Electrode slurry and preparation method and application thereof

By using carbon nanosphere-based composite electrode slurry in liquid flow supercapacitors, the double layer is formed by using the adsorption and desorption characteristics of carbon materials, the problem of electrode slurry pooling in traditional liquid flow batteries is solved, and the problem of electrode slurry pooling is realized. Fast charging and discharging and battery stability uniformity improve battery energy and Coulomb efficiency.

CN118899170APending Publication Date: 2024-11-05DALIAN INSTITUTE OF CHEMICAL PHYSICS CHINESE ACADEMY OF SCIENCES
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310497652.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-05
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

Traditional liquid flow batteries have problems such as low power density, high concentration liquid flow type supercapacitor electrode slurry pooling and blocking of the electrode slurry, which leads to an increase in the internal resistance of the battery and ultimately leads to the failure of the battery.

Method used

Carbon nanosphere-based composite electrode slurry is used to form an electric double layer through non-ionic conductivity/energy storage characteristics using carbon materials to adsorption and desorption electrons. The electrolyte is maintained uniformly and stable with surface modification technology to avoid pooling and blockage.

Benefits of technology

Fast charging and discharging are achieved, effectively avoiding the problem of sinking and blocking during the use of the battery, and improving the battery's energy and coulomb efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004215148550000011
    Figure HDA0004215148550000011
  • Figure HDA0004215148550000021
    Figure HDA0004215148550000021
Patent Text Reader

Abstract

The invention discloses electrode slurry and a preparation method and application thereof. The preparation method of the electrode slurry comprises the following steps: step (1), dissolving nickel nitrate, sodium hydroxide, ascorbic acid and citric acid betaine in water to obtain a solution B; and (2) mixing the solution B with an aqueous solution containing a carbon source, and reacting I to obtain the electrode slurry. The prepared high-concentration carbon nanosphere composite material electrode slurry has the characteristics of non-ionic conduction / energy storage, double electric layers are formed by using the carbon material to adsorb and desorb electrons so as to achieve the purpose of rapid charging and discharging, and the prepared carbon nanosphere slurry can keep the uniformity and stability of an electrolyte by using a surface modification mode; and the problem of battery failure caused by blockage of a battery pipeline due to coagulation and increase of internal resistance of the battery in a battery using process can be effectively avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to an electrode slurry and a preparation method and application thereof, belonging to the technical field of liquid flow type supercapacitors. Background Art

[0002] Energy storage technology has become a key technology for making full use of intermittent renewable energy such as wind and solar energy. In the past two decades, major breakthroughs have been made in the field of energy storage technology, including the development of emerging technologies such as batteries and supercapacitors, which mainly solve the problem of small-scale energy storage. Recently, technologies such as lead-carbon battery energy storage technology, liquid flow battery energy storage technology, molten salt battery (mainly Na-S), and all-solid-state lithium-ion battery energy storage technology are expected to become future products of large-scale energy storage technology.

[0003] Liquid flow battery energy storage technology is different from other types of battery energy storage technologies. Its uniqueness lies in that this technology can decouple energy density and power density. In other words, the battery storage capacity is determined by the size of the electrolyte storage tank, while the battery power depends on the size of the battery stack and the electrochemical process during charging and discharging. In order to further improve the power density of liquid flow batteries, the successful development and application of liquid flow supercapacitors in the energy storage market is the biggest opportunity and challenge facing this technology. Compared with battery energy storage, supercapacitors have the characteristics of fast charging and discharging and strong resistance to large current shocks.

[0004] However, the current traditional liquid flow batteries have problems such as low power density, sedimentation of high-concentration liquid flow supercapacitor electrode slurry, and slurry blockage in the electrode. Summary of the invention

[0005] The present application provides an electrode slurry. The electrode slurry used in liquid flow supercapacitors has strong anti-aggregation ability and can form a uniform and stable electrolyte. Compared with other types of electrode slurries, the carbon nanosphere-based composite material electrode slurry provided by the present invention adopts the characteristics of non-ionic conductivity / energy storage, and uses the carbon material itself to adsorb and desorb electrons to form a double layer to achieve the purpose of rapid charging and discharging. The prepared carbon nanosphere slurry uses surface modification to maintain the uniformity and stability of the electrolyte, which can effectively avoid the problem of aggregation during battery use, which blocks the battery pipeline, increases the internal resistance of the battery, and ultimately causes the battery to fail.

