Phosphorus-doped rGO-coated lithium-rich manganese-based material as well as preparation method and application thereof
By doping phosphorus in lithium-rich manganese-based materials and coating rGO, the problems of material structure instability and oxygen escape are solved, the conductivity and rate performance are improved, and higher battery capacity and cycle stability are achieved.
Patent Information
- Application Number
- CN202411239599.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-05
- Publication Date
- 2024-11-05
AI Technical Summary
Lithium-rich manganese-based materials have problems such as structural instability, poor rate performance and oxygen emission in lithium-ion batteries, which are mainly due to the irreversible migration of transition metal ions and the escape of lattice oxygen.
By doping phosphorus in the core of the lithium-rich manganese-based material and coating the surface with reduced graphene oxide (rGO) to form a phosphorus-doped and rGO-coated lithium-rich manganese-based material, reducing the migration of transition metal ions and blocking oxygen Escape, increase electron transfer channels, and improve structural stability and conductivity.
It effectively improves the structural stability and conductivity of the material, enhances the capacity and circulation performance of the battery, reduces structural collapse, and improves the rate performance.
Smart Images

Figure BDA0005028832300000131
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of batteries and relates to a phosphorus-doped and rGO-coated lithium-rich manganese-based material and a preparation method and application thereof. Background Art
[0002] Lithium-ion batteries are widely used in electric vehicles, mobile devices and other fields due to their high energy density, long life and low cost. As the positive electrode material of lithium-ion batteries, lithium-rich manganese-based materials have attracted widespread attention due to their ultra-high specific capacity, but their application is restricted by irreversible capacity loss, extreme voltage decay, insufficient rate performance and excessive oxygen emission.
[0003] The above problems are largely related to the irreversible migration of transition metal ions and the escape of lattice oxygen in lithium-rich manganese-based materials, which is due to the activation of the Li2MnO3 component at 4.5V and the oxidation of oxygen anions during the cycle. In addition, transition metal ions will irreversibly migrate into the Li layer, causing the layered phase to transform into a spinel phase, and the spinel structure will cause structural instability in lithium-rich manganese-based materials, thereby exacerbating the decrease in voltage and capacity of lithium-rich manganese-based positive electrode materials. In addition, the interaction of the electrolyte interface and the increase in interface resistance hinder the Li + Diffusion dynamics, resulting in limited rate performance.
[0004] Based on the above research, there is a need to provide a phosphorus-doped and rGO (reduced graphene oxide)-coated lithium-rich manganese-based material, wherein the lithium-rich manganese-based precursor can overcome the problems of structural instability and poor rate performance of the above lithium-rich manganese-based precursor. Summary of the invention
[0005] The purpose of the present invention is to provide a lithium-rich manganese-based material doped with phosphorus and coated with rGO, as well as a preparation method and application. The lithium-rich manganese-based precursor can reduce the migration of transition metal ions and improve structural stability by doping with phosphorus and coating with rGO. It can also form oxygen vacancies in the material to prevent oxygen from escaping. At the same time, it also increases the transfer channel of electrons, improves the electrical conductivity, and thus improves the capacity of the material.
[0006] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:
[0007] In a first aspect, the present invention provides a lithium-rich manganese-based material doped with phosphorus and coated with rGO, wherein the lithium-rich manganese-based material doped with phosphorus and coated with rGO comprises a core and a coating layer on the surface of the core, wherein the core comprises a lithium-rich manganese-based material doped with phosphorus, and the coating layer comprises rGO.
[0008] On the one hand, the present invention dopes phosphorus into the inner core lithium-rich manganese-based material, and on the other hand, coats reduced graphene oxide on the surface of the lithium-rich manganese-based material, which effectively improves the migration of transition metal ions, thereby improving the structural stability, and can also form oxygen vacancies in the sandwich structure of the lithium-rich manganese-based material, thereby preventing oxygen from escaping, which is beneficial to minimize structural collapse and improve the structural strength of the material. At the same time, the rGO coating increases the electron transfer channel, improves the electrical conductivity, and thus improves the capacity of the lithium-rich manganese-based material.
