Double-active-component organic matter intercalation layered vanadium oxide positive electrode material, preparation method and application
By using a dual-active component organic carbonyl intercalated layered vanadium oxide positive electrode material in aqueous zinc ion batteries, the problem of poor electrochemical performance caused by structural changes in the electrode material during circulation is solved, and higher cycle stability is achieved and capacity, and the preparation method is safe and efficient.
Patent Information
- Application Number
- CN202410940053.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-11-05
AI Technical Summary
The electrode materials of aqueous zinc ion batteries have poor electrochemical properties due to structural changes during circulation, which limits their development, especially the collapse of inorganic materials and the easy soluble organic matter in electrolytes.
Using biactive components organic carbonyl interlayer layered vanadium oxide positive electrode material, the layer spacing is widened, and the kinetics of Zn2+ embedded in the vanadium oxide layer are used to utilize organic carbonyl small molecules or polymers. Stability prevents structure collapse and provides energy storage sites through carbonyl functional groups.
The cycle stability and capacity of the battery are improved, and the electrochemical performance and discharge specific capacity are achieved, and the preparation method is simple and without risk.
Smart Images

Figure CN118899415A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to an aqueous zinc ion battery positive electrode material, a preparation method and an application thereof, and specifically relates to a dual-active component organic intercalated layered vanadium oxide positive electrode material, a preparation method and an application thereof. Background Art
[0002] In the face of global energy and environmental issues, the development of sustainable and low-cost electrochemical energy storage devices is of great significance. Lithium-ion batteries are the most widely used, but their high price and high activity of lithium metal limit their large-scale application. In recent years, with the increasing requirements for the safety system of battery systems, the electrolyte of aqueous zinc-ion batteries has shown potential for application in large-scale energy storage due to its high safety and low cost. However, the narrow electrochemical stability window of aqueous electrolytes limits the choice of electrode materials. Currently, aqueous zinc-ion batteries mostly use inorganic compounds as electrode materials. Inorganic electrode materials based on the insertion / extraction mechanism will undergo structural collapse during repeated charging and discharging, resulting in poor electrochemical performance, which limits the development of aqueous zinc-ion batteries. In addition to inorganic substances, organic compounds as positive electrode materials for aqueous zinc-ion batteries are often easily soluble in electrolytes due to structural changes during the cycle process, resulting in low capacity and poor cycle performance.
[0003] Therefore, it is particularly important to solve the problem of poor electrochemical performance of inorganic and organic substances caused by structural changes during the cycle process. Summary of the invention
[0004] Purpose of the invention: The purpose of the present invention is to provide a dual-active component organic carbonyl intercalated vanadium oxide positive electrode material with superior performance, a synthesis preparation method and application.
[0005] The positive electrode material comprises a vanadium oxide layer, and an organic substance is embedded between the layers. The organic carbonyl is intercalated into a layered vanadium oxide compound in the form of a monomer / polymer.
[0006] Furthermore, the organic matter is an organic carbonyl small molecule or a polymer; and the layered vanadium oxide is V2O5, V2O3 or V3O7.
[0007] Here’s how it works:
[0008] (1) First, the vanadium oxide compounds are rearranged, and then organic carbonyl small molecules or polymers are directly embedded between the layered vanadium oxide compounds to widen the interlayer spacing, making Zn 2+ The kinetics of embedding and disembedding are accelerated;
[0009] (2) Organic matter that has formed a chain or a relatively large organic small molecule has its own stability and acts as a stabilizing "column" to prevent Zn 2+The structure of the layered inorganic material collapses during the insertion and extraction process, thereby improving the cycle stability;
[0010] (3) Organic matter contains carbonyl functional group structure, and the conversion of C=0 / C-0 bond during the charge and discharge process provides Zn 2+ binding sites, providing capacity.
