LIQUID ORGANIC HYDROGEN CARRIER COMPOSITIONS COMPRISING MIXTURES OF MONOBENZYLtoluene ISOMERS AND

By controlling the component ratio of the benzyl toluene isomer mixture and using a catalyst, the problem of reduced hydrogen storage/release cycle efficiency is solved, and the reversibility and stability of efficient hydrogen storage and release are achieved.

CN118900820APending Publication Date: 2024-11-05INDUSTRY UNIVERSITY COOPERATION FOUNDATION HANYANG UNIVERSITY
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202380027842.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-17
Filing Date
2023-03-08
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

When a mixture of benzyl toluene isomer isomer used as a liquid organic hydrogen carrier in the prior art, the hydrogen storage/release cycle efficiency is reduced, especially in the hydrogenation/dehydrogenation cycle, the hydrogenation/dehydrogenation efficiency increases with the increase of the number of cycles. reduce.

Method used

By controlling the proportion of components in the benzyl toluene isomer mixture, especially the paraisomer content of at least 50 mol%, and hydrogenation and dehydrogenation in the presence of a catalyst, ensuring that the methyl fluorene content remains at the dehydrogenation level after dehydrogenation At least 10 mol%, porous inorganic oxides and active metal catalysts were used to improve hydrogenation/dehydrogenation efficiency.

Benefits of technology

It achieves efficient hydrogen storage/release for a long time, inhibits the decrease in efficiency in the hydrogenation/dehydrogenation cycle, and improves the reversibility and stability of hydrogen storage/release.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118900820A_ABST
    Figure CN118900820A_ABST
Patent Text Reader

Abstract

The present disclosure describes a technique that is based on the characteristics of a single structural isomer (ortho-isomer, meta-isomer, and para-isomer) of monobenzyltoluene, uses a mixture of composition-controlled monobenzyltoluene isomers as a liquid organic hydrogen carrier, by inhibiting factors that hinder the stable hydrogenation / dehydrogenation cycle, and uses the isomer mixture of monobenzyltoluene as a liquid organic hydrogen carrier. Hydrogen can be stored and released with high selective conversion and high efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a liquid organic hydrogen carrier composition containing a monobenzyltoluene isomer mixture, and a method for storing and releasing hydrogen using the same. More particularly, the present disclosure relates to using a monobenzyltoluene isomer mixture with controlled composition as a liquid organic hydrogen carrier based on the characteristics of the single positional isomers (ortho-isomer, meta-isomer and para-isomer) of monobenzyltoluene, and storing and releasing hydrogen in a highly selective conversion and efficient manner by suppressing factors that hinder a stable hydrogenation / dehydrogenation cycle. Background Art

[0002] As fossil fuel reserves decrease and environmental pollution problems such as carbon dioxide and pollutants produced during combustion lead to global warming become increasingly serious, the world's interest and demand for developing alternative energy sources are increasing dramatically.

[0003] As alternative energy sources, renewable energy such as wind energy, tidal energy, geothermal energy, hydrogen energy, and solar energy have attracted much attention. Each of the energy sources listed above has its own advantages and disadvantages. In this regard, since the instability of energy depends on time and natural environment, it is difficult to effectively demand and supply renewable energy. Therefore, in order to effectively replace traditional fossil fuels, it is necessary to develop storage and supply technology for surplus energy in order to stably supply energy.

[0004] From this perspective, hydrogen energy has received special attention because it (i) has the highest energy content per unit mass; (ii) produces only water during combustion, with no other harmful byproducts; (iii) has advantages in terms of reuse, because water, the main source of hydrogen, is abundant in nature and can be converted into water after use; and (iv) is suitable for gaining competitiveness in precision industry and IT industries that use hydrogen as a distributed energy resource. In addition, hydrogen can be produced using other renewable energy sources such as solar energy and wind energy, and can be widely used not only in various energy sources, but also in other industrial fields (such as various petrochemical fields), and is becoming an important energy source in the future at home and abroad.

[0005] In general, the research and development of hydrogen energy is mainly divided into the production, delivery (transportation) and storage of hydrogen. Hydrogen has a high energy storage capacity per unit mass, but a low energy storage capacity per unit volume, so the development of efficient hydrogen storage technology is crucial for the practical use of hydrogen energy. For example, it is known that the mass storage density of materials at 77K is 10wt% or more, but the volume storage density of these materials is 40g / L, which is very low for use as practical hydrogen storage materials. Therefore, the technology of storing as much hydrogen as possible in a storage medium that is as light and as compact as possible is currently being intensively studied.

[0006] In this regard, many countries have invested a lot of money in research and development over the years. The efficient hydrogen storage methods that have been researched and developed include: CGH2 method of compressing hydrogen at 700 bar pressure, and LH2 method of storing liquid hydrogen by liquefaction at -253℃. However, this pressurization or liquefaction method must maintain low temperature, and the density of liquid hydrogen is also very low, at 71.2kg / m 3 .

[0007] Recently, hydrogen storage technology has been developed using organic materials, such as liquid organic hydrogen carriers (LOHC) (U.S. Patent No. 7,901,491, etc.) for reversible catalytic hydrogenation / dehydrogenation. The advantages of LOHC technology are that it can not only store 5wt% or more of hydrogen recommended by the U.S. Department of Energy (DOE), but also operate in a low pressure range and is easy to regenerate the stored materials. In addition, since liquid fossil fuels have the advantages of easy handling and high energy density, it is possible to provide a practical hydrogen storage system that utilizes the existing liquid fuel transportation and storage infrastructure to achieve efficient transportation and storage (Energy Rev., 6 (2002) 141, Energy Environ. Sci., 8 (2015) 1035-1045).