[0009] Preferably, the doping content of phosphorus in the core is 5-15wt%, for example, 5wt%, 10wt% or 15wt%, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0010] The amount of phosphorus doped in the present invention will affect the performance of the material. If the amount of phosphorus doped is too much, the structural strength of the material cannot be effectively improved. If the amount of phosphorus doped is too little, sufficient oxygen vacancies cannot be effectively formed.
[0011] Preferably, the general chemical formula of the phosphorus-doped lithium-rich manganese-based material is Li z (Mn y Ni 1-y ) 1-x P x O2, wherein 0.05≤x≤0.15, for example, it can be 0.05, 0.10 or 0.15, 0.5≤y≤0.95, for example, it can be 0.5, 0.6, 0.7, 0.8, 0.9 or 0.95, 1≤z≤1.3, for example, it can be 1.0, 1.1, 1.2 or 1.3, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0012] Preferably, in the phosphorus-doped and rGO-coated lithium-manganese-rich material, the content of the coating layer is 5-20wt%, for example, it can be 5wt%, 10wt%, 15wt% or 20wt%, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0013] The amount of rGO coated in the present invention will affect the effect thereof. If the coating amount is too little, a sufficient graphene coating layer cannot be formed on the surface. If the coating amount is too much, the embedding of lithium ions during calcination of the positive electrode will be affected.
[0014] In a second aspect, the present invention provides a method for preparing a lithium-rich manganese-based material doped with phosphorus and coated with rGO as described in the first aspect, the preparation method comprising the following steps:
[0015] (1) first mixing a mixed metal source solution, a phosphorus source solution, a complexing agent solution and a precipitant solution, and performing a coprecipitation reaction to obtain a phosphorus-doped lithium-rich manganese-based precursor;
[0016] (2) performing a second mixing of the phosphorus-doped lithium-manganese-based precursor, the solvent and rGO described in step (1) to obtain a phosphorus-doped lithium-manganese-based precursor coated with rGO;
[0017] (3) The lithium source and the phosphorus-doped and rGO-coated lithium-manganese-based precursor of step (2) are mixed and calcined for the third time to obtain the phosphorus-doped and rGO-coated lithium-manganese-based material.
[0018] The present invention is to dope phosphorus during the preparation of lithium-rich manganese-based precursors by coprecipitation, and a phosphorus source such as sodium dihydrogen phosphate can be directly introduced into the coprecipitation reaction system to achieve PO4 3- Compared with the lithium-rich manganese-based material prepared by calcination and then coated with rGO, rGO can be made to have a better performance when doped with PO4. 3- The surface of the precursor is coated more tightly and evenly.
[0019] Preferably, the concentration of the phosphorus source solution in step (1) is 0.5-2.5 mol / L, for example, 0.5 mol / L, 1.0 mol / L, 1.5 mol / L, 2.0 mol / L or 2.5 mol / L, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0020] The concentration of the phosphorus source solution during the coprecipitation reaction of the present invention will affect the content of the doped phosphorus element. If the concentration of the phosphorus source is too high or too low, the amount of doped phosphorus will be too much or too little.
[0021] Preferably, the phosphorus source solution in step (1) comprises NaH2PO4 solution.
[0022] Preferably, the concentration of the mixed metal source solution in step (1) is 1-4 mol / L, for example, 1 mol / L, 2 mol / L, 3 mol / L or 4 mol / L, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0023] Preferably, the concentration of the precipitant solution in step (1) is 25-35wt%, for example, 25wt%, 30wt% or 35wt%, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0024] Preferably, the concentration of the complexing agent solution in step (1) is 14-18wt%, for example, 14wt%, 15wt%, 16wt%, 17wt% or 18wt%, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0025] Preferably, the precipitant solution in step (1) comprises sodium hydroxide solution, and the complexing agent solution in step (1) comprises aqueous ammonia.
