Preparation method of flexible BP-coated Ti < 3 > C < 2 > T < x > composite material integrated electrode

The black phosphorus and Ti3C2Tx are mixed into thin film electrodes through suction filtration, which solves the problems of black phosphorus electrode oxidation and volume expansion, and realizes a flexible and efficient negative electrode material of lithium-ion battery, improving circulation performance and capacity.

CN118899388APending Publication Date: 2024-11-05JILIN NORMAL UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410966445.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

As a lithium-ion battery electrode material, black phosphorus is easily oxidized and volume expansion during charging and discharging leads to structure rupture, affecting its cycling performance. The prior art is difficult to effectively solve these problems.

Method used

The black phosphorus and Ti3C2Tx were mixed by suction filtration to form a film electrode, and the BP@Ti3C2Tx composite film was formed by ultraviolet irradiation, and cut into small sheets to prepare a flexible integrated electrode, and the use of conductive agents and binders were omitted.

Benefits of technology

It improves the cycling performance and flexibility of the electrode, reduces the production cost, is suitable for wearable electronic devices, and significantly improves the negative electrode capacity and cycle stability of lithium-ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118899388A_ABST
    Figure CN118899388A_ABST
Patent Text Reader

Abstract

The invention relates to a preparation method of a flexible BP-coated Ti < 3 > C < 2 > T < x > composite material integrated electrode. The preparation method comprises the following steps: preparing filter paper, placing BP and Ti3C2Tx on the filter paper, carrying out suction filtration to form a film, carrying out ultraviolet radiation treatment on the formed film to obtain a BP-coated Ti3C2Tx composite material film, and finally cutting the treated film into small sheets to successfully prepare the flexible BP-coated Ti3C2Tx composite material integrated electrode. According to the method, the electrode is prepared through the simple pure physical method with extremely low energy consumption, harsh experimental conditions are not needed, the operation is simple, and a large number of thin film integrated electrodes can be prepared.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of electrode preparation method, specifically a flexible BP@Ti3C2T x A method for preparing a composite material integrated electrode. Background Art

[0002] Black phosphorus (BP) is a highly regarded battery electrode material, especially as a new cathode material for lithium-ion and sodium-ion batteries. Black phosphorus has some remarkable properties, including its unique layered structure, high specific surface area, and potential high energy and high power performance as an electrode. Black phosphorus electrodes have shown great advantages in research, such as the theoretical specific capacity of black phosphorus is as high as about 2600mAh / g, which greatly exceeds the traditional graphite anode material (about 372mAh / g). Due to its layered structure, black phosphorus electrodes can provide excellent ion transport channels, which is conducive to rapid ion movement, which is conducive to high-speed charging and discharging. However, black phosphorus as a battery electrode material also faces great challenges: for example, in conventional atmospheric environments, black phosphorus is easily oxidized, resulting in the attenuation of its electrochemical performance. In order to improve its stability, black phosphorus needs to be protected by strategies such as surface coating and structural stabilization. Secondly, during the charge and discharge process, black phosphorus will expand by more than 300%, which may cause structural rupture and reduce the cycle performance. Faced with these problems, researchers are using a variety of strategies to improve the performance of black phosphorus electrodes, such as using various materials (such as carbon materials, metal oxides, etc.) to modify the black phosphorus surface to protect black phosphorus from oxidation and maintain its structural integrity. Mixing with other conductive materials to form a black phosphorus composite electrode to improve conductivity and slow down volume expansion. Develop nanostructured black phosphorus, such as black phosphorus nanosheets or nanorods, to provide higher surface area and space for buffering volume expansion. There is also the application of solid electrolytes: combining black phosphorus with solid electrolytes can provide good interfacial contact and improve overall battery safety. Although black phosphorus electrode materials face challenges in the application of lithium-ion batteries, their high specific capacity and potential for rapid ion conduction make it an active research field. Through continuous research and technological innovation, black phosphorus may be able to make breakthroughs in the field of high-performance battery electrodes in the future.