[0008] There are already known technologies for using π-conjugated substrate compounds as LOHC materials (such as U.S. Patent No. 7,351,395, etc.), but due to the π-conjugation effect, it is difficult to obtain consistent reactivity, and such compounds are mostly in solid form, so they are used in a mixed form. In this regard, representative examples of LOHC materials include benzyltoluene, dibenzyltoluene, etc. (for example, Korean Patent Application Publication No. 2015-97558, etc.), among which monobenzyltoluene is particularly noteworthy.

[0009] In this regard, U.S. Patent Application Publication No. 2015 / 0266731 discloses the use of a monobenzyltoluene isomer mixture as LOHC, and the commercially available mixture is a heat transfer oil with the trade name Marlotherm LH (ortho: meta: para = 46:5:49). Compared with pure materials in the form of specific isomers, this product has more advantages in terms of economic benefits, such as easy availability.

[0010] However, when using a monobenzyltoluene isomer mixture as a LOHC, achieving rapid hydrogen storage / release efficiency is limited. In particular, as the hydrogen storage / release cycle proceeds, the hydrogenation / dehydrogenation efficiency decreases, which is undesirable.

[0011] Therefore, there is a need for a method capable of performing stable hydrogenation / dehydrogenation by identifying the hydrogenation / dehydrogenation tendency of monobenzyltoluene and suppressing the phenomenon that reduces the efficiency of the hydrogen storage / release cycle. Summary of the invention

[0012] Technical issues

[0013] One embodiment of the present disclosure provides a method that can achieve good hydrogen storage / release efficiency over a long period of time based on the identified hydrogenation / dehydrogenation tendency of each isomer of monobenzyltoluene as a liquid organic hydrogen carrier.

[0014] Another embodiment of the present disclosure provides a liquid organic hydrogen carrier suitable for reversible hydrogen storage / release via hydrogenation / dehydrogenation.

[0015] Technical Solution

[0016] A first aspect of the present disclosure provides a method for reversibly storing and releasing hydrogen, comprising:

[0017] a) providing a monobenzyltoluene (MBT) isomer mixture having a para-isomer content of at least 50 mol %;

[0018] b) hydrogenating a monobenzyltoluene (MBT) isomer mixture to store hydrogen; and

[0019] c) dehydrogenating the hydrogenated monobenzyltoluene (MBT) isomer mixture to release hydrogen therefrom,

[0020] wherein hydrogen is stored or released by alternating hydrogenation and dehydrogenation, and

[0021] The methylfluorene content in the dehydrogenated monobenzyltoluene (MBT) isomer mixture is maintained below 10 mol%.

[0022] In one embodiment, the halogen content in the monobenzyltoluene (MBT) isomer mixture may be maintained below 30 ppm (w / w).

[0023] In one embodiment, the monobenzyltoluene (MBT) isomer mixture may contain 42 mol% or less of ortho-benzyltoluene (o-MBT), 15 mol% or less of meta-benzyltoluene (m-MBT), and 55 to 90 mol% of para-benzyltoluene (p-MBT).

[0024] In one embodiment, step b) may be carried out in the presence of a catalyst, which may include a support comprising a porous inorganic oxide and at least one active metal selected from the group consisting of nickel, cobalt, palladium, platinum, iridium, ruthenium, rhodium, copper, gold, rhenium, zinc, molybdenum, tin, manganese, tungsten and germanium.

[0025] In one embodiment, the content of active metal in the catalyst used in step b) may be set to 0.1 to 50 wt%.

[0026] In one embodiment, the porous inorganic oxide in the catalyst used in step b) may be at least one selected from the group consisting of alumina, silica, silica-alumina, aluminum phosphate, zirconia, titania, cerium and yttrium.

[0027] In one embodiment, step c) may be performed in the presence of a catalyst, which may include a support comprising a porous inorganic oxide, an active metal, and sulfur.

[0028] In one embodiment, the active metal content of the catalyst used in step c) may be determined to be 0.1 to 10 wt %, and the sulfur content may be determined to be 0.001 to 2 wt %.

[0029] In one embodiment, the molar ratio of sulfur / active metal in the catalyst used in step c) may be determined to be in the range of 0.1 to 1.

[0030] In one embodiment, the porous inorganic oxide in the catalyst used in step c) may be alumina and the active metal may be platinum.

[0031] A second aspect of the present disclosure provides a liquid organic hydrogen carrier composition for reversible hydrogen storage / release, comprising:

[0032] 42 mol% or less of o-benzyltoluene (o-MBT);

[0033] 15 mol % or less of meta-benzyltoluene (m-MBT); and

[0034] 55 to 90 mol% of p-benzyltoluene (p-MBT),

[0035] The methylfluorene content is controlled below 10 mol%, and the halogen content is controlled below 30 ppm (w / w).

[0036] In one embodiment, the halogen may be chlorine.

[0037] Beneficial Effects

[0038] According to one embodiment of the present disclosure, based on the influence or tendency of the ortho-isomer, meta-isomer and para-isomer of monobenzyltoluene (MBT) on reversible hydrogenation (hydrogen storage) and dehydrogenation (hydrogen release), a composition-controlled monobenzyltoluene isomer mixture is used as LOHC, and further, the decrease in hydrogen storage / release efficiency occurring during the hydrogenation / dehydrogenation cycle can be suppressed. In addition, the use of a catalyst that can suppress the formation of methylfluorene during the dehydrogenation process can further improve the reversibility of long-term hydrogen storage / release. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 A schematic diagram showing the synthesis of o-benzyltoluene, m-benzyltoluene and p-benzyltoluene by reacting 2-methylbenzyl chloride, 3-methylbenzyl chloride and 4-methylbenzyl chloride with excess benzene in the presence of a homogeneous catalyst;

