Laminated board, multilayer board, and method for manufacturing laminated board
By using liquid crystal polymer film and metal layer with a melting point greater than or equal to 345°C in the laminated plate, the problem of metal lines sinking or deformation during the hot press bonding is solved, and the high heat resistance and goodness of the multi-layer board are achieved quality.
Patent Information
- Application Number
- CN202311043779.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-08-10
- Filing Date
- 2023-08-18
- Publication Date
- 2024-11-05
AI Technical Summary
During the hot press bonding of the laminated plate, insufficient heat resistance of the insulating substrate causes the metal lines to sink or deform, resulting in circuit design impedance errors, increased signal transmission losses and increased crosstalk between lines.
Using a liquid crystal polymer film with a melting point greater than or equal to 345°C, and a metal layer is formed on its surface. The heat resistance of the liquid crystal polymer film is improved through the specific composition and heating process of the liquid crystal polymer to ensure that the metal layer is in the hot pressing process. No sinking or deformation.
It effectively avoids the metal lines sinking or deforming after hot pressing, ensures the accuracy of the circuit design of the multi-layer board, reduces signal transmission losses and crosstalk between lines, and improves the quality of the multi-layer board.
Smart Images

Figure CN118900496A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to a laminate, a multilayer board and a method for manufacturing the laminate. Background Art
[0002] A laminated board usually includes an insulating substrate and a metal circuit. When the multiple laminated boards are stacked and then heat-pressed, if the insulating substrate has poor heat resistance, the metal circuit may easily sink into the insulating substrate or deform. Therefore, the impedance error of the pre-designed circuit may occur, thereby increasing the signal transmission loss and increasing the cross-talk between the circuits. In view of this, it is urgent to develop a solution that can overcome the above problems. Summary of the invention
[0003] The present disclosure provides a laminate, which includes a liquid crystal polymer film and at least one metal layer attached to the surface of the liquid crystal polymer film. The liquid crystal polymer film has a melting point greater than or equal to 345°C. The liquid crystal polymer film includes a liquid crystal polymer, which is polymerized by reactants. The reactants include a plurality of first monomers, a plurality of second monomers, a plurality of third monomers, a plurality of fourth monomers or a combination thereof. These first monomers are aromatic dicarboxylic acids, aliphatic dicarboxylic acids or a combination thereof, these second monomers are aromatic hydroxycarboxylic acids, these third monomers are aromatic diols, aliphatic diols or a combination thereof, and these fourth monomers are aromatic diamines, aromatic hydroxylamines, aromatic aminocarboxylic acids or a combination thereof.
[0004] In some embodiments, the liquid crystal polymer is polymerized from aromatic diol, aromatic dicarboxylic acid and aromatic hydroxycarboxylic acid.
[0005] In some embodiments, the liquid crystal polymer is polymerized from aromatic dicarboxylic acid, aromatic hydroxycarboxylic acid, and aromatic hydroxylamine.
[0006] In some embodiments, the liquid crystal polymer is polymerized from aromatic dicarboxylic acid, aromatic hydroxycarboxylic acid and aliphatic diol.
[0007] In some embodiments, the liquid crystal polymer includes a plurality of first monomer units, a plurality of second monomer units, a plurality of third monomer units, and a plurality of fourth monomer units. Each first monomer unit is Each second monomer unit is Each third monomer unit is Each fourth monomer unit is
[0008] In some embodiments, in the liquid crystal polymer, the first monomer units are 60 mol % to 74 mol %, the second monomer units are 14 mol % to 16 mol %, the third monomer units are 5 mol % to 13 mol %, and the fourth monomer units are 5 mol % to 13 mol %.
[0009] In some embodiments, in the liquid crystal polymer, the first monomer units are 60 mol % to 74 mol %, the second monomer units are 16 mol % to 18 mol %, the third monomer units are 9 mol % to 12 mol %, and the fourth monomer units are 9 mol % to 12 mol %.
[0010] In some embodiments, the liquid crystal polymer includes a plurality of first monomer units and a plurality of second monomer units. Each first monomer unit is Each second monomer unit is The first monomer units are 70 mol% to 85 mol%, and the second monomer units are 15 mol% to 30 mol%.
[0011] In some embodiments, the liquid crystal polymer includes a plurality of first monomer units, a plurality of second monomer units, and a plurality of third monomer units. Each first monomer unit is Each second monomer unit is Each third monomer unit is The first monomer units are 55 mol% to 65 mol%, the second monomer units are 15 mol% to 25 mol%, and the third monomer units are 15 mol% to 25 mol%.
[0012] The present disclosure provides a multilayer board, which includes at least one single-sided board or at least one double-sided board, and the laminate board described in any of the above embodiments. The laminate board is attached to at least one single-sided board or at least one double-sided board.
[0013] The present disclosure provides a method for manufacturing a laminate, which includes the following operations. A liquid crystal polymer film is made of a liquid crystal polymer, and the liquid crystal polymer has a melting point greater than or equal to 345°C. The liquid crystal polymer is polymerized by reactants, and the reactants include a plurality of first monomers, a plurality of second monomers, a plurality of third monomers, a plurality of fourth monomers or a combination thereof. These first monomers are aromatic dicarboxylic acids, aliphatic dicarboxylic acids or a combination thereof, these second monomers are aromatic hydroxycarboxylic acids, these third monomers are aromatic diols, aliphatic diols or a combination thereof, and these fourth monomers are aromatic diamines, aromatic hydroxylamines, aromatic aminocarboxylic acids or a combination thereof. At least one metal layer is formed and attached to the surface of the liquid crystal polymer film.