[0003] Ti3C2T x As a member of the MXenes family, research progress in the field of lithium batteries is remarkable. MXenes are a class of two-dimensional materials composed of layered transition metal carbides and / or nitrides, among which Ti3C2T x Due to its excellent electrical conductivity, high specific surface area and good ion transport performance, it shows great application potential in lithium-ion batteries. xDue to its high electrical conductivity and special layered structure, it exhibits good electrochemical performance during lithium ion insertion and extraction. x It can achieve higher charge and discharge capacity and cycle stability. Its performance can be further improved through modification and composite methods. It can also be composited with other electrode materials (such as graphite, silicon, phosphorus, sulfur, etc.), which can significantly improve the electronic conductivity and ion diffusion properties of these materials. These composite materials show higher specific capacity, cycle stability and charge and discharge efficiency. As an electrode material for supercapacitors, it also shows excellent energy storage performance. Their application in supercapacitor electrodes, especially in combination with other functional materials, shows high energy density and power density. Also using Ti3C2T x The layered structure and surface functional groups can improve the electrolyte performance of lithium-ion batteries, for example, by x The lithium ion conduction channel is introduced at the layer level to improve the lithium ion transmission efficiency and the overall performance of the battery. x Surface functionalization is currently a research hotspot. This strategy aims to improve the insertion / extraction kinetics of lithium ions and the overall performance of the battery by regulating the interaction of the electrode / electrolyte interface.

[0004] Thin film electrodes are a technology used in lithium-ion batteries and other types of batteries such as solid-state batteries. They have many unique advantages, such as high energy density, high power density, better mechanical stability, and material conservation. With the continuous advancement of technology, we may see more batteries based on thin film electrodes being popularized in various applications in the future. Summary of the invention

[0005] The purpose of the present invention is to provide a flexible BP@Ti3C2T x The method for preparing a composite material integrated electrode is to prepare the electrode by a simple, extremely low energy consumption, purely physical method such as filtration. It does not require harsh experimental conditions, is easy to operate, and can prepare a large number of thin film integrated electrodes.

[0006] The technical solution of the present invention:

[0007] A flexible BP@Ti3C2T x Preparation method of composite material integrated electrode, preparing filter paper, mixing BP and Ti3C2T x The film was placed on filter paper and filtered to form a thin film. The film was treated with ultraviolet light to obtain BP@Ti3C2T x Composite material film, and finally cut the processed film into small sheets to successfully produce flexible BP@Ti3C2T x Composite material integrated electrode.

[0008] The BP and Ti3C2T x Place it on filter paper and perform the filtration step. The detailed steps are as follows: First, Ti3C2T x The suspension was filtered to form a thin film, and then the BP particle suspension was filtered to the newly formed Ti3C2T x The Ti3C2T x The suspension was filtered onto the top of the BP membrane.

[0009] The BP and Ti3C2T x Place it on the filter paper and perform the filtration step. The detailed steps are as follows: BP and Ti3C2T x The phases were mixed until uniform, and then slowly poured into deionized water. The uniform suspension was filtered on filter paper. During the filtration process, the solvent in the suspension was effectively removed. At the same time, BP and Ti3C2T x Evenly distributed on the surface of the filter paper, gradually forming a continuous and uniform film.

[0010] Beneficial effects of the present invention:

[0011] 1. The present application prepares electrodes by a simple, low-energy, purely physical method called filtration, which does not require harsh experimental conditions, is easy to operate, and can prepare a large number of thin-film integrated electrodes.

[0012] 2. Compared with the traditional integrated electrode preparation method, the present application omits the use of conductive agent and binder. Moreover, the integrated electrode is a flexible electrode and can be applied to wearable electronic devices.

[0013] 3. This application conducted electrochemical tests on the integrated electrode prepared by filtration as the negative electrode of lithium-ion batteries and found that the cycle performance was improved. This is because black phosphorus reacts with Ti3C2T x The samples interacted to form Ti-OP bonds, Ti3C2T x It effectively alleviates the volume expansion problem of black phosphorus during lithium insertion and extraction, and improves the cycle performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings in the following description are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.