[0006] According to one aspect of the present application, a method for preparing an electrode slurry is provided, comprising the following steps:

[0007] Step (1), dissolving nickel nitrate, sodium hydroxide, ascorbic acid and betaine citrate in water to obtain solution B;

[0008] Step (2), mixing the solution B with an aqueous solution containing a carbon source, reacting I, and obtaining an electrode slurry.

[0009] Optionally, step (2) further includes the following steps:

[0010] Step (2-1), placing the aqueous solution containing the carbon source in a hydrothermal reactor for reaction II, and centrifuging to obtain a carbon nanosphere solution;

[0011] Step (2-2), mixing the solution B with the carbon nanosphere solution to react I to obtain an electrode slurry.

[0012] Optionally, in step (2-1), the solid-to-liquid ratio of the carbon source to water in the aqueous solution containing the carbon source is 2-200 g:500-1000 mL.

[0013] Optionally, in step (2-1), the solid-to-liquid ratio of the carbon source to water in the aqueous solution containing the carbon source is selected from any ratio of 2g:500mL, 47.922g:700mL, 100g:750mL, 200g:1000mL or a range between two ratios.

[0014] Optionally, in step (2-1), the carbon source is selected from at least one of sucrose, glucose, xylitol and starch.

[0015] Optionally, in step (2-1), the conditions of reaction II are: temperature 100-300° C., time 1-24 h.

[0016] Optionally, in step (2-1), the temperature of reaction II is any value among 100°C, 180°C, 300°C, or a range between two values.

[0017] Optionally, in step (2-1), the time of reaction II is any value among 1h, 12h, 24h, or a range between two values.

[0018] Optionally, in step (2-1), the centrifugal speed is 3000 to 20000 rpm, and the centrifugal time is 0.1 to 30 min.

[0019] Optionally, in step (1), the solution B comprises, by mass:

[0020] 100-300 parts of nickel nitrate;

[0021] 2-200 parts of sodium hydroxide;

[0022] 4-400 parts of ascorbic acid;

[0023] 4-400 parts of betaine citrate;

[0024] 500-1000 parts of water.

[0025] Optionally, in step (2), the conditions of reaction I are: temperature 40-300° C., time 0.1-24 h.

[0026] Optionally, in step (2), the temperature of the reaction I is any value of 40°C, 80°C, 120°C, 200°C, 300°C, or a range between two values.

[0027] Optionally, in step (2), the reaction time I is any value among 0.1h, 2h, 5h, 10h, 24h, or a range between two values.

[0028] Optionally, the volume ratio of the carbon nanosphere solution to solution B is 1:0.001-1000.

[0029] According to another aspect of the present application, there is provided an electrode slurry obtained according to the above preparation method, comprising carbon nanospheres and nickel hydroxide, wherein the nickel hydroxide is loaded on the surface of the carbon nanospheres in the form of atomic clusters;

[0030] Optionally, the diameter of the carbon nanospheres is 5 to 500 nm.

[0031] Optionally, the diameter of the nickel hydroxide atomic cluster is 0.1 to 10 nm.

[0032] Optionally, the mass of the nickel hydroxide accounts for 0.1 to 95% of the total mass of the electrode slurry.

[0033] Optionally, the concentration of carbon nanospheres in the electrode slurry is 0.001-100 g / mL, wherein the concentration of the electrode slurry is 0.001-100 g / mL according to the mass of the carbon nanosphere composite material obtained after drying in the entire slurry solution.

[0034] According to another aspect of the present application, a liquid flow type supercapacitor is provided, comprising a positive electrode, a negative electrode and an electrolyte, wherein the positive electrode and the negative electrode are coated with the above-mentioned electrode slurry;

[0035] The electrolyte is the above-mentioned electrode slurry.