[0040] Figure 2 It is a hydrogen-rich (H 12 Figure 2 shows the GC analysis results of three isomers (ortho, meta and para) of monobenzyltoluene in the hydrogen-deficient (H0-MBT) and hydrogen-deficient (H0-MBT) states and an isomer mixture corresponding to the commercially available Marlotherm LH;

[0041] Figure 3 a to Figure 3 c shows the synthesis of three monobenzyltoluene isomers 1 H NMR (left) and 13 C NMR (right) analysis results;

[0042] Figure 4 a to Figure 4 c is a graph showing the hydrogenation results of three synthesized monobenzyltoluene isomers depending on the concentration of Cl (reaction conditions: 10 g of reactant, hydrogen pressure 50 bar, M / R of 0.15 mol%, 150° C. and 1200 rpm);

[0043] Figure 5 a to Figure 5 c is a graph showing the results of dehydrogenation of three synthesized monobenzyltoluene isomers depending on the concentration of Cl (reaction conditions: 1.5 g of reactant, 1 bar, M / R of 0.60 mol%, 260° C., 215 min and 200 rpm);

[0044] Figure 6 a and Figure 6 b is a graph showing the results of hydrogenation after removal of Cl from three synthesized monobenzyltoluene isomers (reaction conditions: 10 g of reactant, hydrogen pressure of 50 bar, M / R of 0.035 mol%, rotation speed of 1200 rpm);

[0045] Figure 7 a to Figure 7 c is a graph showing the results of dehydrogenation after removal of Cl from three synthesized monobenzyltoluene isomers (reaction conditions: 1.5 g of reactant, 1 bar, M / R of 0.60 mol%, 215 min and 200 rpm);

[0046] Figure 8 a and Figure 8 b shows the Arrhenius plot of hydrogenation and dehydrogenation after removal of Cl from the three synthesized monobenzyltoluene isomers (the conditions for hydrogenation and dehydrogenation are respectively Figure 6 and Figure 7 the same as in );

[0047] Fig. 9 a to Fig. 9 c shows the GC-FID analysis results of the dehydrogenated products after removing Cl from three synthesized monobenzyltoluene isomers (reaction conditions: 1.5 g reactant, 1 bar, M / R of 2.40 mol%, 260° C., 215 min, 200 rpm);

[0048] Fig.10 a to Fig.10 c is the DFT-based plot of the Pt(111), Ru(0001), and γ-Al2O3(110) sites for H0-MBT, cis-H 12 -MBT and trans-H 12 - Diagram of the adsorption energy evaluation results of MBT;

[0049] Fig.11 a and Fig.11 b is a graph showing the results of thermogravimetric analysis of catalysts (Al2O3 and Ru / Al2O3) adsorbed with three monobenzyltoluene isomers;

[0050] Fig.12 a and Fig.12 b is a graph showing the hydrogenation and dehydrogenation results of a binary physical mixture of two monobenzyltoluene isomers (para and meta) (hydrogenation conditions: 10 g reactant, hydrogen pressure 50 bar, M / R 0.035 mol%, 110° C. and 1200 rpm; dehydrogenation conditions: 1.5 g reactant, 1 bar, M / R 0.60 mol%, 240° C., 215 min and 200 rpm);

[0051] Fig.13 a and Fig.13 b is a graph showing the results of hydrogenation and dehydrogenation of a binary physical mixture of two monobenzyltoluene isomers (para and ortho) (hydrogenation conditions: 10 g reactant, hydrogen pressure 50 bar, M / R 0.035 mol%, 110° C. and 1200 rpm; dehydrogenation conditions: 1.5 g reactant, 1 bar, M / R 0.60 mol%, 240° C., 215 min and 200 rpm);

[0052] Fig.14 a and Fig.14b is a graph showing the hydrogenation and dehydrogenation results of a ternary physical mixture of three monobenzyltoluene isomers (ortho, meta and para) (hydrogenation conditions: 10 g reactant, hydrogen pressure 50 bar, M / R 0.035 mol%, 110° C. and 1200 rpm; dehydrogenation conditions: 1.5 g reactant, 1 bar, M / R 0.60 mol%, 240° C., 215 min and 200 rpm);

[0053] Fig.15 The hydrogen-rich state (H) of the selective isomer compositions (p72 and p55) prepared by the synthesis step of increasing the p-benzyltoluene component is shown. 12 -MBT) and hydrogen-poor state (H0-MBT);

[0054] Fig.16 a to Fig.16 d shows the hydrogen storage and release results (a, c) of the selective isomer compositions (p72 and p55) prepared by the synthesis steps of increasing the content of monobenzylbenzene and the content of MLH-sim as comparative examples, and their Arrhenius plots (b, d) (hydrogenation conditions: 10 g reactant, hydrogen pressure 50 bar, M / R 0.035 mol%, 130° C. and 1200 rpm; dehydrogenation conditions: 1.5 g reactant, 1 bar, M / R 2.40 mol%, 260° C., 215 min and 200 rpm);

[0055] Fig.17 a and Fig.17 b is a GC analysis result diagram showing the dehydrogenation product of p-benzyltoluene (a: hydrogen-rich state (pH 12 -MBT); b: hydrogen-poor state (p-H0-MBT);

[0056] Fig.18 is a photograph showing the apparent color of p-benzyltoluene and a product obtained by dehydrogenation reaction using p-benzyltoluene as a reactant (reaction conditions: 10 g reactant, M / R of 2.40 mol%, 270° C., 215 min, 200 rpm);

[0057] Fig.19 is a graph of hydrogenation results depending on the concentration of methylfluorene (MF) in p-benzyltoluene (reaction conditions: 10 g of reactant, hydrogen pressure 50 bar, M / R 0.035 mol%, 130° C. and 1200 rpm);

