Activated carbon-elemental iodine composite material and preparation method thereof, positive electrode and zinc-iodine battery

通过活性炭-单质碘复合材料和海水电解质溶液的组合,解决了锌碘电池中I0氧化为I+的稳定性问题,提高了电池的能量密度和电极电势,实现了高效、环保的锌碘电池技术。

CN118899418AInactive Publication Date: 2024-11-05HAINAN UNIV

Patent Information

Application Number
CN202410961545.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-11-05
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In the four-electron transfer reaction of existing zinc-iodine batteries, the process of oxidation of I0 to I+ is difficult to stabilize, resulting in low electrode potential and insufficient energy density, affecting its industrial application.

Method used

The activated carbon-element iodine composite material is used as the positive electrode material and prepared by high-temperature solid iodine treatment. Combining seawater as Cl-ions in the electrolyte solvent, triggering the reaction of oxidation of I0 to I+ to achieve a tetraelectron redox reaction.

Benefits of technology

The high energy density and electrode potential of zinc-iodine batteries have been improved, and the expansion from 1.3V to 1.83V (vs.Zn/Zn2+) is also simple, rich in resources, low-cost, and suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118899418A_ABST
    Figure CN118899418A_ABST
Patent Text Reader

Abstract

The embodiment of the invention relates to an activated carbon-elemental iodine composite material, a preparation method thereof, a positive electrode and a zinc-iodine battery, and belongs to the technical field of electrochemical energy storage batteries. The high-energy-density seawater-based Swagelok type zinc-iodine battery provided by the embodiment of the invention comprises a battery shell, and an iodine-based positive electrode, a negative electrode, a diaphragm and an electrolyte solution which are positioned in the battery shell. According to the zinc-iodine battery provided by the embodiment of the invention, I- / I0 / I + conversion can be realized, the energy density of the zinc-iodine battery is effectively improved, a novel seawater zinc-iodine battery device is developed, and the zinc-iodine battery has a wide industrial application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The embodiments of the present application relate to the technical field of electrochemical energy storage batteries, and in particular to an activated carbon-elemental iodine composite material and a preparation method thereof, a positive electrode and a zinc-iodine battery. Background Art

[0002] With the continuous increase in energy demand and the increasing depletion of traditional energy, the search for renewable, efficient and environmentally friendly energy has become a hot topic in global research. As a key link in energy storage, the development of battery technology is of great significance to solving energy problems. Among them, aqueous zinc ion batteries (AZIBs) have become a viable alternative to current lithium ion batteries due to their low cost, environmental protection and non-flammability. 2+ Compared with the deintercalation cathode materials (including vanadium-based, manganese-based and Prussian blue, etc.), iodine cathode materials with conversion mechanism show broad prospects due to their abundant sources, large capacity, rich redox states and high redox potential. At present, the reaction of iodine-based cathode usually occurs in the two-electron redox reaction, between I - and I 0 The theoretical capacity is 211 mAh.g -1 , the potential is about 1.3V (vs. Zn 2+ / Zn); theoretically, I 0 It can be further oxidized to a higher valence state in the four-electron transfer of I - / I 0 / I + During the reaction, it releases 422 mAh.g -1 The four-electron reaction also leads to a higher electrode potential from 1.3 V to 1.83 V (vs. Zn / Zn 2+ ); however, with I - Different ions, I + Ions are difficult to stabilize in traditional electrolytes and require a high energy barrier to break. 0 Oxidized to I + Therefore, it is of great significance to develop a new type of seawater zinc-iodine battery device (four-electron transfer). Summary of the invention

[0003] In view of this, the embodiments of the present application provide an activated carbon-elemental iodine composite material and a preparation method thereof, a positive electrode and a zinc-iodine battery. The zinc-iodine battery has the advantages of high energy density, abundant resources, low cost, safety and environmental protection, etc., which is of great significance for promoting the industrialization process of aqueous batteries and can effectively overcome the defects of the above-mentioned prior art.

[0004] A first aspect of an embodiment of the present application provides an activated carbon-elemental iodine composite material, wherein the activated carbon-elemental iodine composite material is obtained by subjecting activated carbon to a high-temperature iodine-fixing treatment.

[0005] In some embodiments that may include the above embodiments, the activated carbon has a specific surface area of ​​not less than 1000m 2 .g -1 of carbon materials.