[0036] The beneficial effects of this application include:

[0037] 1) The preparation method of the electrode slurry provided in the present application prepares a high-concentration carbon nanosphere composite material electrode slurry, which has the characteristics of non-ionic conductivity / energy storage. The prepared carbon nanosphere composite material itself adsorbs and desorbs the electrode to form a double electric layer to achieve the purpose of rapid charging and discharging.

[0038] 2) The liquid flow supercapacitor provided in the present application, the positive and negative electrodes and the electrolyte all adopt the electrode slurry prepared in the present application, and the carbon nanospheres in the electrode slurry are modified in a manner so that the electrolyte can be kept uniform and stable, which can effectively avoid the problem of flocculation during the use of the battery, clogging the battery pipeline, increasing the internal resistance of the battery and ultimately causing the battery to fail. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 This is a transmission electron microscopy image of carbon nanospheres loaded with nickel hydroxide atomic clusters on the surface of the electrode slurry prepared in Example 1 of the present application;

[0040] Figure 2 This is a transmission electron micrograph of the electrode slurry product prepared in Comparative Example 5 of the present application. DETAILED DESCRIPTION

[0041] The present application is described in detail below with reference to embodiments, but the present application is not limited to these embodiments.

[0042] Unless otherwise specified, the raw materials in the examples of this application were purchased through commercial channels.

[0043] Example 1

[0044] Step 1: Preparation of electrode slurry:

[0045] (1) Preparation of carbon nanosphere solution: 47.922 g of sucrose was dissolved in 700 ml of ultrapure water. The solution was transferred to a 1000 ml hydrothermal kettle and kept at 180 °C for 12 hours. The carbon nanospheres in the product were collected by high-speed centrifugation. The centrifuge was operated at 7500 rpm for 5 minutes to collect the product. The supernatant (800 ml) obtained by centrifugation was named solution A for the next step of slurry preparation.

[0046] (2) Preparation of electrode slurry: 145.395 g of nickel nitrate, 20 g of sodium hydroxide, 40 g of ascorbic acid, and 40 g of betaine citric acid were mixed in 2000 ml of ultrapure water, and 800 ml of the obtained solution was named solution B. Solution A and solution B were fully mixed and kept at 80° C. for 2 hours, and then naturally cooled to obtain electrode slurry.

[0047] The electrode slurry was photographed by transmission electron microscopy (TEM). Figure 1 As shown, according to Figure 1 It can be seen that the nickel hydroxide atomic clusters are uniformly loaded on the surface of the carbon nanospheres, wherein the diameter of the carbon nanospheres is about 40-50nm, and the diameter of the nickel hydroxide atomic clusters is about 1-5nm. The prepared composite material was subjected to a thermogravimetric test, and the test results showed that the mass of nickel hydroxide accounted for about 30% of the total mass of the composite material.

[0048] Step 2: Assembly of liquid flow supercapacitor:

[0049] The positive and negative electrolytes have the same composition, both consisting of the electrode slurry prepared in step one.

[0050] Assembly of single battery:

[0051] The structure of a single cell consists of end plates, graphite plate current collectors, 6cm X 8cm carbon felt as positive and negative electrodes, Daramic 900μm polyethylene membrane as porous membrane, liquid flow frame, silicone pad, positive and negative electrolyte storage tanks and pumps, and pipelines.

[0052] The test conditions of battery performance are: the flow rate of electrolyte (positive and negative electrolyte) in the battery is 50ml / min, the charging current is 60mA / cm2, the charging cut-off voltage is 1.4V, the discharging cut-off voltage is 0.1V, and the charging capacity is 20Ah / L. The average values ​​of coulomb efficiency CE, voltage efficiency VE, and energy efficiency EE in the first 100 cycles of charge and discharge cycles are detected. The test results show that the battery assembled with the electrode slurry of this embodiment has an energy efficiency of 80% and a coulomb efficiency of 94.1%.

