Electrode slurry, electrode plate and lithium ion battery

By adding dibenzylamine to the lithium-ion battery electrode slurry and adjusting the particle size ratio of the active material and the electrolyte ratio, a polyurethane colloidal substance is generated, which solves the problem of high-temperature thermal runaway in lithium-ion batteries and achieves a balance between battery safety and performance.

CN118899443APending Publication Date: 2024-11-05ZHEJIANG LIWINON ENERGY TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410939742.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

Existing lithium-ion batteries are prone to thermal runaway at high temperatures, and current technologies struggle to effectively suppress this phenomenon.

Method used

Add 0.5%-2% dibenzylamine (DBA) to the electrode slurry and control the particle size ratio of the first active material to the second active material between 0.5 and 1.2. At the same time, adjust the ratio of ethylene carbonate to fluoroethylene carbonate in the electrolyte between 2.5 and 3.2 to generate polyurethane colloidal material to block gas series connection and regulate the reaction sequence of battery materials.

Benefits of technology

It effectively suppresses battery thermal runaway, increases the thermal runaway temperature of the battery cell, extends the escape time for personnel, and prevents other battery performance from deteriorating.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004943677690000111
    Figure BDA0004943677690000111
  • Figure BDA0004943677690000121
    Figure BDA0004943677690000121
Patent Text Reader

Abstract

The invention discloses an electrode slurry, an electrode plate and a lithium ion battery, the electrode slurry comprises a first electrode slurry, the first electrode slurry comprises a first active material and dibenzylamine, and the dibenzylamine accounts for 0.5%-2% of the mass of the first electrode slurry. 0.5%-2.0% of dibenzylamine is added into electrode slurry, the dibenzylamine (DBA) can induce ring-opening polymerization and reaction of five-membered cyclic organic compounds ethylene carbonate (EC) and fluoroethylene carbonate (FEC) in electrolyte to generate a polyurethane colloidal substance, the substance can block gas series connection after a battery cell generates gas, the reaction sequence of battery materials is adjusted, and therefore the performance of the battery is improved. Therefore, the heat release intensity of the battery is reduced, the thermal runaway temperature of the battery cell is greatly improved, and the escape time of people is greatly prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of lithium ion batteries, and in particular to an electrode slurry, an electrode sheet and a lithium ion battery. Background Art

[0002] Lithium-ion batteries are widely used in modern electronic devices due to their excellent properties, such as high specific energy, high specific power, high voltage platform, low self-discharge rate, long cycle life, small environmental impact and no memory effect. They have become an indispensable energy solution in a variety of fields such as mobile phones, computers, electric vehicles, military and space technology. The chemical and physical properties of these batteries provide an energy-dense and long-life power source for portable devices, greatly promoting the development of mobile technology and the electric vehicle industry.

[0003] The battery's electrolyte is mainly composed of flammable organic solvents with low flash points and boiling points. When the battery is charged, its internal materials will be transformed into strong oxidizing compounds. Once the battery is overheated, these organic solvents will be easily oxidized, generating gas and heat, causing the battery temperature to rise rapidly. When the temperature is too high, the battery's diaphragm material may shrink thermally, causing a short circuit between the positive and negative electrodes, which will trigger the release of a large amount of energy in a short period of time, causing thermal runaway of the battery, and further causing the battery to burn or even explode.

[0004] Therefore, there is an urgent need to develop an electrode slurry, an electrode sheet and a lithium-ion battery that can suppress thermal runaway and improve hot box performance. Summary of the invention

[0005] The purpose of the present invention is to provide an electrode slurry to effectively suppress thermal runaway of a battery cell at high temperature in view of the deficiencies of the prior art.

[0006] In order to achieve the above object, the present invention adopts the following technical solutions:

[0007] An electrode slurry includes a first electrode slurry, wherein the first electrode slurry includes a first active material and dibenzylamine, wherein the mass content of the dibenzylamine in the first electrode slurry is 0.5%-2%. When the content of diphenylamine is lower than 0.5%, sufficient polyurethane colloid material cannot be generated, and thermal runaway cannot be effectively controlled; when the content of diphenylamine is higher than 2%, the channels for lithium insertion in the negative electrode sheet are reduced, and the lithium ions released from the positive electrode cannot be completely embedded in the negative electrode, resulting in a lower capacity of the battery cell, and lithium deposition may occur, increasing the risk of thermal runaway.