[0058] Fig. 20 a and Fig. 20b is a graph showing the results of dehydrogenation of p-benzyltoluene in the presence of a Pt / Al2O3 catalyst and a Pt-S / Al2O3 catalyst, respectively, and GC analysis of the resulting product (reaction conditions: 10 g of reactant, 1 bar, M / R of 2.40 mol% (Pt / Al2O3 catalyst) and 0.15 mol% (Pt-S / Al2O3 catalyst), 270°C, 215 min and 200 rpm);

[0059] Fig.21 is a graph showing the results of stability evaluation of a selective isomer composition (p72) prepared by a synthesis step of increasing a para-benzyltoluene component (hydrogenation conditions: 10 g of reactant, hydrogen pressure 50 bar, M / R of 0.035 mol% for the first run, M / R of 0.14 mol% for subsequent runs, 130° C., 1200 rpm; dehydrogenation conditions: 10 g of reactant, 1 bar, M / R of 0.15 mol%, 270° C., 215 min, and 200 rpm);

[0060] Fig. 22 a and Fig. 22 b is a graph of hydrogen storage (hydrogenation) and hydrogen release (dehydrogenation) test results, depending on the type of reactants (hydrogenation conditions: 10 g reactants, hydrogen pressure 50 bar, M / R 0.035 mol%, 130° C. and 1200 rpm; dehydrogenation conditions: 1.5 g reactants, 1 bar, M / R 2.40 mol%, 260° C., 215 min and 200 rpm);

[0061] Fig.23 The gas chromatography analysis results of the products obtained by repeated hydrogen storage / release of p-benzyltoluene are shown (hydrogenation conditions: 10 g reactant, hydrogen pressure 50 bar, M / R of the first run is 0.035 mol%, M / R of the subsequent run is 0.14 mol%, temperature 130°C, reaction time of the first run is 44 minutes, and the subsequent run is 82 minutes, and the rotation speed is 1200 rpm; dehydrogenation conditions: 10 g reactant, 1 bar, M / R is 0.15 mol%, 270°C, 215 min and 200 rpm); and

[0062] Fig.24The gas chromatography analysis results of the products obtained by repeated hydrogen storage / release of the selective isomer composition (p72) prepared by the synthesis step of adding a para-benzyltoluene component are shown (hydrogenation conditions: 10 g of reactants, hydrogen pressure of 50 bar, M / R of 0.035 mol% for the first run, M / R of 0.14 mol% for the subsequent runs, temperature of 130°C, reaction time of 43 minutes for the first run, 40 minutes for the subsequent runs, and rotation speed of 1200 rpm; dehydrogenation conditions: 10 g of reactants, 1 bar, M / R of 0.15 mol%, 270°C, 215 min and 200 rpm).

[0063] Best Mode for Carrying Out the Invention

[0064] The present disclosure can be fully implemented according to the following description. It should be understood that the following description gives the preferred embodiments of the present disclosure, and the present disclosure is not necessarily limited thereto. In addition, the accompanying drawings are provided to help understand the present disclosure, and the present disclosure is not limited thereto.

[0065] The terms used herein are defined as follows.

[0066] The term "liquid organic hydrogen carrier (LOHC)" may refer to an organic fluid that can be hydrogenated in the presence of a catalyst for storage and transportation and then dehydrogenated in the presence of a catalyst.

[0067] The term "hydrogenation" may refer to a reaction that chemically adds hydrogen to at least a portion of a compound by contacting the compound with a catalyst under a supply of hydrogen gas, thereby increasing the hydrogen content of the compound.

[0068] The term "dehydrogenation" may refer to a reaction of removing hydrogen from a compound and further releasing the removed hydrogen from the compound.

[0069] The term "support" may refer to a material (eg, a solid material) having a high specific surface area to which a catalytically active component is attached.

[0070] The term "monobenzyltoluene" may refer to a compound in which the benzyl group is located in the ortho, meta and / or para position relative to the methyl group.

[0071] The term "monobenzyltoluene isomer mixture" is understood to include not only a binary mixture containing at least two combinations selected from positional isomers (ortho-isomer, meta-isomer and para-isomer) but also a ternary mixture containing three positional isomers.

[0072] The term "hydrogen-poor benzyltoluene" may refer to dehydrogenated benzyltoluene, represented by HO-MBT, while the term "hydrogen-rich benzyltoluene" may refer to fully hydrogenated benzyltoluene storing 12 hydrogen atoms, represented by H0-MBT. 12 -MBT means.

[0073] Here, when a numerical range is specified as a lower limit and / or an upper limit, it can be understood that any subcombination within the numerical range is also disclosed. For example, when described as "1 to 5", it includes not only 1, 2, 3, 4 and 5, but also any subcombination therebetween.

[0074] When any component or member is described herein as being “connected” to another component or member, it can be understood that it includes not only the case of being directly connected to another component or member but also the case of being connected to another component or member through the intervention of another component or member, unless otherwise specified.

[0075] Likewise, the term "contact" may be understood to include not only direct contact but also contact through the intervention of another component or member.

[0076] When any component is “comprising”, it means that another component may be further included unless otherwise specified.

[0077] In the present disclosure, the composition ratio is controlled by determining the tendency of each of the three positional isomers (ortho-isomer, meta-isomer and para-isomer) of monobenzyltoluene (MBT), one of the LOHCs, in reversible or repeated hydrogenation / dehydrogenation, thereby improving the reaction efficiency and suppressing the decrease in the efficiency of the overall hydrogen storage / release process caused by impurities and / or irreversible by-products, ultimately achieving a stable hydrogen storage / release efficiency.