[0006] Preferably, activated carbon is a general term for a class of carbon materials with a high specific surface area, which is usually not less than 1000 m 2 .g -1 ,, can be obtained through commercial purchase or high-temperature carbonization of porous carbon-based precursors.

[0007] The second aspect of the embodiment of the present application further provides a method for preparing the above-mentioned activated carbon-elemental iodine composite material, comprising the following steps:

[0008] The activated carbon is mixed with elemental iodine and subjected to a sealed high-temperature iodine solidification treatment to obtain an activated carbon-elemental iodine composite material AC@I2.

[0009] In some embodiments that may include the above embodiments, the mass ratio of the activated carbon to elemental iodine is (3-1):1.

[0010] In some embodiments that may include the above embodiments, the sealing high-temperature iodine-solidifying temperature is 100-150° C., and the sealing high-temperature iodine-solidifying time is 2-4 hours.

[0011] Specifically, the sealed high-temperature iodine-fixing treatment is to place activated carbon and elemental iodine in a sealed glass container at a mass ratio of (3-1):1 at 100-150°C for 2-6 hours, and the final black powder obtained is uniformly labeled as activated carbon-elemental iodine composite material AC@I2.

[0012] More specifically, the sealed high-temperature iodine-fixing treatment is to mix activated carbon and iodine in a mass ratio of 1:1, place the mixture in an oven at a temperature of 120° C. for 6 hours to obtain negative iodine carbon.

[0013] The third aspect of the embodiments of the present application further provides an iodine-based positive electrode, wherein the iodine-based positive electrode material includes the above-mentioned activated carbon-elemental iodine composite material.

[0014] The fourth aspect of the embodiments of the present application also provides a high energy density seawater-based Swagelok zinc-iodine battery, comprising the above-mentioned iodine-based positive electrode.

[0015] In some embodiments that may include the above embodiments, the high energy density seawater-based Swagelok zinc-iodine battery further comprises a battery casing and a negative electrode, a separator and an electrolyte solution located in the battery casing, and the positive electrode is located in the battery casing.

[0016] In some embodiments that may include the above embodiments, the negative electrode material is a metal zinc foil, and the purity of the metal zinc foil is not less than 99.9%; or

[0017] The diaphragm material is glass fiber; or

[0018] The solvent of the electrolyte solution is seawater, the solute is a soluble zinc salt, and the concentration of the electrolyte solution is 0.5 to 3 mol / L; or

[0019] The test voltage of the high energy density seawater-based Swagelok zinc-iodine battery is 0.5-1.9V.

[0020] In some embodiments that may include the above embodiments, the seawater is taken from the ocean and can be directly used as a solvent after simple filtration treatment; or

[0021] The soluble zinc salt is at least one of zinc sulfate, zinc chloride, zinc nitrate, zinc acetate, zinc perchlorate, zinc gluconate and zinc trifluoromethanesulfonate.

[0022] Preferably, a more specific method for preparing the electrolyte solution comprises the following steps:

[0023] (1) filtering natural seawater with filter paper to remove impurities and setting aside;

[0024] (2) Weigh a certain amount of zinc sulfate in molar concentration and place it in a beaker;

[0025] (3) Take a corresponding volume of seawater that has been filtered to remove impurities and add it to a beaker containing zinc sulfate. Stir thoroughly for 20 to 30 minutes to obtain a colorless, clear, and transparent liquid. Transfer it to a volumetric flask and make up the volume to obtain an electrolyte solution. Electrolyte solutions of different concentrations can be obtained in this way.

[0026] Specifically, negative iodine carbon, binder sodium alginate, and conductive agent Ketjen black are weighed and fully ground, and an appropriate amount of ultrapure water is added and mixed to form a uniform black paste slurry, which is applied to the current collector to make the positive electrode; the zinc sheet is cut into a circle as the negative electrode; the electrolyte solution uses zinc sulfate solution of different concentrations with seawater as the solvent; and a glass fiber separator, a battery casing, etc. are used to assemble the Swagelok battery.

[0027] It should be noted that the high-energy-density seawater-based Swagelok zinc-iodine battery in the embodiment of the present application is an optimized assembled device, a Swagelok battery, whose internal material is titanium alloy, in order to inhibit the corrosion of chloride ions in seawater on battery devices and the chlorine evolution reaction. This is essentially different from the conventional stainless steel button-type zinc-iodine battery device.