[0008] Among them, dibenzylamine (DBA) can induce the ring-opening polymerization of five-membered cyclic organic compounds ethylene carbonate (EC) and fluoroethylene carbonate (FEC) in the electrolyte to form a polyurethane colloid substance, which can block the gas series after the battery cell produces gas, adjust the reaction order between battery materials, and thus reduce the heat release intensity of the battery.

[0009] Preferably, the electrode slurry further includes a second electrode slurry, and the second electrode slurry includes a second active material; a ratio δ of a particle size D50 of the first active material to a particle size D50 of the second active material satisfies the relationship: 0.5≤δ≤1.2.

[0010] If δ is lower than 0.5, the particle size of the first electrode is small, processing is more difficult, and the cost is higher. Although the fast charging capability can be guaranteed, the cycle life of the battery cell will be greatly reduced; if δ is higher than 1.2, the particle size of the upper graphite will be larger than the lower graphite, and the lithium ion embedding channels will be reduced, resulting in the inability of lithium ions to embed into the lower layer of the negative electrode in time. Even when charging at a higher rate (fast charging), the lithium ions cannot be completely embedded in the lower graphite, which may cause lithium to precipitate on the upper surface. When δ is set within the range of 0.5-1.2, the SEI film can be quickly decomposed when the battery cell has thermal runaway, and the polyurethane colloid generated by the reaction of DBA and EC produced in the upper material of the negative electrode is exposed on the surface of the negative electrode sheet, blocking the lower graphite from continuing to participate in the reaction, thereby suppressing thermal runaway and improving hot box performance.

[0011] Preferably, the particle size D50 of the first active substance is 8 μm-12 μm.

[0012] Preferably, the particle size D50 of the second active substance is 10 μm-16 μm.

[0013] Preferably, the mass ratio of the first electrode slurry to the second electrode slurry is 1:(1-1.2).

[0014] Preferably, the first electrode slurry and the second electrode slurry both further include a conductive agent, a binder and a thickener.

[0015] Preferably, the first active material and the second active material are both selected from one or more of graphite, soft carbon, hard carbon, carbon fiber, mesophase carbon microbeads, silicon-based materials, tin-based materials and lithium titanate.

[0016] In addition, the present invention further provides an electrode sheet, comprising a current collector and a first electrode slurry disposed on at least one surface of the current collector, wherein the first electrode slurry is the above-mentioned first electrode slurry.

[0017] Preferably, the electrode sheet further comprises a second electrode slurry disposed between the current collector and the first electrode slurry, and the second electrode slurry is the above-mentioned second electrode slurry.

[0018] In addition, the present invention also provides a lithium-ion battery, including a battery cell composed of a negative electrode sheet, a positive electrode sheet and a diaphragm stack, an electrolyte, and a shell that encapsulates the battery cell and the electrolyte, wherein the negative electrode sheet is the above-mentioned electrode sheet.

[0019] Preferably, the electrolyte comprises ethylene carbonate and fluoroethylene carbonate, the mass content of ethylene carbonate in the electrolyte is a, the mass content of fluoroethylene carbonate in the electrolyte is b, wherein a and b satisfy the relationship: 2.5≤a / b≤3.2.

[0020] If a / b is lower than 2.5, the a content is too low, and the film-forming potential of EC on the negative electrode is relatively high. When charging, the potential of the negative electrode continues to decrease, and EC with a higher reduction potential is preferentially precipitated, participating in the formation of the SEI film; this content is too low, which will affect the formation of SEI, resulting in the deterioration of various performances of the battery cell. If a / b is higher than 3.2, the a content is too high, and the melting point of EC is 36.4℃. It is solid at room temperature, and a large amount of addition will lead to poor low-temperature performance; this substance is a substance that reacts preferentially during film formation. If the content is too high, the gas production during the battery cell charging process will increase, resulting in an increase in the internal gas pressure of the battery cell, affecting safety. Setting the EC / FEC ratio in the electrolyte between 2.5 and 3.2 can ensure that while improving the hot box performance, other electrical properties will not be deteriorated.

[0021] Preferably, the mass of the ethylene carbonate is A, the mass of the fluoroethylene carbonate is B, and the mass of the dibenzylamine is C;

[0022] Among them, A, B and C satisfy the relationship: 4.4<A / C<28, 1.8<B / C<8.6.

[0023] If the value is greater than this range, DBA will excessively consume EC and FEC in the electrolyte, causing the lithium salt and other additives in the electrolyte to undergo side reactions prematurely and produce a large amount of gas; if the value is less than this range, a sufficient amount of colloidal substances cannot be generated, and thermal runaway cannot be controlled when heated at high temperatures.