[0078] Liquid organic hydrogen carrier (hydrogen storage material)

[0079] The present inventors have found that the hydrogenation (hydrogen storage) rate and dehydrogenation (hydrogen release) rate of the three positional isomers of monobenzyltoluene are different. In LOHC as a hydrogen storage means, high hydrogen storage / release efficiency is the most important factor. Based on the evaluation results of the hydrogen storage / release activity of the individual isomers, a composition-controlled monobenzyltoluene isomer mixture is provided, thereby improving the hydrogenation / dehydrogenation efficiency.

[0080] For the monobenzyltoluene isomer mixture, commercially available heat transfer oil, such as Marlotherm LH, is usually used. However, it is difficult to prepare an isomer mixture with a controllable ratio between multiple isomers using commercial products, and the method of separating and purifying specific isomers is also difficult to achieve physically and chemically.

[0081] In this regard, in one embodiment, in order to prepare a composition-controlled monobenzyltoluene isomer mixture, an ortho-, meta- or para-monobenzyltoluene isomer may be obtained by reacting a compound having an alkyl group attached to a specific position of a benzene ring in a methylbenzyl halide compound represented by the following general formula 1 (i.e., 2-methylbenzyl halide, 3-methylbenzyl halide or 4-methylbenzyl halide) (alkylation; Figure 1 ).

[0082] [General formula 1]

[0083]

[0084] Here, CH3 may be located in the ortho, meta or para position relative to CH2X, and X may be fluorine, chlorine, bromine or iodine, such as chlorine or bromine, such as chlorine (Cl).

[0085] In the above reaction, benzene to be reacted with methylbenzyl halide may be used in excess. The amount of benzene used relative to methylbenzyl halide may be adjusted in the range of, for example, about 1 to 25 mol, for example, about 2 to 20 mol, for example, 3 to 15 mol, for example, about 5 to 10 mol.

[0086] According to one embodiment, the reaction can be carried out in the presence of a homogeneous catalyst, which can be at least one selected from Fe(III) halides such as FeCl3, FeBr3, etc. For example, FeCl3 can be used. The amount of the catalyst is not particularly limited, but can be set in the range of, for example, about 0.001 to 0.8 mol, such as about 0.005 to 0.5 mol, such as about 0.01 to 0.2 mol relative to the methylbenzyl halide.

[0087] Optionally, a solvent may be selected to react, and the solvent may be selected from the type that does not react with the reactants and products. For example, the solvent may be at least one selected from the group consisting of aliphatic hydrocarbons (such as aliphatic hydrocarbons with 6 to 9 carbon atoms), halogenated hydrocarbons (such as methylene chloride, tetrachloroethane, etc.) and halogenated aromatic hydrocarbons (such as dichlorobenzene, trichlorobenzene, etc.).

[0088] In addition, the reaction can be carried out at a temperature of, for example, about 5 to 120° C., for example, about 10 to 100° C., for example, about 20 to 90° C., for example, about 30 to 80° C. The reaction pressure is not particularly limited, but can be adjusted in a range of, for example, about 0.5 to 2 atm, for example, about 0.8 to 1.5 atm. According to one embodiment, the reaction time can be adjusted in a range of, for example, about 0.5 to 5 hours, for example, about 1.5 to 3 hours, for example, about 2 to 2.5 hours, which can be understood as illustrative.

[0089] After the reaction is completed, the monobenzyltoluene isomer can be purified and recovered using currently known separation techniques (such as extraction, distillation, crystallization, etc.) alone or in combination.

[0090] According to one embodiment, since halogen (e.g., chlorine) is used in reactants and / or catalysts, halogen (or halogen compound) may be included in the monobenzyltoluene product, and an example of such halogen component may include hydrochloric acid. In the case of containing halogen components in monobenzyltoluene, hydrogenation efficiency and / or dehydrogenation efficiency may be reduced. Therefore, it is best to keep the halogen content in the monobenzyltoluene below a predetermined level. For example, the halogen content in the monobenzyltoluene can be maintained on an elemental basis, for example, below about 30ppm (w / w), for example, below about 20ppm (w / w), for example, about 10ppm (w / w). For this reason, at least one selected from sodium methoxide (NaOCH3), sodium carbonate (Na2CO3), sodium bicarbonate (NaHCO3), etc. can be used for dehalogenation (e.g., dechlorination) (purification step). For example, according to the measured halogen content, the amount of components used for dehalogenation can be set in the range of, for example, about 10 to 1000 molar equivalents, for example, about 50 to 500 molar equivalents, for example, about 100 to 200 molar equivalents, which can be understood as exemplary.

[0091] In addition, the reaction can be carried out at a temperature of, for example, about 100° C. or higher, for example, about 250 to 270° C., and the reaction time is not particularly limited, but can be adjusted in the range of, for example, about 3 to 25 hours, for example, about 5 to 20 hours, for example, about 10 to 15 hours, which can be understood as illustrative.

[0092] According to one embodiment, the monobenzyltoluene isomers can be prepared separately and mixed in a predetermined ratio to obtain a monobenzyltoluene isomer mixture of desired components. Therefore, the halogen content in the monobenzyltoluene isomer mixture can also be adjusted within the allowable halogen content range of a single isomer.

[0093] According to another embodiment, a combination of methylbenzyl halides (i.e., 2-methylbenzyl halide, 3-methylbenzyl halide, and 4-methylbenzyl halide) corresponding to the ratio between isomers of the monobenzyltoluene isomer mixture finally obtained can be used as a reactant and reacted with benzene to obtain an isomer mixture. Thereafter, the product can be purified to obtain a monobenzyltoluene isomer mixture in which the content of a single isomer is controlled.