[0028] Compared with the prior art, the embodiments of the present application have the following beneficial effects:

[0029] 1. The embodiment of the present application can effectively utilize the earth's marine resources and reduce the consumption of fresh water resources by introducing seawater into the electrolyte solution, and the Cl- activator in the seawater can trigger I 0 Oxidized to I + , generating ICl, stabilizing the zinc-iodine battery from I- to I + A highly reversible four-electron redox reaction releases 422 mAh.g -1 The high theoretical capacity of Zn / Zn leads to a higher electrode potential from 1.3 V to 1.83 V (vs. Zn / Zn 2+ ); In addition, natural seawater is rich in Cl - Ions are the most promising natural solvents for aqueous zinc-iodine battery electrolyte solutions;

[0030] 2. The preparation method of the embodiment of the present application is simple in process, rich in resources, low in cost, safe and environmentally friendly, suitable for large-scale production, and the prepared zinc-iodine battery can achieve I - / I 0 / I + The conversion of zinc-iodine batteries effectively improves the energy density of zinc-iodine batteries, and a new type of seawater zinc-iodine battery device is developed, which has broad prospects for industrial application. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0032] Figure 1 This is a picture of a high energy density seawater-based Swagelok zinc-iodine battery;

[0033] Figure 2 The cyclic voltammetry curves of zinc-iodine batteries assembled in Example 1 and Comparative Example 1;

[0034] Figure 3 The cycle performance diagram of the zinc-iodine battery assembled in Example 1 and Comparative Example 1;

[0035] Figure 4 This is the rate performance diagram of the zinc-iodine battery assembled in Example 1. DETAILED DESCRIPTION

[0036] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.

[0037] Unless otherwise specified, the experimental methods used in the examples of this application are all conventional methods.

[0038] In the following examples and comparative examples, unless otherwise specified, all raw materials can be obtained by commercial purchase or conventional methods.

[0039] Example 1

[0040] The method for preparing the activated carbon-elemental iodine composite material in this embodiment comprises the following steps:

[0041] Activated carbon (specific surface area not less than 1000m 2 .g -1 The carbon material) is mixed with elemental iodine in a mass ratio of 1:1, and a sealed high-temperature iodine solidification treatment is performed. The sealed high-temperature iodine solidification temperature is 120°C, and the sealed high-temperature iodine solidification time is 6 hours to obtain an activated carbon-elemental iodine composite material AC@I2, i.e., negative iodine carbon.

[0042] The method for preparing a high energy density seawater-based Swagelok zinc-iodine battery in this embodiment comprises the following steps:

[0043] Weigh negative iodine carbon, binder sodium alginate, and conductive agent Ketjen black, grind them thoroughly, add appropriate amount of ultrapure water, mix to form a uniform black paste slurry, and apply it on the current collector to make the positive electrode; cut the metal zinc foil (purity not less than 99.9%) into a circle as the negative electrode; use zinc sulfate solution of different concentrations with seawater as the solvent as the electrolyte solution (concentration of 0.5-3 mol / L); use glass fiber diaphragm, battery shell, etc. to assemble into a Swagelok battery.

[0044] The preparation method of the electrolyte solution includes the following steps: first, obtaining natural seawater from the ocean, filtering with filter paper to obtain clear seawater without solid impurities, and setting aside; weighing 86.268g of zinc sulfate and placing it in a beaker; secondly, adding 70mL of seawater filtered with filter paper into the beaker, stirring continuously for 30 minutes under magnetic stirring conditions to obtain a colorless, clear and transparent liquid, transferring it to a 100mL volumetric flask, and continuing to add seawater filtered with filter paper to make up the volume, and marking the electrolyte solution as 3MZnSO4-Seawater.

[0045] The 3M ZnSO4-Seawater electrolyte solution prepared in this example is used to assemble a Swagelok type zinc-iodine battery with a zinc negative electrode and a positive electrode sheet prepared in this example. Figure 1 shown.