[0014] In some embodiments, the liquid crystal polymer is polymerized from aromatic diol, aromatic dicarboxylic acid and aromatic hydroxycarboxylic acid.
[0015] In some embodiments, the liquid crystal polymer includes a plurality of first monomer units, a plurality of second monomer units, a plurality of third monomer units, and a plurality of fourth monomer units. Each first monomer unit is Each second monomer unit is Each third monomer unit is Each fourth monomer unit is
[0016] In some embodiments, in the liquid crystal polymer, the first monomer units are 60 mol % to 74 mol %, the second monomer units are 14 mol % to 16 mol %, the third monomer units are 5 mol % to 13 mol %, and the fourth monomer units are 5 mol % to 13 mol %.
[0017] In some embodiments, in the liquid crystal polymer, the first monomer units are 60 mol % to 74 mol %, the second monomer units are 16 mol % to 18 mol %, the third monomer units are 9 mol % to 12 mol %, and the fourth monomer units are 9 mol % to 12 mol %.
[0018] The present disclosure provides a method for manufacturing a laminate, which includes the following operations. A first liquid crystal polymer film is made of a liquid crystal polymer, and the liquid crystal polymer has a melting point of less than 345°C. The liquid crystal polymer is polymerized by reactants, and the reactants include a plurality of first monomers, a plurality of second monomers, a plurality of third monomers, a plurality of fourth monomers or a combination thereof. These first monomers are aromatic dicarboxylic acids, aliphatic dicarboxylic acids or a combination thereof, these second monomers are aromatic hydroxycarboxylic acids, these third monomers are aromatic diols, aliphatic diols or a combination thereof, and these fourth monomers are aromatic diamines, aromatic hydroxylamines, aromatic aminocarboxylic acids or a combination thereof. The first melting point of the first liquid crystal polymer film is T m , T m The first liquid crystal polymer film is heated by a heating process to form a second liquid crystal polymer film, wherein the second liquid crystal polymer film has a second melting point greater than or equal to 345° C. The heating temperature of the heating process is T m -40℃ to T m At least one metal layer is formed and attached to the surface of the second liquid crystal polymer film.
[0019] In some embodiments, the liquid crystal polymer is polymerized from aromatic dicarboxylic acid, aromatic hydroxycarboxylic acid, and aromatic hydroxylamine.
[0020] In some embodiments, the liquid crystal polymer is polymerized from aromatic dicarboxylic acid, aromatic hydroxycarboxylic acid and aliphatic diol.
[0021] In some embodiments, the liquid crystal polymer includes a plurality of first monomer units and a plurality of second monomer units. Each first monomer unit is Each second monomer unit is The first monomer units are 70 mol% to 85 mol%, and the second monomer units are 15 mol% to 30 mol%.
[0022] In some embodiments, the liquid crystal polymer includes a plurality of first monomer units, a plurality of second monomer units, and a plurality of third monomer units. Each first monomer unit is Each second monomer unit is Each third monomer unit is The first monomer units are 55 mol% to 65 mol%, the second monomer units are 15 mol% to 25 mol%, and the third monomer units are 15 mol% to 25 mol%. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] The present disclosure may be more fully understood by reading the following detailed description of the embodiments and referring to the accompanying drawings.
[0024] Figures 1 to 4 is a schematic cross-sectional view of a multilayer board according to various embodiments of the present disclosure;
[0025] Figure 5 is a schematic diagram of performing a thermal shock test according to various embodiments of the present disclosure;
[0026] Figure 6 Schematic bottom view of a laminate according to various embodiments of the present disclosure.
[0027]
Explanation of symbols
[0028] 110, 120, 210, 220, 310, 320, 410, 420, 430, 440, 450, 460, 510, 520: laminated board
[0029] 212, 222, 312, 322, 512, 522: Liquid crystal polymer film
[0030] 214, 216, 224, 314, 324, 514, 524, 526: metal layer
[0031] 530: Thermocouple
[0032] 532: cushion
[0033] ML1, ML2, ML3, ML4, ML5: Multilayer boards
[0034] S1, S3, S5, S7, S9, S11: upper surface
[0035] S2, S4, S6, S8, S10, S12: bottom surface DETAILED DESCRIPTION
[0036] The following multiple embodiments are described and disclosed in detail with the accompanying drawings. For the purpose of clarity, many practical details will be described together in the following description. However, it should be understood that these practical details are not intended to limit the present disclosure. That is, in some embodiments of the present disclosure, these practical details are not necessary. In addition, to simplify the drawings, some conventional structures and elements will be illustrated in schematic form in the drawings.
[0037] Although a series of operations or steps are used below to illustrate the methods disclosed herein, the order in which these operations or steps are shown should not be construed as a limitation of the present disclosure. For example, certain operations or steps may be performed in different orders and / or simultaneously with other steps. In addition, it is not necessary to perform all of the operations, steps, and / or features illustrated to achieve an embodiment of the present disclosure. In addition, each operation or step described herein may include several sub-steps or actions.
