stress caused by the difference in linear expansion coefficient can be suppressed, and the generation of cracks can be suppressed.
[0094] Preferably, the glass frit contains 0.1 mass % to 10 mass % of phosphorus. The content of phosphorus is measured using a wavelength dispersive X-ray fluorescence analyzer (WDX) or a high-frequency inductively coupled plasma (ICP) emission analyzer.
[0095] The insulating layer 11 includes a glass material, a first inorganic filler and a second inorganic filler. The glass material includes SiO2 and B2O3 as main components, and includes at least one of aluminum, sodium and phosphorus as a subcomponent. The first inorganic filler is a crystalline silicon oxide. The second inorganic filler includes at least one of aluminum oxide, titanium dioxide, zirconium oxide, cerium dioxide, forsterite and an inorganic oxide pigment. Relative to the total volume of 100% by volume of the glass material, the first inorganic filler and the second inorganic filler, the first inorganic filler includes 10% by volume to 40% by volume, and the second inorganic filler includes 0% by volume to 30% by volume. That is, relative to the total volume of 100% by volume of the glass material, the first inorganic filler and the second inorganic filler, the glass material includes 30% by volume to 90% by volume, the first inorganic filler includes 10% by volume to 40% by volume, and the second inorganic filler includes 0% by volume to 30% by volume. It should be noted that the main component refers to a component that includes 60% by volume or more relative to 100% by volume of the glass material. The upper limit of the main component is not particularly limited, for example, it is 99% by volume or less. A secondary component refers to a component that is contained in 40% by volume or less relative to 100% by volume of the glass material. The lower limit of the secondary component is not particularly limited, for example, it is 0.1% by volume or more. The ratio of the glass material, the first inorganic filler, and the second inorganic filler contained in the insulating layer 11 is substantially the same as the ratio of the glass frit, the first inorganic filler, and the second inorganic filler contained in the photosensitive insulating paste. The glass material contained in the insulating layer 11 is obtained by calcining the glass frit contained in the photosensitive insulating paste. The type and composition of the first inorganic filler and the second inorganic filler contained in the insulating layer 11 are the same as the type and composition of the first inorganic filler and the second inorganic filler contained in the photosensitive insulating paste.
[0096] By including the glass material, the first inorganic paste, and the second inorganic paste in the above-mentioned ranges as in the glass frit of the photosensitive insulating paste, the first inorganic paste, and the second inorganic paste, the insulating layer 11 (main body 10) having a good balance among resolution, dielectric constant, and linear expansion coefficient can be formed.
[0097] (Manufacturing method)
[0098] Next, a method for manufacturing the inductor component 1 will be described.
[0099] First, negative-type photosensitive insulating paste and conductive paste are prepared.
[0100] like Figure 4A As shown, a photosensitive insulating paste is applied to form the outer insulating layer 11a. The photosensitive insulating paste is applied by screen printing, for example. FIG. 4A to FIG. 4E It is a cross-sectional view in the XY direction.
[0101] like Figure 4BAs shown in FIG. 1 , a photosensitive insulating paste is applied to the outer insulating layer 11a to form the first insulating layer 11b. Then, the first insulating layer 11b is exposed to light while the first portion 111 (indicated by a double-dashed line) of the first insulating layer 11b is shielded from light by a mask 110. Figure 4C As shown in FIG. 1 , the first portion 111 of the first insulating layer 11b is removed by development, and a groove 112 is formed at a position corresponding to the first portion 111. Figure 4D As shown, the coil wiring 25 is formed in the slot 112 .
[0102] like Figure 4E As shown, a photosensitive insulating paste is applied on the first insulating layer 11b and the coil wiring 25 to form the second insulating layer 11c. The above steps are repeated several times to form a laminate, which is then fired to manufacture the inductor component 1.
[0103] Example
[0104] The present invention will be specifically described by the following examples, but the present invention is not limited to these examples.
[0105] (Examples 1 to 9, Comparative Examples 1 to 3)
[0106] Borosilicate glass containing phosphorus as glass frit, quartz as a first inorganic filler, and alumina as a second inorganic filler were mixed in the ratios shown in Table 1 to form a photosensitive insulating paste.
[0107] The obtained photosensitive insulating paste was used to form the inductor component 1. In addition, the resolution, dielectric constant, and crack prevention effect were measured when the inductor component 1 was formed. The results are shown in Table 1.
[0108] (Resolution)
[0109] The paste was printed with a thickness of 20 μm by screen printing, dried in a safety oven, exposed through a photomask having openings of various sizes, and developed with an alkaline aqueous solution to form a wiring pattern. The width and thickness of the pattern that could be produced without residue or pattern loss were measured, and the aspect ratio (thickness / width) was calculated.
[0110] ◎: Resolution is 1.0 or more.
[0111] ○: The resolution is greater than 0.5 and less than 1.0.
[0112] ×: Resolution is less than 0.5.
[0113] (Dielectric constant)
[0114] An insulating layer was formed from the photosensitive insulating paste, and the dielectric constant was measured. The dielectric constant was measured using a signal analyzer (manufactured by Keysight Technologies).