[0046] Example 2

[0047] The method for preparing the activated carbon-elemental iodine composite material in this embodiment comprises the following steps:

[0048] Activated carbon (specific surface area not less than 1000m 2 .g -1 The carbon material) is mixed with elemental iodine in a mass ratio of 2:1, and a sealed high-temperature iodine solidification treatment is performed. The sealed high-temperature iodine solidification temperature is 100°C, and the sealed high-temperature iodine solidification time is 4 hours to obtain an activated carbon-elemental iodine composite material AC@I2, i.e., negative iodine carbon.

[0049] The method for preparing a high energy density seawater-based Swagelok zinc-iodine battery in this embodiment comprises the following steps:

[0050] Weigh negative iodine carbon, binder sodium alginate, and conductive agent Ketjen black, grind them thoroughly, add appropriate amount of ultrapure water, mix to form a uniform black paste slurry, and apply it on the current collector to make the positive electrode; cut the metal zinc foil (purity not less than 99.9%) into a circle as the negative electrode; use zinc sulfate solution of different concentrations with seawater as the solvent as the electrolyte solution (concentration of 0.5-3 mol / L); use glass fiber diaphragm, battery shell, etc. to assemble into a Swagelok battery.

[0051] The preparation method of the electrolyte solution includes the following steps: first, obtaining natural seawater from the ocean, filtering with filter paper to obtain clear seawater without solid impurities, and setting aside; weighing 57.512g of zinc sulfate and placing it in a beaker; secondly, adding 70mL of seawater filtered with filter paper into the beaker, stirring continuously for 30 minutes under magnetic stirring conditions to obtain a colorless, clear and transparent liquid, transferring it to a 100mL volumetric flask, and continuing to add seawater filtered with filter paper to make up the volume, and marking the electrolyte solution as 2MZnSO4-Seawater.

[0052] The 2M ZnSO4-Seawater electrolyte solution prepared in this example was used to assemble a Swagelok type zinc-iodine battery with a zinc negative electrode and a positive electrode sheet prepared in this example. -1 The discharge capacity can still be maintained at 345.8 mAh g after 100 cycles at the current density. -1 .

[0053] Example 3

[0054] The method for preparing the activated carbon-elemental iodine composite material in this embodiment comprises the following steps:

[0055] Activated carbon (specific surface area not less than 1000m 2 .g -1 The carbon material) is mixed with elemental iodine in a mass ratio of 3:1, and a sealed high-temperature iodine solidification treatment is performed. The sealed high-temperature iodine solidification temperature is 150°C, and the sealed high-temperature iodine solidification time is 2h to obtain an activated carbon-elemental iodine composite material AC@I2, i.e., negative iodine carbon.

[0056] The method for preparing a high energy density seawater-based Swagelok zinc-iodine battery in this embodiment comprises the following steps:

[0057] Weigh negative iodine carbon, binder sodium alginate, and conductive agent Ketjen black, grind them thoroughly, add appropriate amount of ultrapure water, mix to form a uniform black paste slurry, and apply it on the current collector to make the positive electrode; cut the metal zinc foil (purity not less than 99.9%) into a circle as the negative electrode; use zinc sulfate solution of different concentrations with seawater as the solvent as the electrolyte solution (concentration of 0.5-3 mol / L); use glass fiber diaphragm, battery shell, etc. to assemble into a Swagelok battery.

[0058] The preparation method of the electrolyte solution includes the following steps: first, obtaining natural seawater from the ocean, filtering with filter paper to obtain clear seawater without solid impurities, and setting aside; weighing 28.75g of zinc sulfate and placing it in a beaker; secondly, adding 70mL of seawater filtered with filter paper into the beaker, stirring continuously for 30 minutes under magnetic stirring conditions to obtain a colorless, clear and transparent liquid, transferring it to a 100mL volumetric flask, and continuing to add seawater filtered with filter paper to make up the volume, and marking the electrolyte solution as 1MZnSO4-Seawater.

[0059] The 1M ZnSO4-Seawater electrolyte solution prepared in this example was used to assemble a Swagelok type zinc-iodine battery with a zinc negative electrode and a positive electrode sheet prepared in this example. -1 The discharge capacity can still be maintained at 320.8 mAh g after 100 cycles at the current density. -1 .

[0060] Example 4

[0061] The method for preparing the activated carbon-elemental iodine composite material in this embodiment comprises the following steps:

[0062] Activated carbon (specific surface area not less than 1000m 2 .g -1The carbon material) is mixed with elemental iodine in a mass ratio of 1:1, and a sealed high-temperature iodine solidification treatment is performed. The sealed high-temperature iodine solidification temperature is 150°C, and the sealed high-temperature iodine solidification time is 2h to obtain an activated carbon-elemental iodine composite material AC@I2, i.e., negative iodine carbon.