[0038] The present disclosure provides a laminate, which includes a liquid crystal polymer film and at least one metal layer attached to the surface of the liquid crystal polymer film. The liquid crystal polymer film has a melting point greater than or equal to 345°C. In some embodiments, the melting point is 345°C to 400°C, for example: 345, 350, 355, 360, 365, 370, 375, 385, 390, 395 or 400°C. The liquid crystal polymer film includes a liquid crystal polymer, which is polymerized by reactants. The reactants include a plurality of first monomers, a plurality of second monomers, a plurality of third monomers, a plurality of fourth monomers or a combination thereof. These first monomers are aromatic dicarboxylic acids, aliphatic dicarboxylic acids or a combination thereof, these second monomers are aromatic hydroxycarboxylic acids, these third monomers are aromatic diols, aliphatic diols or a combination thereof, and these fourth monomers are aromatic diamines, aromatic hydroxylamines, aromatic aminocarboxylic acids or a combination thereof. Since the liquid crystal polymer film has good heat resistance, the laminate can withstand a thermal shock test at 250° C. to 320° C. Specifically, the metal layer will not sink into the liquid crystal polymer film or deform during the thermal shock test.
[0039] The present disclosure provides a multilayer board, which includes at least one single-sided board or at least one double-sided board, and the above-mentioned laminated board. The laminated board is attached to at least one single-sided board or at least one double-sided board. In detail, the laminated board and at least one single-sided board or at least one double-sided board are pressed together. Since the laminated board of the present disclosure has good heat resistance, when the multilayer laminated board of the present disclosure is hot-pressed to form a multilayer board, the metal circuit can be prevented from sinking into the liquid crystal polymer film, so that the circuit deformation can be avoided to cause circuit impedance errors, increased transmission losses, and increased crosstalk between circuits. Therefore, the multilayer board can have good quality after hot pressing.
[0040] Figure 1 Schematic cross-sectional view of a multilayer board according to various embodiments of the present disclosure. Figure 1 As shown, the multilayer board ML1 includes a laminate board 110 and a laminate board 120. The laminate board 110 and the laminate board 120 each include a liquid crystal polymer film having a melting point greater than or equal to 345°C and at least one metal layer (not shown) attached to the surface of the liquid crystal polymer film. Since the liquid crystal polymer film has a high melting point, when the laminate board 110 and the laminate board 120 are pressed (hot pressed) together to form the multilayer board ML1, the metal layer will not sink into the liquid crystal polymer film and will not deform. Accordingly, the multilayer board ML1 can have good quality after pressing. In some embodiments, the laminate board 110 and the laminate board 120 are independently single-sided boards or double-sided boards.
[0041] Figure 2 It is a cross-sectional schematic diagram of a multilayer board according to various embodiments of the present disclosure. Multilayer board ML2 includes laminate board 210 and laminate board 220. Laminate board 210 is a double-sided board, and laminate board 220 is a single-sided board. Laminate board 210 includes a liquid crystal polymer film 212, a metal layer 214 and a metal layer 216, and metal layer 214 and metal layer 216 are respectively attached to the upper surface S1 and the lower surface S2 of the liquid crystal polymer film 212. In more detail, metal layer 214 directly contacts the upper surface S1, and metal layer 216 directly contacts the lower surface S2. Laminate board 220 includes a liquid crystal polymer film 222 and a metal layer 224. Metal layer 224 is attached to the upper surface S3 of the liquid crystal polymer film 222. In more detail, metal layer 224 directly contacts the upper surface S3. Both liquid crystal polymer films 212 and 222 have a melting point greater than or equal to 345°C. As Figure 2As shown, the metal layers 214, 216, and 224 are metal circuits, which can also be called patterned metal layers. The metal circuits are, for example, copper circuits. The method of forming the metal circuits includes: forming a metal foil (such as a copper foil) on the surface of the liquid crystal polymer film, and then etching the metal foil to form the metal circuits. The method of forming the metal foil is, for example, sputtering, electroless plating, or electrolytic plating. In other embodiments, the metal circuits are formed directly on the surface of the liquid crystal polymer film by printing or electroplating. However, in other embodiments, the metal layers 214, 216, and 224 may be unetched metal foils, so that the upper surfaces S1, S2, and S3 are completely covered by the metal layers 214, 216, and 224, respectively. In some embodiments, the liquid crystal polymer films 212 and 222 are independently thermoplastic liquid crystal polymer films or thermotropic liquid crystal polymer films.
[0042] Please continue to refer to Figure 2 , the laminate 210 and the laminate 220 are overlapped so that the metal layer 214 contacts the lower surface S4 of the liquid crystal polymer film 222. Since the liquid crystal polymer film 212 has a high melting point, when the laminate 210 and the laminate 220 are pressed (hot pressed) to form the multilayer board ML2, the metal layer 214 will not sink into the liquid crystal polymer film 212, and the metal layer 214 will not be deformed due to pressing. Therefore, the distance between the metal layer 214 and the metal layer 216 can meet the predetermined circuit design. According to the above, pressing (hot pressing) will not cause impedance errors of the predetermined circuit design, will not increase signal transmission loss, and will not increase crosstalk between lines. The multilayer board ML2 can have good quality.