[0026] Preferably, the temperature of the coprecipitation reaction in step (1) is 40-65°C, for example, 40°C, 50°C, 60°C or 65°C, and the pH is 9.5-12, for example, 9.5, 10.5, 11.5 or 12, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0027] Preferably, the feeding rate of the phosphorus source solution in step (1) is 0.5-2 L / h, for example, 0.5 L / h, 1 L / h, 1.5 L / h or 2 L / h, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0028] Preferably, the feed rate of the mixed metal source solution in step (1) is 5-15 L / h, for example, 5 L / h, 10 L / h or 15 L / h, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0029] Preferably, the mixed metal source solution in step (1) comprises a nickel source and a manganese source, and the nickel source and the manganese source independently comprise any one of acetate, nitrate, sulfate or chloride, or a combination of at least two thereof.
[0030] Preferably, the feed rate of the precipitant solution in step (1) is 1.5-3.5 L / h, for example, 1.5 L / h, 2.5 L / h or 3.5 L / h, and the feed rate of the complexing agent solution in step (1) is 0.5-2.5 L / h, for example, 0.5 L / h, 1.5 L / h or 2.5 L / h, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0031] Preferably, the first mixing in step (1) comprises passing a mixed metal source solution, a phosphorus source solution, a complexing agent solution and a precipitant solution into a base solution to perform a co-precipitation reaction.
[0032] Preferably, the base liquid comprises water, a precipitant and a complexing agent.
[0033] Preferably, the pH of the base solution is 9-10, for example, 9, 9.5 or 10, and the concentration of the complexing agent is 3-4wt%, for example, 3wt%, 3.5wt% or 4wt%, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0034] Preferably, the coprecipitation reaction is carried out until the product particles D50 is 3-8 μm, for example, 3 μm, 5 μm, 7 μm or 8 μm, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0035] Preferably, the second mixing in step (2) comprises mixing the phosphorus-doped lithium-rich manganese-based precursor in step (1) with a solvent to obtain a precursor solution, mixing rGO with the solvent to obtain an rGO solution, and passing the rGO solution into the precursor solution for reaction.
[0036] Preferably, the concentration of the rGO solution is 0.5-5wt%, for example, 0.5wt%, 2wt%, 4wt% or 5wt%, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0037] Preferably, the speed at which the rGO solution is introduced into the precursor solution is 0.1-1.5 L / h, for example, 0.1 L / h, 0.5 L / h, 1.0 L / h or 1.5 L / h, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0038] Preferably, the rGO solution is introduced into the precursor solution for reaction for 20-30 hours, for example, 20 hours, 25 hours or 30 hours, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0039] Preferably, the calcination temperature in step (3) is 600-800°C, for example, 600°C, 700°C or 800°C, and the calcination time is 10-15h, for example, 10h, 12h, 14h or 15h, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0040] Preferably, the heating rate of the calcination in step (3) is 8-12°C / min, for example, 8°C / min, 10°C / min or 12°C / min, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0041] Preferably, the ratio of the total molar amount of metal ions in the phosphorus-doped and rGO-coated lithium-manganese-rich precursor to the molar amount of lithium ions in the lithium source in step (3) is 1:(1-1.3), for example, it can be 1:1, 1:1.1, 1:1.2 or 1:1.3, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0042] In a third aspect, the present invention provides a lithium-ion battery, comprising the phosphorus-doped and rGO-coated lithium-manganese-rich material as described in the first aspect.