[0011] Another aspect of the present invention provides a method for preparing a dual-active component organic intercalated layered vanadium oxide positive electrode material, comprising the following steps:
[0012] Step 1, dissolving a vanadium source in deionized water to obtain a solution A;
[0013] Step 2, adding a strong oxidant to solution A and performing ultrasonication to fully dissolve the solid and obtain solution B;
[0014] Step 3, adding an organic polymer to solution B, then pouring the mixed solution into a hydrothermal kettle for hydrothermal heating, cooling to room temperature, vacuum filtering the mixed solution to obtain a solid product, and vacuum drying to obtain a powder material.
[0015] Furthermore, in step 1, the molar concentration of the vanadium source dissolved in deionized water is 0.02-0.5 mol / L.
[0016] Furthermore, in step 1, the vanadium source is any one of vanadium pentoxide, vanadium dioxide, sodium metavanadate, vanadium acetylacetonate, vanadyl acetylacetonate, vanadium chloride, and vanadyl sulfate, or a combination of several of them.
[0017] Furthermore, the molar ratio of the vanadium source to the organic polymer is 1:(0.01-0.2).
[0018] Furthermore, in step 2, the strong oxidant is one or a combination of hydrogen peroxide, potassium persulfate, ammonium persulfate or potassium dichromate.
[0019] Furthermore, in step 3, the organic polymer is one or more or a combination of catechol, resorcinol, polycatechol, phloroglucinol, cyclohexanehexaone, and inositol; the hydrothermal reaction temperature is 120-180° C., and the hydrothermal time is 4-16 hours; the drying temperature is 40-90° C., and the drying time is 12-24 hours.
[0020] The last aspect of the present invention provides the use of the dual-active component organic intercalated layered vanadium oxide positive electrode material in aqueous zinc ion battery positive electrode and aqueous zinc ion battery.
[0021] The preparation method of the aqueous zinc ion battery positive electrode is:
[0022] The organic intercalated layered vanadium oxide, a binder and a conductive agent are mixed into a slurry, coated on a titanium platinum current collector, and cured to obtain the aqueous zinc ion battery positive electrode.
[0023] Compared with the prior art, the present invention has the following beneficial effects:
[0024] (1) The carbonyl intercalation cathode material of the present invention has excellent electrochemical performance; the composite material has a current density of 463 mAh·g at a current density of 0.1 A / g. -1 The discharge capacity.
[0025] (2) By intercalating vanadium oxide with organic matter, the interlayer spacing is increased and the Zn 2+ Embedding and extraction channels improve reaction kinetics; organic matter plays a stabilizing pillar role, preventing the layered inorganic matter from dissolving or changing phases during the charge and discharge process, thereby improving cycle stability.
[0026] (3) Organic matter has carbonyl energy storage functional groups, which combine with Zn during the charge and discharge process. 2+ , providing organic additional capacity
[0027] (4) The preparation method is simple and non-hazardous. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 is the X-ray diffraction pattern (XRD pattern) of the layered vanadium oxide positive electrode material in the comparative example;
[0029] Figure 2 The X-ray diffraction pattern (XRD pattern) of the organic intercalated layered vanadium oxide positive electrode material in Example 1;
[0030] Figure 3 is a scanning electron microscope image (SEM) of the layered vanadium oxide in the comparative example;
[0031] Figure 4 This is a scanning electron microscope image (SEM) of the organic intercalated layered vanadium oxide in Example 1;
[0032] Figure 5 It is the CV curve of the layered vanadium oxide positive electrode material in the comparative example at a scan rate of 0.2 mV / s;
[0033] Figure 6 The CV curve of the organic intercalated layered vanadium oxide positive electrode material in Example 1 at a scan rate of 0.2 mV / s;
[0034] Figure 7 The charge and discharge comparison curves of the positive electrode material before and after organic intercalation at a current density of 0.1 A / g in Example 1 of the present invention;
[0035] Figure 8This is a long cycle comparison curve of the positive electrode material before and after organic intercalation at a current density of 5 A / g in Example 1 of the present invention. DETAILED DESCRIPTION
[0036] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be further described below.