[0043] Figure 3 It is a cross-sectional schematic diagram of a multilayer board according to various embodiments of the present disclosure. Multilayer board ML3 includes laminate board 310 and laminate board 320. Laminate board 310 and laminate board 320 are both single-sided boards. Laminate board 310 includes a liquid crystal polymer film 312 and a metal layer 314, wherein the metal layer 314 is attached to the upper surface S5 of the liquid crystal polymer film 312, and the lower surface S6 of the liquid crystal polymer film 312 is not covered by the metal layer. In more detail, the metal layer 314 is in direct contact with the upper surface S5. Laminate board 320 includes a liquid crystal polymer film 322 and a metal layer 324. The metal layer 324 is attached to the upper surface S7 of the liquid crystal polymer film 322. In more detail, the metal layer 324 is in direct contact with the upper surface S7. The liquid crystal polymer films 312 and 322 have a melting point greater than or equal to 345°C. As Figure 3 As shown, the metal layers 314 and 324 are metal lines, which can also be called patterned metal layers. However, in other embodiments, the metal layers 314 and 324 can be unetched metal foils, so that the upper surfaces S5 and S7 are completely covered by the metal layers 314 and 324 respectively.
[0044] Please continue to refer to Figure 3 , the laminated board 310 and the laminated board 320 are overlapped so that the metal layer 314 contacts the lower surface S8 of the liquid crystal polymer film 322. Since the liquid crystal polymer film 312 has a high melting point, when the laminated board 310 and the laminated board 320 are pressed (hot pressed) to form the multilayer board ML3, the metal layer 314 will not sink into the liquid crystal polymer film 312, and the metal layer 314 will not be deformed by pressing. Therefore, pressing (hot pressing) will not cause impedance errors in the predetermined circuit design, will not increase signal transmission losses, and will not increase crosstalk between lines. The multilayer board ML3 can have good quality.
[0045] Figure 4 Schematic cross-sectional view of a multilayer board according to various embodiments of the present disclosure. Multilayer board ML4 includes laminates 410, 420, 430, 440, 450, 460, each of which contains a liquid crystal polymer film having a melting point greater than or equal to 345°C. Each laminate may be a single-sided board or a double-sided board. The implementation of the single-sided board may refer to the implementation of the aforementioned laminate 220, laminate 310 or laminate 320, and the implementation of the double-sided board may refer to the implementation of the aforementioned laminate 210. Laminated boards 410, 420, 430, 440, 450, 460 are laminated to form multilayer board ML4. In multilayer board ML4, the number of laminates may be adjusted arbitrarily according to design requirements, and the number may be 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20 or 21, but is not limited thereto.
[0046] The present disclosure provides a method for manufacturing a laminate, which includes the following operations. A liquid crystal polymer film is made from a liquid crystal polymer, the liquid crystal polymer having a melting point greater than or equal to 345°C. In some embodiments, the melting point is 345°C to 400°C, for example: 345, 350, 355, 360, 365, 370, 375, 385, 390, 395 or 400°C. The liquid crystal polymer is polymerized by reactants, and the reactants include a plurality of first monomers, a plurality of second monomers, a plurality of third monomers, a plurality of fourth monomers or a combination thereof. These first monomers are aromatic dicarboxylic acids, aliphatic dicarboxylic acids or a combination thereof, these second monomers are aromatic hydroxycarboxylic acids, these third monomers are aromatic diols, aliphatic diols or a combination thereof, and these fourth monomers are aromatic diamines, aromatic hydroxylamines, aromatic aminocarboxylic acids or a combination thereof. At least one metal layer is formed and attached to the surface of the liquid crystal polymer film.
[0047] For example, the first monomer includes
[0048] HOOC(CH2) nCOOH (n is an integer from 2 to 12) or a combination thereof, but not limited thereto. A1 is a halogen group or an alkyl group, the halogen group is, for example, a fluorine group, a chlorine group, a bromine group or an iodine group, and the alkyl group is, for example, a methyl group, an ethyl group, a n-propyl group or an isopropyl group. For example, the second monomer includes or a combination thereof, but not limited thereto. A2 is a halogen group or an alkyl group, the halogen group is, for example, a fluorine group, a chlorine group, a bromine group or an iodine group, and the alkyl group is, for example, a methyl group, an ethyl group, a n-propyl group or an isopropyl group. For example, the third monomer includes
[0049] HO(CH2) n OH (n is an integer from 2 to 12) or a combination thereof, but not limited thereto. A3 and A4 are independently halogen or alkyl, A5 is H, halogen or alkyl, the halogen is, for example, fluoro, chloro, bromo or iodo, the alkyl is, for example, methyl, ethyl, n-propyl or isopropyl. For example, the fourth monomer includes or a combination thereof, but not limited thereto.
[0050] In some embodiments, the liquid crystal polymer having a melting point greater than or equal to 345° C. is polymerized from an aromatic diol and an aromatic dicarboxylic acid.
[0051] In some embodiments, the liquid crystal polymer having a melting point greater than or equal to 345° C. is polymerized from an aromatic diol and an aromatic hydroxycarboxylic acid.