[0043] Compared with the prior art, the present invention has the following beneficial effects:
[0044] The present invention effectively improves the migration of transition metal ions by doping phosphorus in the inner core and coating rGO on the surface of the inner core, thereby improving the structural stability. At the same time, the present invention doping phosphorus and coating rGO can form oxygen vacancies in the sandwich structure of the lithium-rich manganese-based material, thereby preventing oxygen from escaping, which is beneficial to minimize structural collapse and improve the structural strength of the material. In addition, the rGO coating increases the electron transfer channel and improves the electrical conductivity, thereby improving the capacity of the lithium-rich manganese-based material. DETAILED DESCRIPTION
[0045] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0046] Example 1
[0047] This embodiment provides a lithium-rich manganese-based material doped with phosphorus and coated with rGO, wherein the lithium-rich manganese-based material doped with phosphorus and coated with rGO comprises a core and a coating layer on the surface of the core, wherein the core comprises a lithium-rich manganese-based material doped with phosphorus, and the coating layer comprises rGO;
[0048] The phosphorus doping content in the core is 10wt%; the general chemical formula of the phosphorus doped lithium-rich manganese-based material is Li 1.2 (Mn 0.75 Ni 0.25 ) 0.9 P 0.1 O2; in the phosphorus-doped and rGO-coated lithium-rich manganese-based material, the content of the coating layer is 12wt%;
[0049] The preparation method of the phosphorus-doped and rGO-coated lithium-rich manganese-based material comprises the following steps:
[0050] (1) nickel sulfate and manganese sulfate were weighed according to the formula to prepare a mixed metal source solution with a concentration of 2.5 mol / L; a sodium hydroxide solution with a concentration of 31 wt%, an ammonia solution with a concentration of 16 wt% and a NaH2PO4 solution with a concentration of 1 mol / L were also prepared;
[0051] Add 130L of pure water to a 200L reactor, add a certain amount of the above sodium hydroxide solution and ammonia water to make the pH reach 9.5 and the ammonia concentration reach 3.5wt%, keep the reactor at 52°C and keep the temperature constant, turn on the stirring device, and introduce nitrogen as a protective gas in advance to prevent oxidation;
[0052] The prepared mixed metal source solution is added to the reactor at a rate of 8 L / h, and the sodium hydroxide solution is added to the reactor at a rate of 2.66 L / h, and the ammonia solution is added to the reactor at a flow rate of 1.5 L / h, and the NaH2PO4 solution is added to the reactor at a rate of 1 L / h to perform a coprecipitation reaction, during which the pH of the reaction is controlled to be 10. After the reaction is performed until the product particle size D50 is 5 μm, centrifugal dehydration is performed to obtain a phosphorus-doped lithium-rich manganese-based precursor;
[0053] (2) dispersing rGO in water and ultrasonically dispersing to prepare a rGO solution with a concentration of 2 wt%;
[0054] The phosphorus-doped lithium-rich manganese-based precursor described in step (1) is put into a 200L reactor, water is added and stirred to form a slurry of the phosphorus-doped lithium-rich manganese-based precursor, and then the ultrasonically treated rGO solution is added into the reactor at a rate of 0.5L / h and the reaction is continued for 24h to obtain a phosphorus-doped and rGO-coated lithium-rich manganese-based precursor;
[0055] (3) The phosphorus-doped and rGO-coated lithium-manganese-based precursor of step (2) and lithium hydroxide are calcined at 700° C. in a rotary kiln at a heating rate of 10° C. / min, and then cooled to room temperature after keeping the temperature for 12 hours to obtain the phosphorus-doped and rGO-coated lithium-manganese-based material.