[0037] Example 1
[0038] This example provides a method for preparing an organic intercalated layered vanadium oxide positive electrode material for an aqueous zinc ion battery, comprising the following steps:
[0039] Step 1: Disperse 0.36 g of vanadium pentoxide in 60 mL of deionized water and add 2 ml of hydrogen peroxide;
[0040] Step 2: Add 0.0182 g of polycatechol to the above (1).
[0041] Step 3, the above (2) was ultrasonically treated until the wine red color was uniform, and then the mixed solution was poured into a hydrothermal kettle and hydrothermaled at 160°C for 12 hours, cooled to room temperature, centrifuged three times with water, twice with ethanol, and vacuum dried at 80°C for 10 hours to obtain a solid powder product;
[0042] Step 4: Take 0.1 g of the above solid powder to obtain an organic intercalated layered vanadium oxide positive electrode material, the product is recorded as V0-PCL, and then directly assembled into a button cell for electrochemical testing.
[0043] Comparative Example:
[0044] This example provides a method for preparing a layered vanadium oxide positive electrode material, which is basically the same as Example 1, except that the addition of step 2 is eliminated and the product is recorded as VOH.
[0045] Figure 1 This is the X-ray diffraction pattern (XRD pattern) of the comparative example layered vanadium oxide positive electrode material of the present invention.
[0046] like Figure 1 As shown, the preparation method of this embodiment obtains a pure phase V2O5·H2O positive electrode material.
[0047] Figure 2 The X-ray diffraction pattern (XRD pattern) of the organic intercalated layered vanadium oxide positive electrode material in Example 1 of the present invention;
[0048] like Figure 2 As shown, the polycatechol intercalated vanadium pentoxide positive electrode material obtained by the preparation method of this example is a pure phase, the main peak is shifted to the left due to the insertion of organic matter, and the interlayer spacing increases. This shows that after the catechol intercalation, the crystal structure of hydrated vanadium pentoxide has not changed significantly.
[0049] Figure 3 is a scanning electron microscope image (SEM) of the layered vanadium oxide in the comparative example of the present invention;
[0050] Figure 4 This is a scanning electron microscope image (SEM) of the organic intercalated layered vanadium oxide in Example 1 of the present invention;
[0051] like Figure 3 , 4 As shown, the modification in this example does not damage the morphology, and the morphology remains in a flaky form.
[0052] Figure 5 The CV curve of the layered vanadium oxide positive electrode material in the comparative example of the present invention at a scan rate of 0.2 mV / s;
[0053] Figure 6 This is a CV curve of the organic intercalated layered vanadium oxide positive electrode material in Example 1 of the present invention at a scan rate of 0.2 mV / s;
[0054] like Figure 5 , 6 As shown, in this example, the prepared polycatechol intercalated layered V2O5·H2O cathode material has an additional pair of redox peaks compared with pure V2O5·H2O, proving that organic matter is involved in energy storage.
[0055] Figure 7 The charge and discharge comparison curves of the positive electrode material before and after organic intercalation at a current density of 0.1 A / g in Example 1 of the present invention;
[0056] like Figure 7 As shown, when charging and discharging were carried out at a current density of 0.1 A / g, the specific capacity of the material after organic intercalation was significantly higher than that before intercalation, proving its superior diffusion kinetics.
[0057] Figure 8 This is a long cycle comparison curve of the positive electrode material before and after organic intercalation at a current density of 1 A / g in Example 1 of the present invention;
[0058] like Figure 8 As shown, at a circuit density of 5A / g, the material specific capacity and stability after organic intercalation are significantly higher than those before intercalation, demonstrating its superior long-cycle stability performance.
[0059] Example 2
[0060] A method for preparing a positive electrode material for an aqueous zinc ion secondary battery comprises the following steps:
[0061] (1) Dissolve 0.36 g of vanadium pentoxide in 60 mL of deionized water and add 2 mL of hydrogen peroxide; ultrasonicate for 30 min.