[0052] In some embodiments, the liquid crystal polymer is a first type thermotropic liquid crystal polymer. In some embodiments, the first type thermotropic liquid crystal polymer contains a plurality of first monomer units, a plurality of second monomer units, and a plurality of third monomer units. Each first monomer unit is Each second monomer unit is Each third monomer unit is
[0053] In some embodiments, a liquid crystal polymer having a melting point greater than or equal to 345° C. is polymerized from an aromatic diol, an aromatic dicarboxylic acid, and an aromatic hydroxycarboxylic acid. For example, a liquid crystal polymer is polymerized from 4-Hydroxybenzoic acid (HBA), 6-Hydroxy-2-naphthalene carboxylicacid (HNA), terephthalic acid (TPA), and hydroquinone (HQ). The following first monomer unit, second monomer unit, third monomer unit, and fourth monomer unit can be obtained from HBA, HNA, TPA, and HQ, respectively. In some embodiments, a liquid crystal polymer includes a plurality of first monomer units, a plurality of second monomer units, a plurality of third monomer units, and a plurality of fourth monomer units. Each first monomer unit is Each second monomer unit is Each third monomer unit is Each fourth monomer unit is In some embodiments, in the liquid crystal polymer, the first monomer units are 60 mol% to 74 mol%, the second monomer units are 14 mol% to 16 mol%, the third monomer units are 5 mol% to 13 mol%, and the fourth monomer units are 5 mol% to 13 mol%. In some embodiments, in the liquid crystal polymer, the first monomer units are 60 mol% to 74 mol%, the second monomer units are 16 mol% to 18 mol%, the third monomer units are 9 mol% to 12 mol%, and the fourth monomer units are 9 mol% to 12 mol%. The molar percentages of the first monomer unit, the second monomer unit, the third monomer unit, and the fourth monomer unit may be any positive integer within the above numerical range.
[0054] Next, thermal shock tests were performed on laminates containing liquid crystal polymer films and copper circuits. Figure 5 , Figure 5Schematic diagram of performing thermal shock test according to various embodiments of the present disclosure. Laminated board 510 includes a liquid crystal polymer film 512 and a metal layer 514, and the metal layer 514 is attached to the lower surface S10 of the liquid crystal polymer film 512. Laminated board 520 includes a liquid crystal polymer film 522, a metal layer 524 and a metal layer 526, and the metal layer 526 and the metal layer 524 are attached to the upper surface S11 and the lower surface S12 of the liquid crystal polymer film 522, respectively. Laminated board 510 is a single-sided flexible printed circuit board, and laminated board 520 is a double-sided flexible printed circuit board. Laminated boards 510 and laminated boards 520 are overlapped so that the metal layer 524 contacts the upper surface S9 of the liquid crystal polymer film 512. Laminated boards 510 and laminated boards 520 are hot pressed by the buffer pad 532 of the hot electrode 530, wherein the thickness of the buffer pad 532 is 25 μm. The materials of the liquid crystal polymer films 512 and 522 are the same, each including a liquid crystal polymer polymerized from HBA, HNA, TPA and HQ, so the liquid crystal polymer contains the above-mentioned first monomer unit, second monomer unit, third monomer unit and fourth monomer unit. The thickness of the liquid crystal polymer films 512 and 522 is 50μm, and the metal layers 514, 524, and 526 are copper lines with a thickness of 12μm, a line width of 1mm, and a line spacing of 1mm. The hot pressing temperature can be between 250°C and 320°C, the hot pressing pressure is 10N, the hot pressing time is 20 seconds, and the number of hot pressing times is 10. Please refer to Figure 6 , Figure 6 Schematic bottom view of a laminate according to various embodiments of the present disclosure. Figure 5 The laminate 510 is shown as Figure 6 The circuit patterns of the metal layers 524 and 526 can be designed with reference to the circuit pattern of the metal layer 514. The test results of thermal shock on different liquid crystal polymer films are shown in Table 1 below.
[0055] Table 1
[0056]
[0057] As can be seen from Table 1, the melting points of the liquid crystal polymer films of Examples 1 to 4 are higher than 345°C. The liquid crystal polymer film with a melting point of 350°C can withstand a hot pressing temperature of 275°C. Specifically, the copper circuit of the liquid crystal polymer laminate will not sink into the liquid crystal polymer film at 275°C. The liquid crystal polymer film with a melting point of 355°C can withstand a hot pressing temperature of 285°C. Specifically, the copper circuit of the liquid crystal polymer laminate will not sink into the liquid crystal polymer film at 285°C. In contrast, in Comparative Examples 1 and 2, since the melting points of the liquid crystal polymer films are lower than 345°C, the copper circuit will completely sink into the liquid crystal polymer film.