[0053] Example 2

[0054] According to the requirements of Example 1, without changing other conditions, the amount of sucrose added in step 1, step (1) is changed to 2g. The diameter of the prepared carbon nanospheres is about 5-10nm, and the diameter of the nickel hydroxide atomic clusters is about 1-5nm. The prepared composite material was subjected to thermogravimetric testing, and the test results showed that the mass of nickel hydroxide accounted for about 90% of the total mass of the composite material. The energy efficiency of the assembled liquid flow supercapacitor was 83%, and the coulombic efficiency was 91.8%.

[0055] Example 3

[0056] According to the requirements of Example 1, without changing other conditions, the amount of sucrose added in step 1, step (1) is changed to 200g. The diameter of the prepared carbon nanospheres is about 400-450nm, and the diameter of the nickel hydroxide atomic cluster is about 1-5nm. The prepared composite material is subjected to thermogravimetric testing, and the test results show that the mass of nickel hydroxide accounts for about 10% of the total mass of the composite material. The energy efficiency of the assembled liquid flow supercapacitor is 79%, and the coulombic efficiency is 90.3%.

[0057] Example 4

[0058] According to the requirements of Example 1, without changing other conditions, the amount of nickel nitrate added in step 1 and step (2) was changed to 100g. The diameter of the prepared carbon nanospheres was about 40-50nm, and the diameter of the nickel hydroxide atomic clusters was about 0.1-1nm. The prepared composite material was subjected to thermogravimetric testing, and the test results showed that the mass of nickel hydroxide accounted for about 20% of the total mass of the composite material. The energy efficiency of the assembled liquid flow supercapacitor was 78%, and the coulombic efficiency was 92.7%.

[0059] Example 5

[0060] According to the requirements of Example 1, without changing other conditions, the amount of nickel nitrate added in step 1 and step (2) was changed to 300g. The diameter of the prepared carbon nanospheres was about 40-50nm, and the diameter of the nickel hydroxide atomic clusters was about 5-10nm. The prepared composite material was subjected to thermogravimetric testing, and the test results showed that the mass of nickel hydroxide accounted for about 40% of the total mass of the composite material. The energy efficiency of the assembled liquid flow supercapacitor was 76%, and the coulombic efficiency was 90.4%.

[0061] Example 6

[0062] According to the requirements of Example 1, without changing other conditions, the amount of sodium hydroxide added in step 1 and step (2) was changed to 2g. The diameter of the prepared carbon nanospheres was about 40-50nm, and the diameter of the nickel hydroxide atomic clusters was about 5-10nm. The prepared composite material was subjected to thermogravimetric testing, and the test results showed that the mass of nickel hydroxide accounted for about 30% of the total mass of the composite material. The energy efficiency of the assembled liquid flow supercapacitor was 82%, and the coulombic efficiency was 92.8%.

[0063] Example 7

[0064] According to the requirements of Example 1, without changing other conditions, the amount of sodium hydroxide added in step 1 and step (2) was changed to 200g. The diameter of the prepared carbon nanospheres was about 40-50nm, and the diameter of the nickel hydroxide atomic clusters was about 5-10nm. The prepared composite material was subjected to thermogravimetric testing, and the test results showed that the mass of nickel hydroxide accounted for about 35% of the total mass of the composite material. The energy efficiency of the assembled liquid flow supercapacitor was 81%, and the coulombic efficiency was 93.2%.

[0065] Example 8

[0066] According to the requirements of Example 1, without changing other conditions, the amount of ascorbic acid added in step 1 and step (2) is changed to 4g. The diameter of the prepared carbon nanospheres is about 40-50nm, and the diameter of the nickel hydroxide atomic clusters is about 0.1-1nm. The prepared composite material was subjected to thermogravimetric testing, and the test results showed that the mass of nickel hydroxide accounted for about 10% of the total mass of the composite material. The energy efficiency of the assembled liquid flow supercapacitor was 77%, and the coulombic efficiency was 90.5%.