[0056] Example 2
[0057] This embodiment provides a lithium-rich manganese-based material doped with phosphorus and coated with rGO, wherein the lithium-rich manganese-based material doped with phosphorus and coated with rGO comprises a core and a coating layer on the surface of the core, wherein the core comprises a lithium-rich manganese-based material doped with phosphorus, and the coating layer comprises rGO;
[0058] The phosphorus doping content in the core is 5wt%; the general chemical formula of the phosphorus doped lithium-rich manganese-based material is Li 1.1 (Mn 0.55 Ni 0.45 )0.95 P 0.05 O2; in the phosphorus-doped and rGO-coated lithium-rich manganese-based material, the content of the coating layer is 5wt%;
[0059] The preparation method of the phosphorus-doped and rGO-coated lithium-rich manganese-based material comprises the following steps:
[0060] (1) nickel sulfate and manganese sulfate were weighed according to the formula to prepare a mixed metal source solution with a concentration of 1 mol / L; a sodium hydroxide solution with a concentration of 32 wt%, an ammonia solution with a concentration of 14 wt% and a NaH2PO4 solution with a concentration of 0.5 mol / L were also prepared;
[0061] Add 130L of pure water to a 200L reactor, add a certain amount of liquid alkali and ammonia water to make the pH reach 9 and the ammonia concentration reach 3wt%, keep the reactor at 40°C and keep the temperature constant, turn on the stirring device, and introduce nitrogen as a protective gas in advance to prevent oxidation;
[0062] The prepared mixed metal source solution is added to the reactor at a rate of 15 L / h, and the sodium hydroxide solution is added to the reactor at a rate of 3.5 L / h, and the ammonia solution is added to the reactor at a flow rate of 2.5 L / h, and the NaH2PO4 solution is added to the reactor at a rate of 0.5 L / h to perform a coprecipitation reaction, during which the pH of the reaction is controlled to be 9.5. After the reaction is performed until the product particle size D50 is 3 μm, centrifugal dehydration is performed to obtain a phosphorus-doped lithium-rich manganese-based precursor;
[0063] (2) dispersing rGO in water and ultrasonically dispersing to prepare an rGO solution with a concentration of 0.5 wt %;
[0064] The phosphorus-doped lithium-rich manganese-based precursor described in step (1) is put into a 200L reactor, water is added and stirred to form a slurry of the phosphorus-doped lithium-rich manganese-based precursor, and then the ultrasonically treated rGO solution is added into the reactor at a rate of 0.1L / h and the reaction is continued for 20h to obtain a phosphorus-doped and rGO-coated lithium-rich manganese-based precursor;
[0065] (3) The phosphorus-doped and rGO-coated lithium-manganese-based precursor of step (2) and lithium hydroxide are calcined at 800° C. in a rotary kiln at a heating rate of 12° C. / min, and then cooled to room temperature after being kept for 10 hours to obtain the phosphorus-doped and rGO-coated lithium-manganese-based material.
[0066] Example 3
[0067] This embodiment provides a lithium-rich manganese-based material doped with phosphorus and coated with rGO, wherein the lithium-rich manganese-based material doped with phosphorus and coated with rGO comprises a core and a coating layer on the surface of the core, wherein the core comprises a lithium-rich manganese-based material doped with phosphorus, and the coating layer comprises rGO;
[0068] The phosphorus content in the core is 15 wt %; the general chemical formula of the phosphorus-doped lithium-rich manganese-based material is Li 1.3 (Mn 0.75 Ni 0.25 ) 0.85 P 0.15 O2; in the phosphorus-doped and rGO-coated lithium-rich manganese-based material, the content of the coating layer is 20wt%;
[0069] The preparation method of the phosphorus-doped and rGO-coated lithium-rich manganese-based material comprises the following steps:
[0070] (1) nickel sulfate and manganese sulfate were weighed according to the formula to prepare a mixed metal source solution with a concentration of 4 mol / L; a sodium hydroxide solution with a concentration of 31 wt%, an ammonia solution with a concentration of 18 wt% and a NaH2PO4 solution with a concentration of 2.5 mol / L were also prepared;
[0071] Add 130L of pure water to a 200L reactor, add a certain amount of liquid alkali and ammonia water to make the pH reach 10 and the ammonia concentration reach 4wt%, keep the reactor at 65°C and keep the temperature constant, turn on the stirring device, and introduce nitrogen as a protective gas in advance to prevent oxidation;