[0058] The present disclosure provides another method for manufacturing a laminate, which includes the following operations. A first liquid crystal polymer film is made of a liquid crystal polymer, and the liquid crystal polymer has a melting point less than 345°C. The liquid crystal polymer is polymerized by reactants, and the reactants include a plurality of first monomers, a plurality of second monomers, a plurality of third monomers, a plurality of fourth monomers or a combination thereof. These first monomers are aromatic dicarboxylic acids, aliphatic dicarboxylic acids or a combination thereof, these second monomers are aromatic hydroxycarboxylic acids, these third monomers are aromatic diols, aliphatic diols or a combination thereof, and these fourth monomers are aromatic diamines, aromatic hydroxylamines, aromatic aminocarboxylic acids or a combination thereof. The implementation methods of the first monomer, the second monomer, the third monomer and the fourth monomer refer to the aforementioned implementation methods and will not be repeated here. The melting point of the liquid crystal polymer can be adjusted to be less than, equal to or greater than 345°C by adjusting the monomer ratio of the synthesized liquid crystal polymer. A first melting point of the first liquid crystal polymer film is T m , T m The first liquid crystal polymer film is heated by a heating process to form a second liquid crystal polymer film, wherein the second liquid crystal polymer film has a second melting point greater than or equal to 345° C. The heating temperature of the heating process is T m -40℃ to T m At least one metal layer is formed and attached to the surface of the second liquid crystal polymer film. The laminated board in any of the above embodiments can be manufactured by this method, and the laminated board can be a single-sided board or a double-sided board.
[0059] In some embodiments, the heating temperature is, for example, T m -40, T m -35, T m -30, T m -25, T m -20, T m -15, T m -10, T m-5 or Tm℃. When heated, the polymers in the liquid crystal polymer film will rearrange, increasing the molecular weight of the polymer and arranging the polymer more neatly, thereby increasing the melting point of the liquid crystal polymer film. Raising the melting point can make the liquid crystal polymer film have better heat resistance. When a multi-layer liquid crystal polymer laminate is pressed to form a multi-layer board, the pressing quality can be better and the metal circuit is not easy to sink into the liquid crystal polymer film. In some embodiments, the heating rate of the heating process is 0.1℃ / min to 30℃ / min. The heating rate is, for example, 0.1, 0.5, 1, 5, 10, 15, 20, 25 or 30℃ / min. In some embodiments, the heating time of the heating process is 10 minutes to 900 minutes. The heating time is, for example, 10, 20, 40, 60, 80, 100, 200, 300, 400, 500, 600, 700, 800 or 900 minutes. In some embodiments, the heating process is performed in an inert environment. For example, the inert gas in the inert environment is argon, nitrogen, or a combination thereof.
[0060] In some embodiments, the liquid crystal polymer having a melting point less than 345°C is polymerized from an aromatic diol, an aromatic dicarboxylic acid, and an aromatic hydroxycarboxylic acid. In some embodiments, the liquid crystal polymer having a melting point less than 345°C is polymerized from an aromatic diol and an aromatic dicarboxylic acid. In some embodiments, the liquid crystal polymer having a melting point less than 345°C is polymerized from an aromatic diol and an aromatic hydroxycarboxylic acid.
[0061] In some embodiments, the reactants include different first aromatic hydroxycarboxylic acids and second aromatic hydroxycarboxylic acids. In some embodiments, the liquid crystal polymer film includes a second type thermotropic liquid crystal polymer. In some embodiments, the second type thermotropic liquid crystal polymer is obtained by polymerization of p-hydroxybenzoic acid (HBA) and 6-hydroxy-2-naphthoic acid (HNA). The following first monomer units and second monomer units can be obtained from HBA and HNA, respectively. In some embodiments, the liquid crystal polymer includes a plurality of first monomer units and a plurality of second monomer units. Each first monomer unit is Each second monomer unit is The first monomer units are 70 mol% to 85 mol%, and the second monomer units are 15 mol% to 30 mol%. The molar percentages of the first monomer units and the second monomer units can be any positive integer within the above numerical range.
[0062] In some embodiments, a liquid crystal polymer having a melting point less than 345°C is polymerized from an aromatic dicarboxylic acid, an aromatic hydroxycarboxylic acid, and an aromatic hydroxylamine. In some embodiments, a liquid crystal polymer is polymerized from 6-hydroxy-2-naphthoic acid (HNA), terephthalic acid (TPA), and p-Aminophenol (AP). The second monomer unit, the third monomer unit, and the fourth monomer unit in the following liquid crystal polymer can be obtained from HNA, TPA, and AP, respectively. In some embodiments, the liquid crystal polymer includes a plurality of second monomer units, a plurality of third monomer units, and a plurality of fourth monomer units. Each second monomer unit is Each third monomer unit is Each fourth monomer unit is The second monomer units are 55 mol% to 65 mol%, the third monomer units are 15 mol% to 25 mol%, and the fourth monomer units are 15 mol% to 25 mol%. The molar percentages of the second monomer units, the third monomer units, and the fourth monomer units can be any positive integer within the above numerical range.
[0063] In some embodiments, a liquid crystal polymer having a melting point of less than 345°C is polymerized from an aromatic diol, an aromatic dicarboxylic acid, and an aromatic hydroxycarboxylic acid. In some embodiments, a liquid crystal polymer is polymerized from p-hydroxybenzoic acid (HBA), 6-hydroxy-2-naphthoic acid (HNA), terephthalic acid (TPA), and 4,4'-biphenol (BP). The first monomer unit, the second monomer unit, the third monomer unit, and the fifth monomer unit in the following liquid crystal polymer can be obtained from HBA, HNA, TPA, and BP, respectively. In some embodiments, the liquid crystal polymer includes a plurality of first monomer units, a plurality of second monomer units, a plurality of third monomer units, and a plurality of fifth monomer units. Each first monomer unit is Each second monomer unit is Each third monomer unit is Each fifth monomer unit is
[0064] The melting points and molar percentages of the monomer units of the liquid crystal polymer films 1 to 4 are shown in Table 2 below.