[0115] ◎: Dielectric constant is 6.0 or more.
[0116] ○: Dielectric constant is greater than or equal to 6.0 and less than 7.0.
[0117] ×: Dielectric constant is less than 7.0.
[0118] (Crack prevention effect)
[0119] The crack prevention effect was measured as follows.
[0120] The inductor component made of insulating paste is fixed on the substrate, and the test load (p)-displacement (h) graph is obtained when the nanoindenter is pressed against the main body of the inductor component. The contact rigidity (S=dp / dh) when the load increases is calculated from the obtained test load (p)-displacement (h) data, and a contact rigidity (S)-test load (p) graph is prepared. The peak with the lowest load among the peaks showing a decrease in contact rigidity in the prepared graph is judged as the first crack to occur in the main body of the component, and the load at this time is defined as the "crack generation load".
[0121] The nanoindenter device and measurement conditions are as follows.
[0122] Equipment: Nano-indenter ENT-1100a (manufactured by ELIONIX)
[0123] Test load: 100gf
[0124] Step distance: 20msec
[0125] ◎: Crack initiation load is 70N or more.
[0126] ○: The crack initiation load is 30N or more and less than 70N.
[0127] ×: The crack initiation load is less than 30 N.
[0128] [Table 1]
[0129]
[0130] In Examples 1 to 4, a photosensitive insulating paste containing glass frit and a first inorganic filler was used. In Examples 1 to 4, the photosensitive insulating paste had good resolution, dielectric constant, and crack prevention effect. In particular, by containing 20 volume % to 40 volume % of the first inorganic filler, the dielectric constant became better.
[0131] In Examples 5 to 9, a photosensitive insulating paste containing glass frit, a first inorganic filler, and a second inorganic filler is used. In Examples 5 to 9, the resolution, dielectric constant, and crack prevention effect of the photosensitive insulating paste are all good. In particular, in terms of the crack prevention effect, Examples 5 to 9 are better than Examples 1 to 4. It is believed that this is because the strength of the main body is improved by including the second inorganic filler. In addition, in Examples 5 and 6, the resolution of the photosensitive insulating paste, the dielectric constant of the inductor component, and the crack prevention effect are all particularly good.
[0132] In Comparative Example 1, a photosensitive insulating paste containing only glass frit is used. In Comparative Example 1, the resolution and dielectric constant are good, but the crack prevention effect is evaluated as ×. In Comparative Example 2, a photosensitive insulating paste containing 40 volume % of the first inorganic filler and the second inorganic filler is used. However, the resolution, dielectric constant, and crack prevention effect are all evaluated as ×. It is believed that this is because, in Comparative Example 2, as the content of the first inorganic filler and the second inorganic filler increases, the content of the glass frit decreases, and the formed insulating layer becomes brittle. In Comparative Example 3, the content of the glass frit is the same as that in Comparative Example 2, which is 20 volume %, but the first inorganic filler is 50 volume % and the second inorganic filler is 30 volume %, to form a photosensitive insulating paste. The resolution and dielectric constant are evaluated as good, but the crack prevention effect is evaluated as ×. It is believed that this is because the content of the glass frit is not within an appropriate range.
[0133] As described above, it is understood that good results can be obtained in terms of resolution, dielectric constant, and crack prevention effect by using a photosensitive insulating paste containing glass frit, the first inorganic filler, and the second inorganic filler in appropriate ranges.
[0134] It should be noted that the present disclosure is not limited to the above-mentioned embodiment, and design changes can be made within the scope of the present disclosure. The shape of the magnetic core is not limited to the present embodiment, and design changes can be made. In addition, the number of coils is not limited to the present embodiment, and design changes can be made.
[0135] The present disclosure includes the following aspects.
[0136] <1>
[0137] A photosensitive insulating paste comprises glass frit, a first inorganic filler, a second inorganic filler, an alkali-soluble polymer, a photosensitive monomer, a photopolymerization initiator and a solvent.
[0138] The glass frit contains SiO2 and B2O3 as main components, and contains at least one of aluminum, sodium and phosphorus as a subsidiary component.
[0139] The first inorganic filler is crystalline silicon oxide.
[0140] The second inorganic filler comprises at least one of alumina, titanium dioxide, zirconium oxide, cerium dioxide, forsterite and inorganic oxide pigments.
[0141] The first inorganic filler is contained in an amount of 10 to 40% by volume and the second inorganic filler is contained in an amount of 0 to 30% by volume with respect to 100% by volume of the total of the glass frit, the first inorganic filler and the second inorganic filler.
[0142] <2>
[0143] The photosensitive insulating paste according to <1>, wherein the glass frit has a softening point of 700°C or higher and lower than 900°C.
[0144] <3>
[0145] The photosensitive insulating paste according to <1> or <2> comprises 20% to 40% by volume of the first inorganic filler and 0% to 20% by volume of the second inorganic filler, relative to 100% by volume of the total of the glass frit, the first inorganic filler and the second inorganic filler.