[0024] Compared with the prior art, the present invention has at least the following beneficial effects:

[0025] (1) The present invention adds 0.5%-2.0% dibenzylamine to the electrode slurry, wherein dibenzylamine (DBA) can induce the ring-opening polymerization of five-membered cyclic organic compounds ethylene carbonate (EC) and fluoroethylene carbonate (FEC) in the electrolyte to react and generate a polyurethane colloid substance. The polyurethane colloid substance can block the gas series connection after the battery cell produces gas, adjust the reaction sequence between battery materials, thereby reducing the heat release intensity of the battery, and greatly improving the thermal runaway temperature of the battery cell and the escape time of personnel.

[0026] (2) The present invention controls the ratio δ of the particle size D50 of the first active material to the particle size D50 of the second active material to be between 0.5 and 1.2, and adds DBA to the first slurry in the upper layer. When thermal runaway occurs in the battery cell, the SEI film decomposes rapidly, so that the polyurethane colloid generated by the reaction of DBA and EC is exposed on the surface of the negative electrode sheet, blocking the second active material in the lower layer from continuing to participate in the reaction, thereby effectively suppressing thermal runaway and improving the battery hot box performance.

[0027] (3) The present invention controls the EC / FEC ratio in the electrolyte to be between 2.5 and 3.2, thereby ensuring that the hot box performance is improved while not deteriorating other electrical properties of the battery. DETAILED DESCRIPTION

[0028] In order to make the technical solutions and advantages of the present invention clearer, the technical solutions of the present invention will be clearly and completely described below in conjunction with specific embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0029] According to a first aspect of the present application, the present application aims to provide an electrode slurry, comprising a first electrode slurry, the first slurry comprising a first active substance and dibenzylamine, the mass content of dibenzylamine in the first electrode slurry being 0.5%-2%, for example, 0.5%, 0.6%, 0.8%, 0.9%, 1.0%, 1.3%, 1.5%, 1.6%, 1.8%, 1.9%, or 2.0%.

[0030] In some embodiments, a second electrode slurry is further included, and the second electrode slurry includes a second active material; the ratio δ of the particle size D50 of the first active material to the particle size D50 of the second active material satisfies the relationship: 0.5≤δ≤1.2, for example, it can be 0.5, 0.7, 0.8, 1.0, 1.2.

[0031] In some embodiments, the particle size D50 of the first active material is 8 μm-12 μm, for example, 8 μm, 8 μm, 9 μm, 10 μm, 11 μm, or 12 μm.

[0032] In some embodiments, the particle size D50 of the second active material is 10 μm-16 μm, for example, 10 μm, 11 μm, 12 μm, 13 μm, 14 μm, 15 μm, or 16 μm.

[0033] In some embodiments, the mass ratio of the first electrode slurry to the second electrode slurry is 1:(1-1.2), for example, 1, 1.1, or 1.2.

[0034] In some embodiments, the first electrode slurry and the second electrode slurry each further include a conductive agent, a binder, and a thickener.

[0035] In some embodiments, the conductive agent is selected from one or more of carbon black, conductive graphite, vapor-grown carbon fiber, carbon nanotubes, and graphene.

[0036] In some embodiments, the binder is selected from one or more of polyvinylidene fluoride, carboxymethyl cellulose, polyacrylic acid, and styrene-butadiene rubber.

[0037] In some embodiments, the thickener is selected from one or more of sodium alginate, polyvinyl alcohol, polyacrylic acid, and carbomer resin.

[0038] In some embodiments, the first active material and the second active material are both selected from one or more of graphite, soft carbon, hard carbon, carbon fiber, mesocarbon microbeads, silicon-based materials, tin-based materials, and lithium titanate.

[0039] According to a second aspect of the present application, the present application aims to provide an electrode sheet, comprising a current collector and a first electrode slurry disposed on at least one surface of the current collector, wherein the first electrode slurry is the above-mentioned first electrode slurry.

[0040] In some embodiments, a second electrode slurry is further included and disposed between the current collector and the first electrode slurry. The second electrode slurry is the second electrode slurry described above.

[0041] According to the third aspect of the present application, the present application provides a lithium-ion battery, including a battery cell composed of a negative electrode sheet, a positive electrode sheet and a diaphragm stack, an electrolyte, and a shell that encapsulates the battery cell and the electrolyte, wherein the negative electrode sheet is the above-mentioned electrode sheet.