[0062] (2) Add 0.036 g of phloroglucinol to the above (1);
[0063] (3) The above (2) was stirred evenly, and then the mixed solution was poured into a hydrothermal kettle and hydrothermaled at 160°C for 12 hours. After cooling to room temperature, the mixed solution was vacuum filtered to obtain a solid product, and vacuum dried at 80°C for 10 hours to obtain a solid powder; then directly assembled into button cells for electrochemical testing.
[0064] It has been verified that the positive electrode material prepared in this embodiment has a greatly improved reversible capacity.
[0065] The above is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any technician in the relevant technical field, without departing from the scope of the technical solution of the present invention, makes any form of equivalent replacement or modification to the technical solution and technical content disclosed in the present invention, which does not depart from the content of the technical solution of the present invention and still falls within the protection scope of the present invention.
Claims
1. A dual-active component organic intercalated layered vanadium oxide positive electrode material, characterized in that: The positive electrode material comprises a vanadium oxide layer, and organic matter is embedded between the layers.
2. The dual-active component organic intercalated layered vanadium oxide positive electrode material according to claim 1, characterized in that: The organic matter is an organic carbonyl small molecule or a polymer; the layered vanadium oxide is V2O5, V2O3 or V3O7.
3. The method for preparing the dual-active component organic intercalated layered vanadium oxide positive electrode material according to claim 1 or 2, characterized in that: The steps include: Step 1, dissolving a vanadium source in deionized water to obtain a solution A; Step 2, adding a strong oxidant to solution A and performing ultrasonication to fully dissolve the solid and obtain solution B; Step 3, adding organic polymer C to solution B, then pouring the mixed solution into a hydrothermal kettle for hydrothermal heating, cooling to room temperature, vacuum filtering the mixed solution to obtain a solid product, and vacuum drying to obtain a powder material.
4. The method for preparing the dual-active component organic intercalated layered vanadium oxide positive electrode material according to claim 3, characterized in that: In step 1, the molar concentration of the vanadium source dissolved in deionized water is 0.02-0.5 mol / L.
5. The method for preparing the dual-active component organic intercalated layered vanadium oxide positive electrode material according to claim 3, characterized in that: In step 1, the vanadium source is any one of vanadium pentoxide, vanadium dioxide, sodium metavanadate, vanadium acetylacetonate, vanadyl acetylacetonate, vanadium chloride, and vanadyl sulfate, or a combination of several of them.
6. The method for preparing the dual-active component organic intercalated layered vanadium oxide positive electrode material according to claim 3, characterized in that: The molar ratio of the vanadium source and the organic polymer is: 1:(0.01-0.2).
7. The method for preparing the dual-active component organic intercalated layered vanadium oxide positive electrode material according to claim 3, characterized in that: In step 2, the strong oxidant is one or a combination of hydrogen peroxide, potassium persulfate, ammonium persulfate or potassium dichromate.
8. The method for preparing the dual-active component organic intercalated layered vanadium oxide positive electrode material according to claim 3, characterized in that: In step 3, the organic polymer is one or more or a combination of catechol, resorcinol, polycatechol, phloroglucinol, cyclohexanehexaone, and inositol; the hydrothermal reaction temperature is 120-180° C., and the hydrothermal time is 4-16 hours; the drying temperature is 40-90° C., and the drying time is 12-24 hours.
9. Use of the dual-active component organic intercalated layered vanadium oxide positive electrode material according to any one of claims 1 to 8 in aqueous zinc ion battery positive electrode and aqueous zinc ion battery.
10. The use according to claim 9, wherein the preparation method of the aqueous zinc ion battery positive electrode is: mixing the organic intercalated layered vanadium oxide with a binder and a conductive agent into a slurry, coating the slurry on a titanium platinum current collector, and curing the slurry to obtain the aqueous zinc ion battery positive electrode.
Citation Information
Cited By
Vanadium oxide positive electrode intercalation layer for battery and preparation method of vanadium oxide positive electrode intercalation layer
CN119673939A
Modified positive electrode structure, zinc-vanadium battery, and preparation methods thereof
TWI880877B
Modified positive electrode structure, zinc-vanadium battery, and preparation methods thereof
TWI880878B