[0094] Meanwhile, the above method prepares monobenzyltoluene or its isomer mixture by reacting methylbenzyl halide and benzene as reactants, but in another embodiment, monobenzyltoluene or its isomer mixture can be obtained by reacting benzyl halide (e.g., benzyl chloride) and toluene as reactants. The catalyst here can use a heterogeneous catalyst instead of a homogeneous catalyst, such as a porous catalyst, such as a solid acid catalyst, such as a zeolite catalyst. As a zeolite catalyst, a large-pore zeolite (e.g., 12-ring zeolite) can be used, for example, any one or a combination of two or more selected from zeolite β, ultra-stable zeolite Y (USY, ultra-stable zeolite Y), faujasite (FAU, faujasite), modasite, etc. can be used as a catalyst. Explanation: The silica-alumina molar ratio (SAR, silica-aluminamolar ratio) of this zeolite can be, for example, in the range of about 5 to 90, for example, about 10 to 80, for example, about 25 to 70. In addition, the zeolite catalyst can be subjected to a preliminary heat treatment at a temperature of, for example, about 200 to 600° C., for example, about 300 to 550° C., for example, about 400 to 500° C., for about 0.5 to 10 hours, for example, about 1 to 7 hours, for example, about 1.5 to 5 hours before the reaction. Thereafter, the reaction between the benzyl halide and toluene can be carried out at, for example, about 25 to 200° C. (for example, about 50 to 150° C., for example, about 80 to 120° C.) for about 0.5 to 10 hours (for example, about 1 to 6 hours, for example, about 2 to 4 hours). After the reaction is completed, the catalyst can be removed from the product by solid-liquid separation known in the art (for example, filtration, precipitation, membrane separation, centrifugation, adsorption, chromatography, ion exchange, etc.), and the above separation and purification techniques can be used to obtain high-purity monobenzyltoluene or a mixture of isomers thereof.

[0095] According to one embodiment of the present disclosure, among the three isomers of monobenzyltoluene, the ortho isomer has the slowest hydrogenation / dehydrogenation rate (e.g., hydrogenation rate), while the para isomer has the fastest reaction rate, and the components of the isomer mixture (composition) are controlled accordingly. In this regard, the order of activity for hydrogenation and dehydrogenation is para-MBT>meta-MBT>ortho-MBT. Therefore, considering the trends observed when using a single isomer, it can be expected that in order to maximize hydrogen storage / release efficiency, it is best to use para-monenzyltole as a LOHC alone rather than using an isomer mixture.

[0096] However, the present inventors have determined that when a single regioisomer is used for dehydrogenation, when the conversion rate is increased (e.g., about 90% or more, such as about 95% or more), in addition to the production of hydrogen-deficient monobenzyltoluene, a fused hydrocarbon ring between two benzene rings is further produced to form methylfluorene (MF) as represented by the following chemical formula 1.

[0097] [Chemical formula 1]

[0098]

[0099] In particular, methylfluorene exhibits irreversibility during the subsequent hydrogenation process, which reduces the reaction efficiency. During the dehydrogenation process, methylfluorene tends to be generated in the order of para-MBT>meta-MBT>ortho-MBT. Even when the para-benzyltoluene isomer is used alone, the dehydrogenation selectivity is reduced due to the increased formation of methylfluorene during the dehydrogenation process caused by repeated hydrogenation / dehydrogenation.

[0100] In view of the above, in the present embodiment, the components of the isomer mixture are mainly controlled so that the methylfluorene content in the dehydrogenated monobenzyltoluene (MBT) isomer mixture can be maintained at, for example, less than about 10 mol%, for example, less than about 7 mol%, for example, less than about 5 mol%, for example, less than about 3 mol%. In this regard, when the methylfluorene content in the monobenzyltoluene isomer mixture is greater than or equal to a predetermined level, the hydrogenation efficiency decreases with the repetition of the hydrogen storage / release cycle, which is undesirable in terms of stability. Therefore, during the hydrogen storage / release cycle, the methylfluorene content must be adjusted within the above range.

[0101] Although the present disclosure is not bound by any particular theory, it can be considered that hydrogen or intermediates (H6-MBT) adsorbed on the catalyst surface during the dehydrogenation process participate in the formation of methylfluorene, and as the reaction proceeds to a certain extent (such as about 90% or more, for example, about 95% or more), methylfluorene is inevitably formed.

[0102] Therefore, in this embodiment, instead of using a specific monobenzyltoluene isomer as LOHC alone, a monobenzyltoluene isomer mixture is used, wherein the content of para-monobenzyltoluene in the isomer mixture is adjusted, thereby improving hydrogenation / dehydrogenation efficiency and suppressing the stability deterioration caused by methylfluorene. It is worth noting that these complex effects are not taken into account in the conventional technology. In this embodiment, the isomer mixture substantially contains para-monobenzyltoluene, but can also be formulated to contain at least one of the remaining two isomers. Here, the content of para-monobenzyltoluene in the isomer mixture can reach, for example, at least about 50mol%, for example, at least about 55mol%, for example, at least about 60mol%. However, when the proportion of para-monobenzyltoluene increases too much, close to the use of pure isomers, as mentioned above, the formation of irreversible methylfluorene will also increase, so setting an appropriate upper limit may be advantageous.

[0103] In one embodiment, when p-benzyltoluene is mixed with one or two different regioisomers in appropriate ratios, a balancing effect can be provided, namely, appropriate suppression of methylfluorene formation while maintaining the good reaction efficiency expected when p-benzyltoluene is used alone.