[0042] In some embodiments, the electrolyte includes ethylene carbonate and fluoroethylene carbonate, the mass content of ethylene carbonate in the electrolyte is a, the mass content of fluoroethylene carbonate in the electrolyte is b, wherein a and b satisfy the relationship: 2.5≤a / b≤3.2; for example, it can be 2.5, 2.6, 2.7, 2.8, 2.9, 3.0, 3.1, 3.2. In some embodiments, the mass of ethylene carbonate is A, the mass of fluoroethylene carbonate is B, and the mass of dibenzylamine is C;

[0043] Among them, A, B and C satisfy the relationship: 4.4<A / C<28, for example, it can be 4.5, 8.5, 10, 12, 14, 16, 18, 20, 22, 24, 26, 27.5; 1.8<B / C<8.6, for example, it can be 2, 3, 4, 5, 6, 7, 8, 8.5.

[0044] The positive electrode sheet includes a positive electrode current collector and a positive electrode active material layer disposed on at least one surface of the positive electrode current collector. The positive electrode active material layer includes a positive electrode active material. The positive electrode active material may include but is not limited to a chemical formula such as Li a Ni x Co y M z O 2-b N b (wherein 0.95≤a≤1.2, x>0, y≥0, z≥0, and x+y+z=1, 0≤b≤1, M is selected from a combination of one or more of Mn and Al, and N is selected from a combination of one or more of F, P, and S) The positive electrode active material may also be, but is not limited to, LiCoO2, LiNiO2, LiVO2, LiCrO2, LiMn2O4, LiCoMnO4, Li2NiMn3O8, LiNi 0.5 Mn 1.5 O4, LiCoPO4, LiMnPO4, LiFePO4, LiNiPO4, LiCoFSO4, CuS2, FeS2, MoS2, NiS, TiS2, etc. The positive active material may also be modified. The method of modifying the positive active material should be known to those skilled in the art. For example, the positive active material may be modified by coating, doping, etc. The material used for the modification may include but is not limited to a combination of one or more of Al, B, P, Zr, Si, Ti, Ge, Sn, Mg, Ce, W, etc. The positive current collector is usually a structure or part for collecting current. The positive current collector may be various materials suitable for use as a positive current collector for lithium-ion batteries in the art. For example, the positive current collector may include but is not limited to metal foil, etc., and more specifically may include but is not limited to aluminum foil, etc.

[0045] The separator can be any material suitable for lithium-ion battery separators in the art, for example, it can be a combination of one or more materials including but not limited to polyethylene, polypropylene, polyvinylidene fluoride, aramid, polyethylene terephthalate, polytetrafluoroethylene, polyacrylonitrile, polyimide, polyamide, polyester and natural fibers.

[0046] The lithium-ion battery also includes an electrolyte, which includes an organic solvent, an electrolyte lithium salt and an additive. Among them, the electrolyte lithium salt can be LiPF6 and / or LiBOB used in high-temperature electrolytes; it can also be at least one of LiBF4, LiBOB, and LiPF6 used in low-temperature electrolytes; it can also be at least one of LiBF4, LiBOB, LiPF6, and LiTFSI used in anti-overcharge electrolytes; it can also be at least one of LiClO4, LiAsF6, LiCF3SO3, and LiN(CF3SO2)2. The organic solvent can be a cyclic carbonate, including PC and EC; it can also be a chain carbonate, including DFC, DMC, or EMC; it can also be a carboxylic acid ester, including MF, MA, EA, MP, etc. The additives include but are not limited to at least one of film-forming additives, conductive additives, flame retardant additives, anti-overcharge additives, additives for controlling the content of H2O and HF in the electrolyte, additives for improving low-temperature performance, and multifunctional additives.

[0047] To make the technical solutions and advantages of the present invention more clear, the present invention and its beneficial effects will be further described in detail below in conjunction with specific implementation methods, but the implementation methods of the present invention are not limited thereto.

[0048] Example 1

[0049] Preparation of positive electrode

[0050] The positive electrode material lithium cobalt oxide, the conductive agent acetylene black, and the binder polyvinylidene fluoride (PVDF) are fully stirred and mixed in an N-methylpyrrolidone solvent system at a mass ratio of 97.6:1.4:1.0, and then coated on an Al foil, and then dried, rolled, and slit to obtain a positive electrode sheet.