[0063] The method for preparing a high energy density seawater-based Swagelok zinc-iodine battery in this embodiment comprises the following steps:

[0064] Weigh negative iodine carbon, binder sodium alginate, and conductive agent Ketjen black, grind them thoroughly, add appropriate amount of ultrapure water, mix to form a uniform black paste slurry, and apply it on the current collector to make the positive electrode; cut the metal zinc foil (purity not less than 99.9%) into a circle as the negative electrode; use zinc sulfate solution of different concentrations with seawater as the solvent as the electrolyte solution (concentration of 0.5-3 mol / L); use glass fiber diaphragm, battery shell, etc. to assemble into a Swagelok battery.

[0065] The preparation method of the electrolyte solution includes the following steps: first, obtaining natural seawater from the ocean, filtering with filter paper to obtain clear seawater without solid impurities, and setting aside; weighing 14.375g of zinc sulfate and placing it in a beaker; secondly, adding 70mL of seawater filtered with filter paper into the beaker, stirring continuously for 30 minutes under magnetic stirring conditions to obtain a colorless, clear and transparent liquid, transferring it to a 100mL volumetric flask, and continuing to add seawater filtered with filter paper to make up the volume, and marking the electrolyte solution as 0.5MZnSO4-Seawater.

[0066] The 0.5M ZnSO4-Seawater electrolyte solution prepared in this example was used to assemble a Swagelok type zinc-iodine battery with a zinc negative electrode and a positive electrode sheet prepared in this example. -1 The discharge capacity can still be maintained at 324.3 mAh g after 100 cycles at the current density. -1 .

[0067] Comparative Example 1

[0068] This comparative example can refer to Example 1, except that the solvent of the electrolyte solution is replaced by water. First, 86.268 g of zinc sulfate is weighed and placed in a beaker; secondly, 70 mL of ultrapure water is added to the beaker, and the mixture is stirred continuously for 30 min under magnetic stirring conditions to obtain a colorless, clear and transparent liquid, which is transferred to a 100 mL volumetric flask, and ultrapure water is continued to be added to make up the volume. The electrolyte solution is marked as 3M ZnSO4.

[0069] The battery was assembled by using the 3M ZnSO4 electrolyte solution prepared in this comparative example, the zinc negative electrode and the positive electrode sheet prepared in this comparative example. -1The discharge capacity can still be maintained at 120.8 mAh g after 100 cycles at the current density. -1 .

[0070] Comparative Example 2

[0071] This comparative example can refer to Example 2, except that the solvent of the electrolyte solution is replaced by water. First, 57.512 g of zinc sulfate is weighed and placed in a beaker; secondly, 70 mL of ultrapure water is added to the beaker, and the mixture is stirred continuously for 30 min under magnetic stirring conditions to obtain a colorless, clear and transparent liquid, which is transferred to a 100 mL volumetric flask, and ultrapure water is continued to be added to make up the volume. The electrolyte solution is marked as 2M ZnSO4.

[0072] The battery was assembled by using the 2M ZnSO4 electrolyte solution prepared in this comparative example, the zinc negative electrode and the positive electrode sheet prepared in this comparative example. -1 The discharge capacity can still be maintained at 115.2 mAh g after 100 cycles at the current density. -1 .

[0073] Electrochemical performance test

[0074] Figure 2 The zinc-iodine full battery was tested at 0.5mV -1 Cyclic voltammetry curves at scan rates. Compared with Comparative Example 1, it can be seen that Example 1 significantly adds a pair of redox peaks, with the oxidation peak and reduction peak located at 1.83V and 1.71V, respectively, which is I2+2Cl - -2e - =2ICl.

[0075] Figure 3 The zinc-iodine full battery was tested at 1A.g -1 The specific capacity and coulombic efficiency under current density are 386.5 mAh.g compared with comparative example 1. -1 High specific capacity, and high capacity retention rate of 84.7% (Comparative Example 1 is 75.1%).