[0104] For example, the content of ortho-benzyltoluene (o-MBT) in the monobenzyltoluene isomer mixture can be adjusted in the range of, for example, about 42 mol% or less, for example, about 7 to 38 mol%, for example, about 12 to 30 mol%, for example, about 16 to 25 mol%. In addition, the content of meta-benzyltoluene (m-MBT) can be adjusted in the range of, for example, about 15 mol% or less, for example, about 1 to 12 mol%, for example, about 3 to 10 mol%, for example, about 5 to 9 mol%. In addition, the content of para-benzyltoluene (p-MBT) can be adjusted in the range of, for example, about 55 to 90 mol%, for example, about 60 to 85 mol%, for example, about 65 to 80 mol%, for example, about 70 to 75 mol%.

[0105] According to one embodiment, the boiling point (1atm) of the monobenzyltoluene isomer mixture as LOHC may be, for example, in the range of about 250 to 300°C (e.g., about 260 to 290°C, e.g., about 265 to 285°C), and the melting point may be, for example, in the range of about 10°C or below (e.g., about -28 to 8°C, e.g., about -10 to 5°C).

[0106] In addition, in one embodiment, the viscosity (20°C) of the monobenzyltoluene isomer mixture may be in the range of about 3 to 8 cP (e.g., about 3.5 to 7.5 cP, e.g., about 3.8 to 6.9 cP), and the density (20°C) may be about 0.94 to 1.02 g / cm 3 (e.g. about 0.96 to 1.00 g / cm 3 , for example, about 0.97 to 0.99 g / cm 3 ).

[0107] Catalysts for hydrogen storage

[0108] According to one embodiment, the hydrogen storage reaction of the LOHC may be performed in the presence of a catalyst, ie, a hydrogenation catalyst (eg, a heterogeneous catalyst).

[0109] The basic components of the hydrogenation catalyst are known in the art, and may be in the form of a hydrogenation metal supported on a support comprising a porous inorganic oxide. For example, the porous inorganic oxide may be at least one selected from the group consisting of alumina, silica, silica-alumina, aluminum phosphate, zirconium oxide, titanium dioxide, cerium and yttrium, such as alumina.

[0110] According to one embodiment, the active metal used for hydrogenation can be at least one selected from, for example, metals of Group IB, Group VIB, and Group VIII in the periodic table. For example, the active metal can be at least one selected from the group consisting of nickel, cobalt, palladium, platinum, iridium, ruthenium, rhodium, copper, gold, rhenium, zinc, molybdenum, tin, manganese, tungsten, and germanium. According to a certain embodiment, at least one selected from palladium, platinum, iridium, ruthenium, rhodium, etc., such as platinum, palladium and / or ruthenium can be used as the active metal, and in one embodiment, ruthenium can be used.

[0111] In this regard, the content of the active metal supported on the hydrogenation catalyst can be determined in the range of, for example, about 0.1 to 50 wt%, such as about 0.5 to 30 wt%, such as about 1 to 20 wt%. Therefore, in order to support the active metal, any method known in the art, such as impregnation (such as initial wet impregnation, excess water impregnation and soaking), ion exchange, coprecipitation, solid-state reaction, hydrothermal technology, sol-gel reaction, deposition-precipitation, etc., can be used, and for example, impregnation or solid-state reaction, such as solid-state reaction, can be performed, but the present disclosure is not limited thereto.

[0112] According to one embodiment, a solid-state reaction can be used when preparing the hydrogenation catalyst, and the active metal can be uniformly distributed on the support in a simple manner, that is, an active metal precursor and an inorganic oxide precursor are reacted in a single step by adding an alkali component without using a solvent, and then heat-treated (for example, heat-treated in an oxygen-containing atmosphere).

[0113] In this respect, the active metal precursor can be in the form of a salt. For example, the nickel precursor can be at least one selected from nickel nitrate, nickel sulfate, nickel phosphate, nickel halide, nickel carboxylate, nickel hydroxide, nickel carbonate, acetylacetonate nickel complex, nickel acetate and its hydrate. The cobalt precursor can be at least one selected from the group consisting of nitrate, sulfate, carbonate, acetate, alkoxide and halide of cobalt. In addition, the palladium precursor can be at least one selected from palladium acetate, palladium chloride, palladium nitrate, palladium sulfate, etc. In addition, the platinum precursor can be at least one selected from chloroplatinic acid, ammonium chloroplatinate, dinitrodiaminoplatinum (dinitrodiaminoplatinum), tetrachlorodiaminoplatinum (tetrachlorodiaminoplatinum), hexachlorodiaminoplatinum (hexachlorodiaminoplatinum), dichlorodiaminoplatinum (dichlorodiaminoplatinum), dichloroplatinum (II), tetrachloroplatinum (IV), etc. The ruthenium precursor can be at least one selected from ruthenium chloride, nitroso ruthenium nitrate, chlorohexaaminoruthenium (chlorohexaaminoruthenium), etc. In addition, the rhenium precursor can be at least one selected from perrhenic acid, rhenium chloride, ammonium perrhenate, potassium perrhenate, rhenium oxide, etc., and the iridium precursor can be at least one selected from iridium nitrate, iridium chloride, iridium sulfate, iridium acetate, iridium acetylacetonate, iridium cyanate, iridium isopropoxide, iridium butoxide, etc.

[0114] According to one embodiment, the precursor of the porous inorganic oxide can be an organic or inorganic acid salt of aluminum, silicon, titanium, zirconium, etc., an alkoxide thereof, a complex thereof, or a combination thereof. For example, the precursor of aluminum oxide can be selected from at least one of aluminum acetate, aluminum acetylacetonate, aluminum tert-butoxide, aluminum sec-butoxide, aluminum pentoxide, aluminum ethoxide, aluminum isopropoxide, aluminum butoxide, aluminum chloride, aluminum bromide, aluminum iodide, aluminum sulfate, aluminum nitrate, and a hydrate thereof. In addition, the precursor of titanium dioxide can be selected from at least one of titanium chloride (IV), titanium bromide (IV), titanium butoxide (IV), titanium tert-butoxide (IV), titanium ethoxide (IV), titanium isopropoxide (IV), bis (ethyl acetoacetate) diisopropoxide titanium (IV), etc. The precursor of zirconium oxide can be selected from at least one of zirconium acetate, zirconium acetate hydroxide (IV), zirconium tert-butoxide (IV), zirconium hexoside (IV), zirconium ethoxide (IV), zirconium iodide (IV), etc. In addition, tetraethyl orthosilicate or the like can also be used as a silicon dioxide precursor.