[0065] Table 2
[0066]
[0067] In some embodiments, the liquid crystal polymer is polymerized from aromatic dicarboxylic acid, aromatic hydroxycarboxylic acid and aliphatic diol. In some embodiments, the liquid crystal polymer includes the following monomer units: And *-OCH2CH2O-*.
[0068] Next, with the aforementioned Figure 5 The configuration shown in the figure was used for the thermal shock test, and the test results are shown in Table 3 below. During the test, the liquid crystal polymer film of Comparative Example 3 and Examples 5 to 7 selected the liquid crystal polymer film 1 or liquid crystal polymer film 3 in Table 2 above, and the melting point of the liquid crystal polymer film was adjusted by a heating process to obtain the melting point after heating in Table 3. A copper circuit was formed on the liquid crystal polymer film, and then the thermal shock test was performed. The liquid crystal polymer film of Comparative Example 4 and Examples 8 to 9 selected the liquid crystal polymer film 2 in Table 2 above, and the melting point of the liquid crystal polymer film was adjusted by a heating process to obtain the melting point after heating in Table 3. A copper circuit was formed on the liquid crystal polymer film, and then the thermal shock test was performed.
[0069] Table 3
[0070]
[0071]
[0072] As shown in Table 3, the liquid crystal polymer films with melting points of 345°C, 350°C and 355°C after heating can withstand hot pressing temperatures of 260°C, 275°C and 285°C, respectively. Specifically, the copper circuits of these liquid crystal polymer laminates will not sink into the liquid crystal polymer films at the above hot pressing temperatures. In contrast, in Comparative Examples 3 and 4, since the melting points of the liquid crystal polymer films are lower than 345°C, the copper circuits will completely sink into the liquid crystal polymer films.
[0073] In summary, the present disclosure provides a laminate and a manufacturing method thereof and a multilayer board. The laminate includes a liquid crystal polymer film and at least one metal layer attached to the surface of the liquid crystal polymer film. Since the laminate of the present disclosure has good heat resistance, when the multilayer laminate is hot pressed to form a multilayer board, the metal circuit can be prevented from sinking into the liquid crystal polymer film, so that the circuit deformation can be avoided to cause circuit impedance error, increase in transmission loss and increase in crosstalk between circuits. Therefore, the multilayer board can have good quality after hot pressing.
[0074] Although the present disclosure has been described in considerable detail with reference to certain embodiments, other embodiments are possible. Therefore, the spirit and scope of the appended claims should not be limited to the description of the embodiments contained herein.
[0075] It is obvious to those with ordinary knowledge in the art that various modifications and changes can be made to the structure of the present disclosure without departing from the scope or spirit of the present disclosure. In view of the foregoing, the present disclosure is intended to cover the modifications and changes of the present disclosure that fall within the appended claims.
Claims
1. A laminated board, characterized in that: include: A liquid crystal polymer film having a melting point greater than or equal to 345° C., wherein the liquid crystal polymer film comprises a liquid crystal polymer, which is polymerized by a reactant, wherein the reactant comprises a plurality of first monomers, a plurality of second monomers, a plurality of third monomers, a plurality of fourth monomers or a combination thereof, wherein the plurality of first monomers are aromatic dicarboxylic acids, aliphatic dicarboxylic acids or a combination thereof, the plurality of second monomers are aromatic hydroxycarboxylic acids, the plurality of third monomers are aromatic diols, aliphatic diols or a combination thereof, and the plurality of fourth monomers are aromatic diamines, aromatic hydroxylamines, aromatic aminocarboxylic acids or a combination thereof; and At least one metal layer is attached to a surface of the liquid crystal polymer film.
2. The laminate according to claim 1, wherein: The liquid crystal polymer is polymerized from the aromatic diol, the aromatic dicarboxylic acid and the aromatic hydroxycarboxylic acid.
3. The laminate according to claim 1, wherein: The liquid crystal polymer is polymerized from the aromatic dicarboxylic acid, the aromatic hydroxycarboxylic acid and the aromatic hydroxylamine.
4. The laminate according to claim 1, wherein: The liquid crystal polymer is polymerized from the aromatic dicarboxylic acid, the aromatic hydroxycarboxylic acid and the aliphatic diol.
5. The laminate according to claim 1, wherein: The liquid crystal polymer includes a plurality of first monomer units, a plurality of second monomer units, a plurality of third monomer units and a plurality of fourth monomer units, each of the first monomer units is Each of the second monomer units is Each of the third monomer units is Each of the fourth monomer units is 6. The laminate according to claim 5, wherein: In the liquid crystal polymer, the first monomer units account for 60 mol% to 74 mol%, the second monomer units account for 14 mol% to 16 mol%, the third monomer units account for 5 mol% to 13 mol%, and the fourth monomer units account for 5 mol% to 13 mol%.
7. The laminate according to claim 5, wherein: In the liquid crystal polymer, the first monomer units account for 60 mol% to 74 mol%, the second monomer units account for 16 mol% to 18 mol%, the third monomer units account for 9 mol% to 12 mol%, and the fourth monomer units account for 9 mol% to 12 mol%.