[0067] Example 9

[0068] According to the requirements of Example 1, without changing other conditions, the amount of ascorbic acid added in step 1 and step (2) was changed to 400g. The diameter of the prepared carbon nanospheres was about 40-50nm, and the diameter of the nickel hydroxide atomic clusters was about 5-10nm. The prepared composite material was subjected to thermogravimetric testing, and the test results showed that the mass of nickel hydroxide accounted for about 30% of the total mass of the composite material. The energy efficiency of the assembled liquid flow supercapacitor was 80%, and the coulombic efficiency was 94.3%.

[0069] Example 10

[0070] According to the requirements of Example 1, without changing other conditions, the amount of betaine citric acid added in step 1 and step (2) was changed to 4g. The diameter of the prepared carbon nanospheres was about 40-50nm, and the diameter of the nickel hydroxide atomic clusters was about 0.1-1nm. The prepared composite material was subjected to thermogravimetric testing, and the test results showed that the mass of nickel hydroxide accounted for about 5% of the total mass of the composite material. The energy efficiency of the assembled liquid flow supercapacitor was 79%, and the coulombic efficiency was 92.7%.

[0071] Embodiment 11

[0072] According to the requirements of Example 1, without changing other conditions, the amount of betaine citric acid added in step 1 and step (2) was changed to 400g. The diameter of the prepared carbon nanospheres is about 40-50nm, and the diameter of the nickel hydroxide atomic clusters is about 0.1-1nm. The prepared composite material was subjected to thermogravimetric testing, and the test results showed that the mass of nickel hydroxide accounted for about 35% of the total mass of the composite material. The energy efficiency of the assembled liquid flow supercapacitor was 83%, and the coulombic efficiency was 93.3%.

[0073] Example 12

[0074] According to the requirements of Example 1, without changing other conditions, the step 1, step (1) "transfer the solution to a 1000ml hydrothermal kettle and keep it warm in an environment of 180°C for 12 hours" is changed to "transfer the solution to a 1000ml hydrothermal kettle and keep it warm in an environment of 100°C for 12 hours". The diameter of the prepared carbon nanospheres is about 5-20nm, and the diameter of the nickel hydroxide atomic clusters is about 5-10nm. The prepared composite material was subjected to thermogravimetric testing, and the test results showed that the mass of nickel hydroxide accounted for about 40% of the total mass of the composite material. The energy efficiency of the assembled liquid flow supercapacitor is 75%, and the coulombic efficiency is 90.8%.

[0075] Embodiment 13

[0076] According to the requirements of Example 1, without changing other conditions, the step 1, step (1) "transfer the solution to a 1000ml hydrothermal kettle and keep it warm in an environment of 180°C for 12 hours" is changed to "transfer the solution to a 1000ml hydrothermal kettle and keep it warm in an environment of 300°C for 12 hours". The diameter of the prepared carbon nanospheres is about 200-300nm, and the diameter of the nickel hydroxide atomic clusters is about 5-10nm. The prepared composite material was subjected to thermogravimetric testing, and the test results showed that the mass of nickel hydroxide accounted for about 25% of the total mass of the composite material. The energy efficiency of the assembled liquid flow supercapacitor is 84%, and the coulombic efficiency is 91.2%.

[0077] Embodiment 14

[0078] According to the requirements of Example 1, without changing other conditions, the step 1, step (2) "mix solution A and solution B thoroughly and keep them in an 80°C environment for 2 hours" is changed to "mix solution A and solution B thoroughly and keep them in a 40°C environment for 5 hours". The diameter of the prepared carbon nanospheres is about 40-50nm, and the diameter of the nickel hydroxide atomic clusters is about 1-5nm. The prepared composite material was subjected to thermogravimetric testing, and the test results showed that the mass of nickel hydroxide accounted for about 35% of the total mass of the composite material. The energy efficiency of the assembled liquid flow supercapacitor was 82%, and the coulombic efficiency was 92.5%.