[0015] Figure 1 X-ray diffraction (XRD) spectra of flexible integrated electrodes prepared by different filtration methods.

[0016] Figure 2 Scanning electron microscope (SEM) images and analogy images of sandwich-type and mosaic-type flexible integrated electrodes.

[0017] Figure 3 Raman images of flexible integrated electrodes prepared by different filtration methods.

[0018] Figure 4 O1s XPS graphs of the integrated electrodes formed by different filtration methods.

[0019] Figure 5 Cyclic images of different filtration methods (at 1C (1C = 100mAg -1 ) at a current density of ).

[0020] Figure 6 BP@Ti3C2T with different filtration methods x Electrochemical impedance spectroscopy (EIS) image of the flexible integrated electrode.

[0021] Figure 7-Figure 8 BP@Ti3C2T with different filtration methods x Cyclic voltammetry characteristic curves of the flexible integrated electrode with different numbers of turns. DETAILED DESCRIPTION

[0022] In order to solve the problems existing in the background technology, the present invention has invented a method of using suction filtration to separate black phosphorus and Ti3C2T x The invention discloses a method for preparing an integrated flexible electrode by filtering a thin film.

[0023] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0024] The purpose of the present invention is to overcome the shortcomings of the prior art and prepare BP@Ti3C2T x The flexible integrated electrode of the present invention has the advantages of simple operation and easy achievement of experimental conditions.

[0025] The present invention combines black phosphorus with Ti3C2T x Filtering, without introducing additional impurities and high temperature, BP@Ti3C2T was prepared in one go. x Flexible integrated electrode, first, prepare filter paper, BP and Ti3C2T xThe film was placed on filter paper and filtered to form a thin film. The film was treated with ultraviolet light to obtain BP@Ti3C2T x Composite material film, and finally cut the processed film into small sheets to successfully produce flexible BP@Ti3C2T x Composite material integrated electrode. The detailed steps are as follows:

[0026] Preparation process of "sandwich" type thin film integrated electrode:

[0027] First, a filter paper with a diameter of 47 mm and a pore size of 0.22 μm was used for the filtration process: 20 ml of Ti3C2T x The suspension was filtered to form a thin film; then 20 ml of BP particle suspension with a concentration of 5 mg / ml was filtered to the newly formed Ti3C2T x Finally, 20 ml of 5 mg / ml Ti3C2T x The suspension was filtered onto the top of BP. Then, the formed laminated structure was irradiated with UV light for 5 min to obtain a "sandwich" BP@Ti3C2T x Finally, the film was cut into small slices with a diameter of 12 mm using a 12 mm slicer, and a "sandwich" type thin film integrated electrode was successfully prepared.

[0028] Preparation process of "inlaid" thin film integrated electrode:

[0029] First, during the preparation process, 5 mg of black phosphorus (BP) was mixed with 10 mg of Ti3C2T x The phases were mixed until uniform (relative standard deviation was less than ±5%), and then slowly poured into 60 ml of deionized water. To ensure that the two materials are fully mixed, an oscillator or manual shaking is required until a uniform dispersion is achieved (relative standard deviation is less than ±5%). This step is critical to the formation of high-quality composite film. Next, this uniform suspension was filtered on a precision filter paper with a diameter of 47 mm and a pore size of 0.22 μm. During the filtration process, the solvent in the suspension was effectively removed, and at the same time, BP and Ti3C2T x Evenly distributed on the surface of the filter paper, gradually forming a continuous and uniform film. After UV irradiation treatment, a structurally stable "mosaic" BP@Ti3C2T xComposite film. Finally, a 12 mm slicer was used to accurately cut the processed film into small slices with a diameter of 12 mm. These small slices are the successfully prepared "inlaid" thin film integrated electrodes. This study used the filtration method to prepare thin film integrated electrodes with different structures, characterized the structures of the "inlaid" thin film integrated electrodes and the "sandwich" thin film integrated electrodes, and tested their electrochemical properties.