[0051] Preparation of negative electrode

[0052] The negative electrode active material, sodium carboxymethyl cellulose and styrene-butadiene rubber (SBR) emulsion are mixed in a weight ratio of 97.4:1.3:1.3 to prepare a negative electrode active material slurry, where the negative electrode active material can be a silicon-carbon material; the active material slurry is coated on a copper current collector to obtain an active material layer, and then cold pressed and slit to obtain a negative electrode sheet.

[0053] The first active material (graphite), the conductive agent acetylene black, the lithium polyacrylate (PAA-Li), the binder styrene-butadiene rubber (SBR), and the thickener sodium carboxymethyl cellulose (CMC-Na) are fully stirred and mixed in a deionized water solvent and dibenzylamine system at a mass ratio of 96.7:0.3:2.4:0.3:0.3 to obtain a first electrode slurry;

[0054] The second active material (graphite), the conductive agent acetylene black, the lithium polyacrylate (PAA-Li), the binder styrene-butadiene rubber (SBR), and the thickener sodium carboxymethyl cellulose (CMC-Na) are fully stirred and mixed in a deionized water solvent at a mass ratio of 96.7:0.3:2.4:0.3:0.3 to obtain a second electrode slurry;

[0055] The second electrode slurry and the first electrode slurry are sequentially coated on the copper current collector in a weight ratio of 1:1, and the negative electrode sheet is obtained after drying, rolling and slitting.

[0056] Among them, the mass content of DBA in the first electrode slurry is 0.5%, the particle size D50 of the first active substance is 8μm, the particle size D50 of the second active substance is 16μm, the ratio δ of the particle size D50 of the first active substance to the particle size D50 of the second active substance is 0.5, the mass of ethylene carbonate is 1.05g, the mass of fluoroethylene carbonate is 0.42g, and the mass of dibenzylamine is 0.23g.

[0057] Preparation of diaphragm

[0058] A polyethylene (PE) porous polymer film is used as the isolation membrane.

[0059] Preparation of electrolyte

[0060] The lithium salt LiPF6 and the non-aqueous organic solvent (ethylene carbonate (EC): fluoroethylene carbonate (FEC): diethyl carbonate (DEC): propylene carbonate (PC): propyl propionate (PP): vinylene carbonate (VC)) = 25:8:20:15:28:4, mass ratio) were prepared in a mass ratio of 8:92 as the electrolyte of the lithium battery. The mass ratio a / b of the electrolyte ethylene carbonate and fluoroethylene carbonate was 3.1.

[0061] Preparation of batteries

[0062] The positive electrode sheet, the separator, and the negative electrode sheet are stacked in order, so that the separator is placed between the positive electrode sheet and the negative electrode sheet to play a role of safety isolation, and then wound to obtain an electrode assembly. The electrode assembly is placed in a packaging shell, and the electrolyte is injected and packaged to obtain a lithium battery.

[0063] Example 2

[0064] Different from Example 1, in this embodiment, the mass content of DBA in the first active electrode slurry is 0.5%, the particle size D50 of the first active substance is 11.2 μm, the ratio δ of the particle size D50 of the first active substance to the particle size D50 of the second active substance is 0.7, the mass of ethylene carbonate is 1.75 g, the mass of fluoroethylene carbonate is 0.56 g, and the mass of dibenzylamine is 0.0625 g.

[0065] The rest is the same as Example 1 and will not be described again here.

[0066] Example 3

[0067] Different from Example 1, in this embodiment, the mass content of DBA in the first active electrode slurry is 1.5%, the particle size D50 of the first active substance is 11.7 μm, the particle size D50 of the second active substance is 13 μm, the ratio δ of the particle size D50 of the first active substance to the particle size D50 of the second active substance is 0.9, the mass of ethylene carbonate is 1.4 g, the mass of fluoroethylene carbonate is 0.5 g, and the mass of dibenzylamine is 0.1 g.

[0068] The rest is the same as Example 1 and will not be described again here.

[0069] Example 4

[0070] Different from Example 1, in this embodiment, the mass content of DBA in the first active electrode slurry is 2%, the particle size D50 of the first active substance is 12 μm, the particle size D50 of the second active substance is 10 μm, the ratio δ of the particle size D50 of the first active substance to the particle size D50 of the second active substance is 1.2, the mass of ethylene carbonate is 1.5 g, the mass of fluoroethylene carbonate is 0.48 g, and the mass of dibenzylamine is 0.15 g.