8. The laminate according to claim 1, wherein: The liquid crystal polymer includes a plurality of first monomer units and a plurality of second monomer units, each of the first monomer units is Each of the second monomer units is The plurality of first monomer units is 70 mol % to 85 mol %, and the plurality of second monomer units is 15 mol % to 30 mol %.
9. The laminate according to claim 1, wherein: The liquid crystal polymer includes a plurality of first monomer units, a plurality of second monomer units and a plurality of third monomer units, each of the first monomer units is Each of the second monomer units is Each of the third monomer units is The plurality of first monomer units are 55 mol % to 65 mol %, the plurality of second monomer units are 15 mol % to 25 mol %, and the plurality of third monomer units are 15 mol % to 25 mol %.
10. A multilayer board, characterized in that: include: At least one single-sided board or at least one double-sided board; as well as The laminate as claimed in any one of claims 1 to 9 is bonded to the at least one single-sided board or the at least one double-sided board.
11. A method for manufacturing a laminate, characterized in that: include: A liquid crystal polymer film is prepared by using a liquid crystal polymer, the liquid crystal polymer having a melting point greater than or equal to 345° C., wherein the liquid crystal polymer is polymerized by a reactant, the reactant comprising a plurality of first monomers, a plurality of second monomers, a plurality of third monomers, a plurality of fourth monomers or a combination thereof, the plurality of first monomers are aromatic dicarboxylic acids, aliphatic dicarboxylic acids or a combination thereof, the plurality of second monomers are aromatic hydroxycarboxylic acids, the plurality of third monomers are aromatic diols, aliphatic diols or a combination thereof, and the plurality of fourth monomers are aromatic diamines, aromatic hydroxylamines, aromatic aminocarboxylic acids or a combination thereof; as well as At least one metal layer is formed and attached to a surface of the liquid crystal polymer film.
12. The method according to claim 11, characterized in that The liquid crystal polymer is polymerized from the aromatic diol, the aromatic dicarboxylic acid and the aromatic hydroxycarboxylic acid.
13. The method according to claim 11, characterized in that The liquid crystal polymer includes a plurality of first monomer units, a plurality of second monomer units, a plurality of third monomer units and a plurality of fourth monomer units, each of the first monomer units is Each of the second monomer units is Each of the third monomer units is Each of the fourth monomer units is 14. The method according to claim 13, characterized in that In the liquid crystal polymer, the first monomer units account for 60 mol% to 74 mol%, the second monomer units account for 14 mol% to 16 mol%, the third monomer units account for 5 mol% to 13 mol%, and the fourth monomer units account for 5 mol% to 13 mol%.
15. The method according to claim 13, characterized in that In the liquid crystal polymer, the first monomer units account for 60 mol% to 74 mol%, the second monomer units account for 16 mol% to 18 mol%, the third monomer units account for 9 mol% to 12 mol%, and the fourth monomer units account for 9 mol% to 12 mol%.
16. A method for manufacturing a laminate, characterized in that: include: A first liquid crystal polymer film is prepared by using a liquid crystal polymer, wherein the liquid crystal polymer has a melting point of less than 345° C., wherein the liquid crystal polymer is polymerized by a reactant, wherein the reactant includes a plurality of first monomers, a plurality of second monomers, a plurality of third monomers, a plurality of fourth monomers or a combination thereof, wherein the plurality of first monomers are aromatic dicarboxylic acids, aliphatic dicarboxylic acids or a combination thereof, the plurality of second monomers are aromatic hydroxycarboxylic acids, the plurality of third monomers are aromatic diols, aliphatic diols or a combination thereof, the plurality of fourth monomers are aromatic diamines, aromatic hydroxylamines, aromatic aminocarboxylic acids or a combination thereof, and a first melting point of the first liquid crystal polymer film is T m , T m Less than 345℃; The first liquid crystal polymer film is heated by a heating process to form a second liquid crystal polymer film, wherein the second liquid crystal polymer film has a second melting point greater than or equal to 345° C., wherein a heating temperature of the heating process is T m -40℃ to T m ;as well as At least one metal layer is formed and attached to a surface of the second liquid crystal polymer film.
17. The method according to claim 16, characterized in that The liquid crystal polymer is polymerized from the aromatic dicarboxylic acid, the aromatic hydroxycarboxylic acid and the aromatic hydroxylamine.
18. The method according to claim 16, characterized in that The liquid crystal polymer is polymerized from the aromatic dicarboxylic acid, the aromatic hydroxycarboxylic acid and the aliphatic diol.
19. The method according to claim 16, characterized in that The liquid crystal polymer includes a plurality of first monomer units and a plurality of second monomer units, each of the first monomer units is Each of the second monomer units is The plurality of first monomer units is 70 mol % to 85 mol %, and the plurality of second monomer units is 15 mol % to 30 mol %.
20. The method of claim 16, wherein: The liquid crystal polymer includes a plurality of first monomer units, a plurality of second monomer units and a plurality of third monomer units, each of the first monomer units is Each of the second monomer units is Each of the third monomer units is The plurality of first monomer units are 55 mol % to 65 mol %, the plurality of second monomer units are 15 mol % to 25 mol %, and the plurality of third monomer units are 15 mol % to 25 mol %.