[0030] Finally, we used the prepared "inlaid" and "sandwich" flexible integrated electrodes directly as negative electrode materials for electrochemical testing without applying any protective measures. The results showed that the sample capacities were 210mAh / g and 196mAh / g after 100 cycles, respectively, which was significantly improved compared to the original sample (pure black phosphorus: 40mAh / g).

[0031] Example

[0032] Select black phosphorus with a particle size of 1-5 μm and Ti3C2T with a size of 100-500 nm. x As raw material, 20 ml of Ti3C2T with a concentration of 5 mg / ml x The suspension was filtered to form a thin film; then 20 ml of BP particle suspension with a concentration of 5 mg / ml was filtered to the newly formed Ti3C2T x Finally, 20 ml of 5 mg / ml Ti3C2T x The suspension was filtered onto the BP film. Then, the formed "sandwich" structure was irradiated with UV light for 5 minutes to obtain a "sandwich" BP@Ti3C2T x The black phosphorus with a particle size of 1-5 μm and the Ti3C2T3 with a particle size of 100-500 nm were also selected. x As raw materials, 5 mg of black phosphorus (BP) and 10 mg of Ti3C2T x The phases were mixed until uniform (relative standard deviation was less than ±5%), and then slowly poured into 60 ml of deionized water. To ensure that the two materials are fully mixed, an oscillator or manual shaking is required until a uniform dispersion is achieved (relative standard deviation is less than ±5%). This step is critical to the formation of high-quality composite film. Next, this uniform suspension was filtered on a precision filter paper with a diameter of 47 mm and a pore size of 0.22 μm. During the filtration process, the solvent in the suspension was effectively removed, and at the same time, BP and Ti3C2T x Evenly distributed on the surface of the filter paper, gradually forming a continuous and uniform film. After UV irradiation treatment, a structurally stable "mosaic" BP@Ti3C2T x Composite film. Its XRD is as follows Figure 1 shown. Figure 2 It is a structural analogy diagram. Figure 3 This is the Raman image of the flexible integrated electrode prepared by the same filtration method. Figure 4 The O1s XPS images of the integrated electrodes formed by different filtration methods. x To investigate the electrochemical properties of the composite material, we assembled a half-cell. Lithium sheets were used as counter and reference electrodes. 1M LiPF6 solution (EC / DEC / EMC, 1:1:1 by volume) was used as the electrolyte. x Composite integrated electrodes were used as electrodes and commercial PP separators were used as separators. The batteries were assembled in a glove box in an argon environment with moisture and oxygen concentrations below 1 ppm. Figure 5 Cyclic images of different filtration methods (at 1C (1C = 100mAg -1 ) at a current density of Figure 6 BP@Ti3C2T with different filtration methods x Electrochemical impedance spectroscopy (EIS) image of the flexible integrated electrode. Figure 7 BP@Ti3C2T with different filtration methods x Cyclic voltammetry characteristic curves of the flexible integrated electrode with different numbers of turns.

[0033] This application flexible BP@Ti3C2T x The advantages of the preparation method of composite material integrated electrode are as follows:

[0034] 1. A flexible integrated electrode is formed by a purely physical method using a filtration method.

[0035] 2. The integrated electrode omits the traditional slurry coating process, greatly reduces the preparation process links, and at the same time eliminates the use of conductive agents and adhesives, reducing industrial production costs.

[0036] 3. The flexible integrated electrode prepared by the filtration method is the negative electrode. The performance is tested according to the assembled 2032-type button battery with commercial lithium iron phosphate as the positive electrode. It is found that the battery has better cycle capacity (the initial sample has a capacity of 40mAh / g after 100 cycles, and the "mosaic" flexible integrated electrode formed by filtration has a capacity of 210mAh / g after 100 cycles. The "sandwich-type" flexible integrated electrode formed by filtration has a capacity of 196mAh / g after 100 cycles.