[0072] The prepared mixed metal source solution is added to the reactor at a rate of 5 L / h, and the sodium hydroxide solution is added to the reactor at a rate of 1.5 L / h, and the ammonia solution is added to the reactor at a flow rate of 0.5 L / h, and the NaH2PO4 solution is added to the reactor at a rate of 2 L / h to perform a coprecipitation reaction, during which the pH of the reaction is controlled to be 12, and after the reaction is performed until the product particle size D50 is 8 μm, centrifugal dehydration is performed to obtain a phosphorus-doped lithium-rich manganese-based precursor;
[0073] (2) dispersing rGO in water and ultrasonically dispersing to prepare a rGO solution with a concentration of 5 wt%;
[0074] The phosphorus-doped lithium-rich manganese-based precursor described in step (1) is put into a 200L reactor, water is added and stirred to form a slurry of the phosphorus-doped lithium-rich manganese-based precursor, and then the ultrasonically treated rGO solution is added into the reactor at a rate of 1.5L / h and the reaction is continued for 30h to obtain a phosphorus-doped and rGO-coated lithium-rich manganese-based precursor;
[0075] (3) The phosphorus-doped and rGO-coated lithium-manganese-based precursor of step (2) and lithium hydroxide are calcined at 600° C. in a rotary kiln at a heating rate of 8° C. / min, and then cooled to room temperature after being kept for 10 hours to obtain the phosphorus-doped and rGO-coated lithium-manganese-based material.
[0076] Example 4
[0077] This embodiment provides a lithium-rich manganese-based material doped with phosphorus and coated with rGO, wherein the phosphorus-doped lithium-rich manganese-based material doped with phosphorus and coated with rGO is the same as that of Embodiment 1 except that the phosphorus doping content in the core is 2 wt%;
[0078] The preparation method of the phosphorus-doped and rGO-coated lithium-rich manganese-based material is the same as that of Example 1, except that the concentration of the NaH2PO4 solution in step (1) is 0.2 mol / L.
[0079] Example 5
[0080] This embodiment provides a lithium-rich manganese-based material doped with phosphorus and coated with rGO, wherein the phosphorus-doped lithium-rich manganese-based material doped with phosphorus and coated with rGO is the same as that of Embodiment 1 except that the phosphorus doping content in the core is 20wt%;
[0081] The preparation method of the phosphorus-doped and rGO-coated lithium-rich manganese-based material is the same as that of Example 1, except that the concentration of the NaH2PO4 solution in step (1) is 3 mol / L.
[0082] Example 6
[0083] This embodiment provides a lithium-rich manganese-based material doped with phosphorus and coated with rGO, wherein the lithium-rich manganese-based material doped with phosphorus and coated with rGO is the same as that of Embodiment 1 except that the content of the coating layer is 2wt%;
[0084] The preparation method of the phosphorus-doped and rGO-coated lithium-rich manganese-based material is the same as that of Example 1, except that the concentration of the rGO solution in step (2) is 0.2 wt%.
[0085] Example 7
[0086] This embodiment provides a lithium-rich manganese-based material doped with phosphorus and coated with rGO, wherein the lithium-rich manganese-based material doped with phosphorus and coated with rGO is the same as that of Embodiment 1 except that the content of the coating layer is 25wt%;
[0087] The preparation method of the phosphorus-doped and rGO-coated lithium-manganese-rich based material is the same as that of Example 1, except that the concentration of the rGO solution in step (2) is 7 wt %.
[0088] Example 8
[0089] The present embodiment provides a phosphorus-doped and rGO-coated lithium-rich manganese-based material. The phosphorus-doped and rGO-coated lithium-rich manganese-based material is the same as Example 1 except that in the preparation method, the phosphorus-doped lithium-rich manganese-based precursor and lithium hydroxide in step (1) are calcined at 700°C in a rotary kiln at a heating rate of 10°C / min according to the ratio of metal ions to lithium hydroxide in a ratio of 1:1.2, and the temperature is kept for 12 hours and then cooled to room temperature to obtain the phosphorus-doped lithium-rich manganese-based material, and then the phosphorus-doped lithium-rich manganese-based material is replaced with the phosphorus-doped lithium-rich manganese-based precursor in step (2) to coat rGO, and then spray-drying is performed to make the adaptability of the obtained phosphorus-doped and rGO-coated lithium-rich manganese-based material change.