[0071] The rest is the same as Example 1 and will not be described again here.

[0072] Example 5

[0073] Different from Example 1, in this embodiment, the mass ratio a / b of ethylene carbonate and fluoroethylene carbonate in the electrolyte is 2.5, the mass of ethylene carbonate is 1.6 g, the mass of fluoroethylene carbonate is 0.52 g, and the mass of dibenzylamine is 0.08 g.

[0074] The rest is the same as Example 1 and will not be described again here.

[0075] Example 6

[0076] Different from Example 1, in this example, the mass ratio a / b of ethylene carbonate and fluoroethylene carbonate in the electrolyte is 3.0, the mass of ethylene carbonate is 1.3 g, the mass of fluoroethylene carbonate is 0.46 g, and the mass of dibenzylamine is 0.18 g.

[0077] The rest is the same as Example 1 and will not be described again here.

[0078] Example 7

[0079] Different from Example 1, in this example, the mass ratio a / b of ethylene carbonate to fluoroethylene carbonate in the electrolyte is 3.0, the mass of ethylene carbonate is 1.2 g, the mass of fluoroethylene carbonate is 0.54 g, and the mass of dibenzylamine is 0.2 g.

[0080] The rest is the same as Example 1 and will not be described again here.

[0081] Comparative Example 1

[0082] Different from Example 1, DBA is not added to the first active electrode slurry in this comparative example, the particle size D50 of the first active substance is 8 μm, the particle size D50 of the second active substance is 10 μm, the ratio δ of the particle size D50 of the first active substance to the particle size D50 of the second active substance is 0.8, the mass of ethylene carbonate is 0.5 g, the mass of fluoroethylene carbonate is 0.48 g, and the mass of dibenzylamine is 0.15 g.

[0083] The rest is the same as Example 1 and will not be described again here.

[0084] Comparative Example 2

[0085] Different from Example 2, in this comparative example, the particle size D50 of the first active substance is 4.8 μm, the ratio δ of the particle size D50 of the first active substance to the particle size D50 of the second active substance is 0.3, the mass of ethylene carbonate is 3 g, the mass of fluoroethylene carbonate is 0.48 g, and the mass of dibenzylamine is 0.1 g.

[0086] The rest is the same as Example 2 and will not be described again here.

[0087] Comparative Example 3

[0088] Different from Example 3, in this comparative example, the particle size D50 of the first active substance is 20.8 μm, the particle size D50 of the second active substance is 16 μm, the ratio δ of the particle size D50 of the first active substance to the particle size D50 of the second active substance is 1.3 g, the mass of ethylene carbonate is 1.5 g, the mass of fluoroethylene carbonate is 2 g, and the mass of dibenzylamine is 0.15 g.

[0089] The rest is the same as Example 3 and will not be described again here.

[0090] Comparative Example 4

[0091] Different from Example 1, in this comparative example, the mass content of DBA in the first active electrode slurry is 3%, the particle size D50 of the second active substance is 10 μm, the ratio δ of the particle size D50 of the first active substance to the particle size D50 of the second active substance is 0.8, the mass of ethylene carbonate is 1.5 g, the mass of fluoroethylene carbonate is 0 g, and the mass of dibenzylamine is 0.15 g.

[0092] The rest is the same as Example 1 and will not be described again here.

[0093] Comparative Example 5

[0094] Different from Example 1, in this comparative example, the mass ratio a / b of the electrolyte ethylene carbonate to fluoroethylene carbonate is 3.5, the mass of ethylene carbonate is 1.5 g, the mass of fluoroethylene carbonate is 0.48 g, and the mass of dibenzylamine is 0.01 g.

[0095] The rest is the same as Example 1 and will not be described again here.

[0096] Comparative Example 6

[0097] Different from Example 1, in this comparative example, the mass ratio a / b of the electrolyte ethylene carbonate to fluoroethylene carbonate is 2.0, the mass of ethylene carbonate is 1.5 g, the mass of fluoroethylene carbonate is 0.48 g, and the mass of dibenzylamine is 0.3 g.

[0098] The rest is the same as Example 1 and will not be described again here.

[0099] The specific parameters of Examples 1-7 and Comparative Examples 1-6 are shown in Tables 1 and 2 below.