[0037] The above schematically describes the present invention and its implementation methods, which are not restrictive. The drawings show only one implementation method of the present invention, and the actual structure is not limited thereto. Therefore, if a person skilled in the art is inspired by it and does not deviate from the technical solution of the present invention, and designs a structure and implementation similar to the technical solution based on the above implementation examples without creativity according to the technical essence of the present invention, they should all fall within the protection scope of the present invention.

Claims

1. A flexible BP@Ti3C2T x The method for preparing a composite material integrated electrode is characterized by: Prepare filter paper and mix BP and Ti3C2T x The film was placed on filter paper and filtered to form a thin film. The film was treated with ultraviolet light to obtain BP@Ti3C2T x Composite material film, and finally cut the processed film into small sheets to successfully produce flexible BP@Ti3C2T x Composite material integrated electrode.

2. A flexible BP@Ti3C2T according to claim 1 x The method for preparing a composite material integrated electrode is characterized by: The BP and Ti3C2T x Place it on the filter paper and perform the filtration step. The detailed steps are as follows: First, Ti3C2T x The suspension was filtered to form a thin film, and then the BP particle suspension was filtered to the newly formed Ti3C2T x The Ti3C2T x The suspension was filtered onto the top of the BP membrane.

3. A flexible BP@Ti3C2T according to claim 2 x The method for preparing a composite material integrated electrode is characterized by: First, a filter paper with a diameter of 47 mm and a pore size of 0.22 μm was used for the filtration process: 20 ml of Ti3C2T x The suspension was filtered to form a thin film, and then 20 ml of BP particle suspension with a concentration of 5 mg / ml was filtered to the newly formed Ti3C2T x Finally, 20 ml of 5 mg / ml Ti3C2T x The suspension was filtered onto the BP film, and then the formed laminated structure was irradiated with UV light for 5 minutes to obtain a "sandwich" BP@Ti3C2T x Finally, the film was cut into small slices with a diameter of 12 mm using a 12 mm slicer, and a "sandwich" type thin film integrated electrode was successfully prepared.

4. A flexible BP@Ti3C2T according to claim 1 x The method for preparing a composite material integrated electrode is characterized by: The BP and Ti3C2T x Place it on the filter paper and perform the filtration step. The detailed steps are as follows: BP and Ti3C2T x The phases were mixed until uniform, and then slowly poured into deionized water. The uniform suspension was filtered on filter paper. During the filtration process, the solvent in the suspension was effectively removed. At the same time, BP and Ti3C2T x Evenly distributed on the surface of the filter paper, gradually forming a continuous and uniform film.

5. A flexible BP@Ti3C2T according to claim 4 x The method for preparing a composite material integrated electrode is characterized by: First, during the preparation process, 5 mg of BP was mixed with 10 mg of Ti3C2T x Slowly pour into 60 ml of deionized water. To ensure that the two materials can be fully mixed, use an oscillator or shake manually until they are evenly dispersed. The relative standard deviation is less than ±5%. Next, filter the uniform suspension on a precision filter paper with a diameter of 47 mm and a pore size of 0.22 μm. During the filtration process, the solvent in the suspension is effectively removed. At the same time, BP and Ti3C2T x The BP@Ti3C2T nanostructured films were evenly distributed on the surface of the filter paper, gradually forming a continuous and uniform film. After UV irradiation, a structurally stable "mosaic" BP@Ti3C2T nanostructured films were obtained. x Composite material film, finally, use a 12 mm slicer to accurately cut the processed film into small thin slices with a diameter of 12 mm. These small thin slices are the successfully prepared "inlaid" type thin film integrated electrodes.

6. Flexible BP@Ti3C2T prepared by the preparation method according to any one of claims 1 to 5 x Composite material integrated electrode.

7. The flexible BP@Ti3C2T as claimed in claim 6 x Application of composite integrated electrodes as negative electrodes in lithium-ion batteries.