[0090] Comparative Example 1
[0091] This comparative example provides a lithium-rich manganese-based material, which is the same as Example 1 except that the core is not doped with phosphorus and is not coated with rGO;
[0092] The method for preparing the lithium-rich manganese-based material is the same as that of Example 1, except that the NaH2PO4 solution is not introduced in step (1) and step (2) is not performed.
[0093] Comparative Example 2
[0094] This comparative example provides a lithium-rich manganese-based material, which is the same as Example 1 except that the core is not doped with phosphorus;
[0095] The preparation method of the lithium-rich manganese-based material is the same as that of Example 1, except that the NaH2PO4 solution is not introduced in step (1).
[0096] Comparative Example 3
[0097] This comparative example provides a lithium-rich manganese-based material, which is the same as Example 1 except that it is not coated with rGO;
[0098] The method for preparing the lithium-rich manganese-based material is the same as that of Example 1 except that step (2) is not performed.
[0099] The lithium-rich manganese-based materials obtained in the above embodiments and comparative examples were prepared into positive electrode sheets, and then prepared into lithium-ion batteries with metal lithium sheets, lithium hexafluorophosphate electrolytes and polyethylene separators. The lithium-ion batteries were charged to 4.2 V at a rate current of 0.1 C, and then discharged at the charging rate current until the discharge voltage was cut off at 2.0 V. The interval between each charge and discharge was 10 minutes, and the initial capacity and capacity retention rate of the battery were tested at 100 charge and discharge cycles at each rate.
[0100] The test results are shown in Table 1:
[0101] Table 1
[0102]
[0103] From Table 1 we can see that:
[0104] It can be seen from Example 1 and Comparative Examples 1-3 that the present invention doping with phosphorus and coating rGO can improve the structural stability and electrical conductivity of the material, thereby improving the cycle performance and rate performance of the battery; it can be seen from Example 1 and Examples 4-5 that the amount of phosphorus doped in the present invention will affect the structural stability, thereby affecting the performance of the battery; it can be seen from Example 1 and Examples 6-7 that the amount of rGO coated in the present invention will affect its function, thereby affecting the performance of the battery; it can be seen from Example 1 and Example 8 that the present invention preferably coats rGO on the surface of the precursor to achieve rGO coating on the surface of the lithium-rich manganese-based material.
[0105] In summary, the present invention provides a lithium-rich manganese-based material doped with phosphorus and coated with rGO, as well as a preparation method and application. The lithium-rich manganese-based precursor can reduce the migration of transition metal ions and improve structural stability by doping with phosphorus and coating with rGO. It can also form oxygen vacancies in the material to prevent oxygen from escaping, while also increasing the electron transfer channel, improving the electrical conductivity, and thereby increasing the capacity of the material.
[0106] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention are within the protection scope and disclosure scope of the present invention.
Claims
1. A lithium-rich manganese-based material doped with phosphorus and coated with rGO, It is characterized in that The phosphorus-doped and rGO-coated lithium-manganese-rich material comprises a core and a coating layer on the surface of the core, wherein the core comprises the phosphorus-doped lithium-manganese-rich material, and the coating layer comprises rGO.
2. The phosphorus-doped and rGO-coated lithium-rich manganese-based material according to claim 1, It is characterized in that In the core, the doping content of phosphorus element is 5-15wt%; Preferably, the general chemical formula of the phosphorus-doped lithium-rich manganese-based material is Li z (Mn y Ni 1-y ) 1-x P x O 2 , where 0.05≤x≤0.15, 0.5≤y≤0.95, 1≤z≤1.3; Preferably, in the phosphorus-doped and rGO-coated lithium-manganese-based material, the content of the coating layer is 5-20wt%.