[0100] Table 1

[0101]

[0102]

[0103] Table 2

[0104] Group A(EC content) B(FEC content) C(DBA content) A / C B / C Example 1 1.05g 0.42g 0.23g 4.6 1.8 Example 2 1.75g 0.56g 0.0625g 28.0 9.0 Example 3 1.40g 0.50g 0.10 14.0 5.0 Example 4 1.50g 0.48g 0.15 10.0 3.2 Example 5 1.60g 0.52g 0.08g 20.0 6.5 Example 6 1.30g 0.46g 0.18g 7.2 2.6 Example 7 1.20g 0.54g 0.20g 6.0 2.7 Comparative Example 1 0.50g 0.48g 0.15g 3.3 3.2 Comparative Example 2 3.00g 0.48g 0.10g 30.0 4.8 Comparative Example 3 1.50g 2.00g 0.15g 10.0 13.3 Comparative Example 4 1.50g 0.00g 0,15g 10.0 0.0 Comparative Example 5 1.50g 0.48g 0.01g 150.0 48.0 Comparative Example 6 1.50g 0.48g 0.30g 5.0 1.6

[0105] The following performance tests were performed on the lithium ion batteries prepared in the examples and comparative examples:

[0106] (1) Hot box test: The finished battery cell is discharged at a constant current of 0.2C to 3V, left for 5 minutes, and then charged at a constant current and constant voltage of 0.5C to 4.50V, with a cut-off rate of 0.02C, and left for 5 minutes. Then the battery cell is placed in a thermal shock box (hanging test) and heated by convection or circulating hot air at a starting temperature of 25±3℃. The oven temperature is raised to 132±2℃ at a rate of 5±2℃ / min and kept for 60 minutes before stopping. Then, a 135℃ hot box test is performed using the same test method.

[0107] (2) Cycle test: 1. Charge at 20A constant current and constant voltage to 4.3V, cut-off rate 3.3C; 2. Charge at 3.3C constant current and constant voltage to 4.35V, cut-off rate 1.8C; 3. Charge at 1.8C constant current and constant voltage to 4.4V, cut-off rate 1.5C; 4. Charge at 1.5C constant current and constant voltage to 4.5V, cut-off rate 1.2C; 5. Charge at 1.2C constant current and constant voltage to 4.55V, cut-off rate 0.2C; 6. Leave for 5 minutes; 7. Discharge at 0.2C constant current, cut-off voltage 3.0V; 8. Cycle 1-7 for 200 cycles to obtain the remaining capacity and thickness expansion of the battery cell.

[0108] The results of the above performance tests are shown in Table 3 below.

[0109] Table 3

[0110] Group 132℃ 135℃ Remaining capacity rate (%) Cell expansion rate (%) Example 1 3 / 3Pass 3 / 3Pass 98.35 6.23 Example 2 3 / 3Pass 3 / 3Pass 98.41 6.31 Example 3 3 / 3Pass 3 / 3Pass 98.23 6.22 Example 4 3 / 3Pass 3 / 3Pass 98.66 6.30 Example 5 3 / 3Pass 3 / 3Pass 98.54 6.25 Example 6 3 / 3Pass 3 / 3Pass 98.77 6.37 Example 7 3 / 3Pass 3 / 3Pass 98.41 6.43 Comparative Example 1 3 / 3Pass 0 / 3Pass 98.65 6.45 Comparative Example 2 3 / 3Pass 0 / 3Pass 98.88 6.34 Comparative Example 3 3 / 3Pass 0 / 3Pass 98.53 6.37 Comparative Example 4 3 / 3Pass 0 / 3Pass 98.64 6.45 Comparative Example 5 3 / 3Pass 0 / 3Pass 98.79 7.21 Comparative Example 6 3 / 3Pass 0 / 3Pass 98.66 5.86

[0111] By comparing the experimental data of Examples 1-7 and Comparative Examples 1-6 in Table 3, it can be obtained that when the mass content of dibenzylamine in the first electrode slurry is controlled to be 0.5%-2%, the ratio δ of the particle size D50 of the first active substance to the particle size D50 of the second active substance is 0.5≤δ≤1.2, and the mass ratio a / b of the electrolyte ethylene carbonate and fluoroethylene carbonate is within the range of 2.5-3.2, the hot box performance test at 135°C can be passed, that is, thermal runaway can be effectively suppressed and the hot box performance can be improved.