[0079] Embodiment 15

[0080] According to the requirements of Example 1, without changing other conditions, the step 1, step (2) "mix solution A and solution B thoroughly and keep them in an environment of 80°C for 2 hours" is changed to "mix solution A and solution B thoroughly and keep them in an environment of 200°C for 2 hours". The diameter of the prepared carbon nanospheres is about 40-50nm, and the diameter of the nickel hydroxide atomic clusters is about 5-10nm. The prepared composite material was subjected to thermogravimetric testing, and the test results showed that the mass of nickel hydroxide accounted for about 45% of the total mass of the composite material. The energy efficiency of the assembled liquid flow supercapacitor is 80%, and the coulombic efficiency is 91.5%.

[0081] Example 16

[0082] Intrinsic electrochemical performance test of carbon nanosphere supercapacitor:

[0083] According to the requirements of Example 1, without changing other conditions, step 2 is changed to:

[0084] Preparation of carbon nanosphere supercapacitor:

[0085] Carbon nanospheres, acetylene black, PTFE binder, and ultrapure water were ball-milled in a mass ratio of 80g:10g:10g:100g, and 1g of the mixed product was filled on the surface and pores of nickel foam. A three-electrode system test was carried out on an electrochemical workstation. During the test, the prepared nickel foam electrode was used as a working electrode, the platinum electrode was used as a counter electrode, and the silver / silver chloride electrode was used as a reference electrode. During the test, the working electrode was charged and discharged for 100 times at a current density of 10A / g, and the discharge specific capacitance of the 100th charge and discharge cycle was 1500F / g, and the corresponding coulomb efficiency was 98.9%.

[0086] Comparative Example 1

[0087] According to the requirements of Example 1, without changing other conditions, the amount of sucrose added in step 1, step (1) was changed to 0.1 g. Since the yield of carbon nanospheres in liquid A was too low, it was impossible to form a uniform and stable electrode slurry. As a result, the energy efficiency of the assembled liquid flow supercapacitor was 66% and the coulombic efficiency was 83.3%.

[0088] Comparative Example 2

[0089] According to the requirements of Example 1, without changing other conditions, the amount of nickel nitrate added in step 1 and step (2) was changed to 50 g. Since the amount of nickel nitrate added in liquid B was too low, too few nickel hydroxide atomic clusters were generated on the surface of the carbon nanospheres, and the product flocculation phenomenon was serious, and a stable electrode slurry could not be generated. As a result, the energy efficiency of the assembled liquid flow supercapacitor was 68%, and the coulomb efficiency was 83.6%.

[0090] Comparative Example 3

[0091] According to the requirements of Example 1, without changing other conditions, the amount of nickel nitrate added in step 1 and step (2) was changed to 550 g. Due to the excessive amount of nickel nitrate added in solution B, a nickel hydroxide shell with a thickness of 5 nm was generated on the surface of the carbon nanospheres, and the product flocculation phenomenon was serious, and a stable electrode slurry could not be generated. As a result, the energy efficiency of the assembled liquid flow supercapacitor was 61%, and the coulombic efficiency was 81.0%.

[0092] Comparative Example 4

[0093] According to the requirements of Example 1, without changing other conditions, the amount of ascorbic acid added in step 1 and step (2) was changed to 0.5 g. Since the amount of reducing agent added to the mixed solution A and B was too small, the product was not uniform, and a uniform and stable electrode slurry could not be formed. As a result, the energy efficiency of the assembled liquid flow supercapacitor was 69%, and the coulombic efficiency was 80.1%.

[0094] Comparative Example 5

[0095] According to the requirements of Example 1, without changing other conditions, the step 1, step (1) "transferring the solution to a 1000 ml hydrothermal kettle and keeping it at 180°C for 12 hours" was changed to "transferring the solution to a 1000 ml hydrothermal kettle and keeping it at 50°C for 12 hours". Since solution A cannot generate uniform and stable carbon nanospheres, Figure 2 As shown, it is impossible to form a uniform and stable electrode slurry. As a result, the energy efficiency of the assembled liquid flow supercapacitor is 64% and the coulombic efficiency is 82.3%.