3. A method for preparing the lithium-rich manganese-based material doped with phosphorus and coated with rGO as claimed in claim 1 or 2, It is characterized in that The preparation method comprises the following steps: (1) first mixing a mixed metal source solution, a phosphorus source solution, a complexing agent solution and a precipitant solution, and performing a coprecipitation reaction to obtain a phosphorus-doped lithium-rich manganese-based precursor; (2) performing a second mixing of the phosphorus-doped lithium-manganese-based precursor, the solvent and rGO described in step (1) to obtain a phosphorus-doped lithium-manganese-based precursor coated with rGO; (3) The lithium source and the phosphorus-doped and rGO-coated lithium-manganese-based precursor of step (2) are mixed and calcined for the third time to obtain the phosphorus-doped and rGO-coated lithium-manganese-based material.
4. The preparation method according to claim 3, It is characterized in that The concentration of the phosphorus source solution in step (1) is 0.5-2.5 mol / L; Preferably, the phosphorus source solution in step (1) comprises NaH 2 PO 4 Solution.
5. The preparation method according to claim 3 or 4, It is characterized in that The concentration of the mixed metal source solution in step (1) is 1-4 mol / L; Preferably, the concentration of the precipitant solution in step (1) is 25-35wt%; Preferably, the concentration of the complexing agent solution in step (1) is 14-18 wt %.
6. The preparation method according to any one of claims 3 to 5, It is characterized in that The temperature of the coprecipitation reaction in step (1) is 40-65° C. and the pH is 9.5-12; Preferably, the feeding rate of the phosphorus source solution in step (1) is 0.5-2 L / h; Preferably, the feeding rate of the mixed metal source solution in step (1) is 5-15 L / h; Preferably, the feed rate of the precipitant solution in step (1) is 1.5-3.5 L / h, and the feed rate of the complexing agent solution in step (1) is 0.5-2.5 L / h.
7. The preparation method according to any one of claims 3 to 6, It is characterized in that Step (1) The first mixing includes passing a mixed metal source solution, a phosphorus source solution, a complexing agent solution and a precipitant solution into a base solution to perform a coprecipitation reaction; Preferably, the base liquid comprises water, a precipitant and a complexing agent; Preferably, the pH of the base solution is 9-10, and the concentration of the complexing agent is 3-4wt%; Preferably, the coprecipitation reaction is carried out until the product particles D50 are 3-8 μm.
8. The preparation method according to any one of claims 3 to 7, It is characterized in that Step (2) the second mixing comprises mixing the phosphorus-doped lithium-rich manganese-based precursor of step (1) with a solvent to obtain a precursor solution, mixing rGO with the solvent to obtain an rGO solution, and passing the rGO solution into the precursor solution for reaction; Preferably, the concentration of the rGO solution is 0.5-5wt%; Preferably, the rGO solution is introduced into the precursor solution at a rate of 0.1-1.5 L / h; Preferably, the rGO solution is introduced into the precursor solution for reaction for 20-30 hours.
9. The preparation method according to any one of claims 3 to 8, It is characterized in that The calcination temperature in step (3) is 600-800° C. and the calcination time is 10-15 h; Preferably, the heating rate of the calcination in step (3) is 8-12°C / min; Preferably, the ratio of the total molar amount of metal ions in the phosphorus-doped and rGO-coated lithium-rich manganese-based precursor in step (3) to the molar amount of lithium ions in the lithium source in step (3) is 1:(1-1.3).
10. A lithium ion battery, It is characterized in that The lithium-ion battery comprises the phosphorus-doped and rGO-coated lithium-manganese-rich material as claimed in claim 1 or 2.
Citation Information
Cited By
Preparation method and application of lithium-rich manganese oxide cathode material with high capacity and long cycle stability