[0076] Figure 4 The zinc-iodine full battery was tested at 0.2Ag -1 -5.0Ag -1 Rate performance at different current densities. -1 The results were 358.9, 338.9, 309.3, 269.0 and 216.0 mAh g respectively. -1 High specific capacity; when the current density returns to 0.2A -1 When the discharge capacity is 304.2 mAh g -1 .

[0077] During the operation of the battery of the present invention, the active iodine in the AC@I2 positive electrode can be converted into negative monovalent iodine ions (I2+2e - =2I - , E=0.53V vs.Zn 2+ / Zn), and can react with chloride ions (concentration of 0.55 mol / L) in seawater to generate ICl (I2+2Cl - -2e - =2ICl, E=1.07V vs.Zn 2+ / Zn), inducing the iodine valence state to change from I - To I + The transformation realizes the four-electron transfer process, and the theoretical specific capacity can reach 422mAh.g -1 Under the same conditions, only two electron transfer processes can be achieved without the participation of chloride ions, and the theoretical specific capacity is only 211 mAh.g -1 .

[0078] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit it. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present application.

Claims

1. An activated carbon-elemental iodine composite material, characterized in that: The activated carbon-elemental iodine composite material is obtained by subjecting activated carbon to high-temperature iodine fixation treatment.

2. The activated carbon-elemental iodine composite material according to claim 1, characterized in that: The activated carbon has a specific surface area of ​​not less than 1000m 2 .g -1 of carbon materials.

3. A method for preparing the activated carbon-elemental iodine composite material according to claim 1 or 2, characterized in that: The following steps are involved: The activated carbon is mixed with elemental iodine and subjected to a sealed high-temperature iodine solidification treatment to obtain an activated carbon-elemental iodine composite material AC@I2.

4. The method for preparing the activated carbon-elemental iodine composite material according to claim 3, characterized in that: The mass ratio of the activated carbon to elemental iodine is (3-1):

1.

5. The method for preparing the activated carbon-elemental iodine composite material according to claim 3, characterized in that: The sealing high-temperature iodine-fixing temperature is 100-150° C., and the sealing high-temperature iodine-fixing time is 2-6 hours.

6. An iodine-based positive electrode, characterized in that The iodine-based positive electrode material comprises the activated carbon-elemental iodine composite material according to claim 1 or 2.

7. A high energy density seawater-based Swagelok zinc-iodine battery, characterized in that: Comprising the iodine-based positive electrode as described in claim 6.

8. The high energy density seawater-based Swagelok zinc-iodine battery according to claim 7, characterized in that: The high energy density seawater-based Swagelok zinc-iodine battery further comprises a battery casing and a negative electrode, a separator and an electrolyte solution located in the battery casing, and the positive electrode is located in the battery casing.

9. The high energy density seawater-based Swagelok zinc-iodine battery according to claim 8, characterized in that: The negative electrode material is a metal zinc foil, and the purity of the metal zinc foil is not less than 99.9%; or The diaphragm material is glass fiber; or The solvent of the electrolyte solution is seawater, the solute is a soluble zinc salt, and the concentration of the electrolyte solution is 0.5 to 3 mol / L; or The test voltage of the high energy density seawater-based Swagelok zinc-iodine battery is 0.5-1.9V.

10. The high energy density seawater-based Swagelok zinc-iodine battery according to claim 9, characterized in that: The seawater is taken from the ocean and can be used directly as a solvent after simple filtration; or The soluble zinc salt is at least one of zinc sulfate, zinc chloride, zinc nitrate, zinc acetate, zinc perchlorate, zinc gluconate and zinc trifluoromethanesulfonate.

Citation Information

Patent Citations

  • Water-phase electrolyte system zinc iodine secondary battery and preparation method thereof

    CN107666015A

  • Aqueous zinc-iodine battery based on four-electron conversion reaction and electrolyte thereof

    CN111540950A

  • Three-dimensional alloy negative electrode material and application thereof in preparation of secondary energy storage battery

    CN112510178A

  • Method for improving performance of zinc-iodine battery based on halogen bond effect

    CN112563586A

  • Aqueous zinc ion energy storage device

    CN113381081A

Cited By

  • Wide-temperature-range high-iodine-loading positive electrode material, preparation method thereof and zinc-iodine battery

    CN119764429A

  • A wide temperature range high iodine loading positive electrode material and preparation method thereof and zinc-iodine battery