[0112] Among them, by comparing the experimental data of Example 2-3 with that of Comparative Example 2-3, it can be obtained that when δ is less than the preset range, the particle size of the upper graphite is too small, and the upper and lower layers are easily mixed during the processing process, resulting in the polyurethane colloid substance generated by DBA and EC / FEC being unable to completely exist in the upper graphite, resulting in the inability of the negative electrode sheet surface of the battery cell to completely expose the polyurethane colloid substance under high temperature conditions, thereby causing the battery cell to have overall thermal runaway; when δ is greater than the preset range, the particle size of the upper graphite is larger, the specific surface area is smaller, and the lithium insertion channels are fewer. The lithium ions released from the positive electrode cannot be completely embedded in the lower layer of the negative electrode, thereby precipitating on the surface and losing control after heating.

[0113] By comparing the experimental data of Examples 1-4 with Comparative Examples 1 and 4, it can be seen that when DBA is not added to the first active electrode slurry, the battery cannot pass the 135°C hot box performance test; when the mass content of DBA in the first active electrode slurry is greater than 2%, DBA will over-consume EC and FEC in the electrolyte, causing the lithium salt and other additives in the electrolyte to react prematurely and produce a large amount of gas. The masses of EC, FEC and DBA are A, B and C respectively, and the ratios of the three must simultaneously satisfy the relationship: 4.4<A / C<28, 1.8<B / C<8.6. If it is greater than this range, DBA will over-consume EC and FEC in the electrolyte, causing the lithium salt and other additives in the electrolyte to react prematurely and produce a large amount of gas; if it is less than this range, it is impossible to generate sufficient colloidal substances, and thus it is impossible to control thermal runaway when heated at high temperatures.

[0114] By comparing the experimental data of Examples 1 and 5-7 with Comparative Examples 5-6, it can be obtained that when a / b is less than the preset range, the EC content is low, resulting in insufficient polyurethane colloid material generated by its reaction with DBA; when a / b is greater than the preset range, the EC content is too high, resulting in continuous gas production when generating the SEI film, resulting in increased gas production and increased air pressure inside the battery cell, which in turn causes the thickness of the battery cell to expand.

[0115] According to the disclosure and teaching of the above description, those skilled in the art to which the present invention belongs can also change and modify the above embodiment. Therefore, the present invention is not limited to the above specific embodiment, and any obvious improvement, replacement or modification made by those skilled in the art on the basis of the present invention belongs to the protection scope of the present invention. In addition, although some specific terms are used in this specification, these terms are only for the convenience of description and do not constitute any limitation to the present invention.

Claims

1. An electrode slurry, characterized in that: The invention comprises a first electrode slurry, wherein the first electrode slurry comprises a first active material and dibenzylamine, and the mass content of the dibenzylamine in the first electrode slurry is 0.5%-2%.

2. The electrode slurry according to claim 1, characterized in that: It also includes a second electrode slurry, which includes a second active material; a ratio δ of the particle size D50 of the first active material to the particle size D50 of the second active material satisfies the relationship: 0.5≤δ≤1.

2.

3. The electrode slurry according to claim 2, characterized in that: The particle size D50 of the first active material is 8 μm-12 μm.

4. The electrode slurry according to claim 2, characterized in that: The particle size D50 of the second active material is 10 μm-16 μm.

5. The electrode slurry according to claim 2, characterized in that: The mass ratio of the first electrode slurry to the second electrode slurry is 1:(1-1.2).

6. The electrode slurry according to claim 2, characterized in that: The first electrode slurry and the second electrode slurry each further include a conductive agent, a binder and a thickener.

7. The electrode slurry according to claim 2, characterized in that: The first active material and the second active material are both selected from one or more of graphite, soft carbon, hard carbon, carbon fiber, mesophase carbon microbeads, silicon-based materials, tin-based materials and lithium titanate.

8. An electrode sheet, characterized in that: The invention comprises a current collector and a first electrode slurry arranged on at least one surface of the current collector, wherein the first electrode slurry is the first electrode slurry according to any one of claims 1 to 7.

9. The electrode sheet according to claim 8, characterized in that: The invention further comprises a second electrode slurry disposed between the current collector and the first electrode slurry, wherein the second electrode slurry is the second electrode slurry according to any one of claims 2 to 7.

10. A lithium ion battery, characterized in that: It comprises the electrode plate and electrolyte as described in any one of claims 8 to 9, wherein the electrolyte comprises ethylene carbonate and fluoroethylene carbonate, the mass content of ethylene carbonate in the electrolyte is a, the mass content of fluoroethylene carbonate in the electrolyte is b, wherein a and b satisfy the relationship: 2.5≤a / b≤3.

2.