[0096] Comparative Example 6

[0097] According to the requirements of Example 1, without changing other conditions, the step 1, step (2) "mix solution A and solution B thoroughly and keep them in an environment of 80°C for 2 hours" is changed to "mix solution A and solution B thoroughly and keep them in an environment of 10°C for 2 hours". Since the temperature of the mixed solution A and B is too low, the thermodynamic basic conditions of the reducing agent reaction cannot be reached, resulting in uneven products and the inability to form a uniform and stable electrode slurry. As a result, the energy efficiency of the assembled liquid flow supercapacitor is 62%, and the coulombic efficiency is 84.3%.

[0098] Comparative Example 7

[0099] According to the requirements of Example 1, without changing other conditions, the amount of betaine citric acid added in step 1 and step (2) was changed to 0g. If betaine citric acid is not added to the reaction solution, uniformly grown nickel atomic clusters cannot be prepared on the surface of the carbon nanospheres, resulting in the inability to form a uniform and stable electrode slurry. The energy efficiency of the assembled liquid flow supercapacitor is 40%, and the coulombic efficiency is 46.6%.

[0100] The above are only a few embodiments of the present application and do not constitute any form of limitation to the present application. Although the present application is disclosed as above with preferred embodiments, it is not intended to limit the present application. Any technician familiar with the profession, without departing from the scope of the technical solution of the present application, using the technical content disclosed above to make slight changes or modifications are equivalent to equivalent implementation cases and fall within the scope of the technical solution.

Claims

1. A method for preparing an electrode slurry, characterized in that: The following steps are involved: Step (1), dissolving nickel nitrate, sodium hydroxide, ascorbic acid and betaine citrate in water to obtain solution B; Step (2), mixing the solution B with an aqueous solution containing a carbon source, reacting I, and obtaining an electrode slurry.

2. The preparation method according to claim 1, characterized in that: Step (2) also includes the following steps: Step (2-1), placing the aqueous solution containing the carbon source in a hydrothermal reactor for reaction II, and centrifuging to obtain a carbon nanosphere solution; Step (2-2), mixing the solution B with the carbon nanosphere solution to react I to obtain an electrode slurry.

3. The preparation method according to claim 2, characterized in that: In step (2-1), the solid-to-liquid ratio of the carbon source to water in the aqueous solution containing the carbon source is 2-200 g:500-1000 mL.

4. The preparation method according to claim 2, characterized in that: In step (2-1), the carbon source is selected from at least one of sucrose, glucose, xylitol and starch.

5. The preparation method according to claim 2, characterized in that: In step (2-1), the conditions of reaction II are: temperature 100-300° C., time 1-24 h.

6. The preparation method according to claim 2, characterized in that: In step (2-1), the centrifugal speed is 3000 to 20000 rpm, and the centrifugal time is 0.1 to 30 min.

7. The preparation method according to claim 1, characterized in that: In step (1), the solution B comprises, by mass: 100-300 parts of nickel nitrate; 2-200 parts of sodium hydroxide; 4-400 parts of ascorbic acid; 4-400 parts of betaine citrate; 500-1000 parts of water.

8. The preparation method according to claim 1, characterized in that: In step (2), the conditions of reaction I are: temperature 40-300° C., time 0.1-24 h.

9. An electrode slurry obtained according to the preparation method according to any one of claims 1 to 8, characterized in that: It comprises carbon nanospheres and nickel hydroxide, wherein the nickel hydroxide is loaded on the surface of the carbon nanospheres in the form of atomic clusters; Preferably, the diameter of the carbon nanospheres is 5 to 500 nm; Preferably, the diameter of the nickel hydroxide atomic cluster is 0.1 to 10 nm; Preferably, the mass of the nickel hydroxide accounts for 0.1 to 95% of the total mass of the electrode slurry; Preferably, the concentration of carbon nanospheres in the electrode slurry is 0.001-100 g / mL.

10. A liquid flow supercapacitor, characterized in that: including a positive electrode, a negative electrode and an electrolyte; The surfaces of the positive electrode and the negative electrode are coated with the electrode slurry according to claim 9; The electrolyte is the electrode slurry according to claim 9.