[0146] <4>
[0147] The photosensitive insulating paste according to any one of <1> to <3>, comprising 30% to 40% by volume of the first inorganic filler and 10% to 20% by volume of the second inorganic filler, relative to 100% by volume of the total of the glass frit, the first inorganic filler and the second inorganic filler.
[0148] <5>
[0149] The photosensitive insulating paste according to any one of <1> to <4>, wherein the glass frit contains phosphorus as a secondary component.
[0150] <6>
[0151] The photosensitive insulating paste according to <5> contains 0.1 mass % to 10 mass % of the phosphorus element.
[0152] <7>
[0153] An electronic component comprising:
[0154] Subject, and
[0155] A coil is disposed in the main body and wound along the axis;
[0156] The coil has a plurality of coil wirings.
[0157] The main body comprises a glass material, a first inorganic filler and a second inorganic filler.
[0158] The glass material contains SiO2 and B2O3 as main components, and contains at least one of aluminum, sodium and phosphorus as a subsidiary component.
[0159] The first inorganic filler is crystalline silicon oxide.
[0160] The second inorganic filler comprises at least one of alumina, titanium dioxide, zirconium oxide, cerium dioxide, forsterite and inorganic oxide pigments.
[0161] The first inorganic filler is contained in an amount of 10 to 40 volume % and the second inorganic filler is contained in an amount of 0 to 30 volume % with respect to 100 volume % of the total of the glass material, the first inorganic filler and the second inorganic filler.
[0162] <8>
[0163] The electronic component according to <7>, wherein a ratio of a thickness of the coil wire in the axial direction to a thickness of a portion of the main body between adjacent coil wires in the axial direction is in a range of 1.0 to 3.0.
[0164] <9>
[0165] The electronic component according to <7> or <8>, wherein an average value of the thickness of the coil wire in the axial direction is 3 μm to 15 μm.
[0166] <10>
[0167] The electronic component according to any one of <7> to <9>, wherein the number of windings of the coil wiring is one or more.
Claims
1. A photosensitive insulating paste comprising glass frit, a first inorganic filler, a second inorganic filler, an alkali-soluble polymer, a photosensitive monomer, a photopolymerization initiator and a solvent, The glass frit contains SiO2 and B2O3 as main components, and contains at least one of aluminum, sodium and phosphorus as a secondary component. The first inorganic filler is crystalline silicon oxide, The second inorganic filler comprises at least one of alumina, titanium dioxide, zirconium oxide, cerium dioxide, forsterite and inorganic oxide pigments, The first inorganic filler is contained in an amount of 10 to 40 volume % and the second inorganic filler is contained in an amount of 0 to 30 volume % with respect to 100 volume % of the total of the glass frit, the first inorganic filler and the second inorganic filler.
2. The photosensitive insulating paste according to claim 1, wherein The glass frit has a softening point of 700°C or more and less than 900°C.
3. The photosensitive insulating paste according to claim 1 or 2, wherein: The first inorganic filler is contained in an amount of 20 to 40 volume % and the second inorganic filler is contained in an amount of 0 to 20 volume % with respect to 100 volume % of the total of the glass frit, the first inorganic filler and the second inorganic filler.
4. The photosensitive insulating paste according to claim 1 or 2, wherein: The first inorganic filler is contained in an amount of 30 to 40 volume % and the second inorganic filler is contained in an amount of 10 to 20 volume % with respect to 100 volume % of the total of the glass frit, the first inorganic filler and the second inorganic filler.
5. The photosensitive insulating paste according to claim 1 or 2, wherein: The glass frit includes phosphorus as a secondary component.
6. The photosensitive insulating paste according to claim 5, wherein The phosphorus element is contained in an amount of 0.1 mass % to 10 mass %.
7. An electronic component comprising: Subject, and A coil is disposed in the main body and wound along an axis; The coil has a plurality of coil wires, The main body comprises a glass material, a first inorganic filler and a second inorganic filler, The glass material contains SiO2 and B2O3 as main components, and contains at least one of aluminum, sodium and phosphorus as a secondary component. The first inorganic filler is crystalline silicon oxide, The second inorganic filler comprises at least one of alumina, titanium dioxide, zirconium oxide, cerium dioxide, forsterite and inorganic oxide pigments, With respect to 100 volume % of the total of the glass material, the first inorganic filler, and the second inorganic filler, 10 volume % to 40 volume % of the first inorganic filler is included, and 0 volume % to 30 volume % of the second inorganic filler is included.
8. The electronic component according to claim 7, wherein A ratio of a thickness of the coil wire in the axial direction to a thickness of a portion of the main body between adjacent coil wires in the axial direction is in a range of 1.0 to 3.
0.
9. The electronic component according to claim 7 or 8, wherein: An average value of the thickness of the coil wire in the axial direction is 3 μm to 15 μm.
10. The electronic component according to claim 7 or 8, wherein: The number of windings of the coil wiring is one or more.