[0115] According to one embodiment, the alkali component may be at least one selected from ammonium carbonate, ammonium bicarbonate, ammonium chloride, ammonium oxalate, ammonium sulfate, ammonium hydroxide, ammonium nitrate, lithium hydroxide, sodium hydroxide, potassium hydroxide, calcium hydroxide and magnesium hydroxide. For example, ammonium bicarbonate may be used.

[0116] According to one embodiment, the molar ratio of the active metal precursor / base component in the precursor mixture can be, for example, in the range of about 0.001 to 0.1, for example, about 0.002 to 0.05, for example, about 0.008 to 0.02, but can vary according to the type of the precursor and the base. In addition, the mixing ratio of the active metal precursor and the inorganic oxide precursor in the precursor mixture can be determined according to the carrier and metal content required in the catalyst. After the precursor mixture is prepared or its physical mixture is formed, the solid-state reaction can be carried out by applying external energy. The external energy applied for the solid-state reaction between the above three components can generally be physical or mechanical energy, such as friction energy generated by grinding, grinding or crushing, such as friction energy generated by ball milling. In addition, the time for the solid-state reaction under the action of external energy can be, for example, about 5 to 40 minutes, such as about 10 to 30 minutes, such as about 13 to 25 minutes, which can be understood as exemplary, and the reaction time can vary according to the scale of the reaction, etc.

[0117] As the solid-state reaction between the precursors proceeds, the hardness is increased by solidification, and then a gel is formed again, and a gel-type catalytic solid can be finally obtained. Next, the catalytic solid formed by the solid-state reaction can be heat-treated in an oxygen-containing environment (e.g., an air environment), i.e., fired (or calcined), to convert the gel-type catalytic solid into an oxide. Here, the heat treatment can be carried out at a temperature of, for example, about 300 to 800 ° C, such as about 400 to 750 ° C, such as about 500 to 700 ° C. By this heat treatment, the active metal can be evenly distributed in the pores of the inorganic oxide support. At the same time, the hydrogenation catalyst manufactured by heat treatment can also be reduced before hydrogen storage (hydrogenation) to activate the catalyst. Therefore, hydrogen, carbon monoxide, methane or a combination thereof can be used as a reducing gas. For example, reduction can be carried out under a hydrogen environment. As an example, the reduction temperature can be, for example, in the range of about 300 to 600 ° C (e.g., about 350 to 550 ° C, such as about 400 to 500 ° C), and the reduction time can be, for example, in the range of about 1 to 10 hours, such as about 2 to 5 hours. Determine. In addition, the pressure during the reduction process (partial pressure of the reducing gas) is not particularly limited, but can be, for example, in the range of about 1 to 5 bar, such as about 1.5 to 4 bar, such as about 2 to 3 bar. The above reduction conditions are to be understood as exemplary and are not necessarily limited thereto.

[0118] As described above, the BET specific surface area of ​​the support in the hydrogenation catalyst produced by the solid-state reaction may be, for example, at least about 200 m 2 / g, for example at least about 300m 2 / g, for example, about 320 to 500 m 2 In a particular embodiment, the BET specific surface area can be as high as about 350 to 480 m 2 / g, for example, about 370 to 450 m 2 / g, for example, about 380 to 400 m 2 / g. This specific surface area is much higher than the specific surface area of ​​the inorganic oxide support in the catalyst prepared by a typical catalyst preparation method (such as an impregnation method). In addition, in one embodiment, the pore volume of the support in the catalyst can be, for example, about 0.3 to 2 cm 3 / g, for example, about 0.4 to 1.5 cm 3 / g, for example, about 0.6 to 1 cm 3 / g. In addition, the average pore size (diameter) of the support in the catalyst can be, for example, in the range of about 3 to 4.5 nm, such as about 3.5 to 4.3 nm, such as about 3.8 to 4.1 nm. In addition, the size of the active metal in the hydrogenation catalyst can be in the range of about 5 nm or less, such as in the range of about 3 nm or less, such as in the range of about 0.1 to 2 nm, and the active metal can be supported in the form of single atoms and / or clusters.

[0119] According to one embodiment, the catalyst can be made into a cylindrical, granular, pellet, flake, spherical, etc. For this purpose, molding, extrusion, spray drying, granulation, etc. methods known in the art can be used, and these methods can be understood as illustrative. In addition, the size (or diameter) of the catalyst manufactured in the form of a molded product can be, for example, in the range of about 0.1 to 10 mm, such as about 0.5 to 5 mm, such as about 1 to 3 mm, which can be understood as illustrative.

[0120] Although the above mainly describes a method for manufacturing a hydrogenation catalyst by a solid-state reaction, the present disclosure is not limited thereto, and as long as a benzyltoluene isomer mixture is used as the LOHC, it can be understood that a hydrogenation catalyst manufactured based on a typical support method such as impregnation is also applicable. In this regard, the concentration of the active metal in the impregnation solution (wherein at least one selected from the group consisting of water, ethanol, acetone, tetrahydrofuran and hexane can be used as a solvent) can be, for example, about 0.6 to 9.1 M, such as about 1.1 to 6.6 M, such as about 3.4 to 5.8 M. The conditions for the impregnation are not particularly limited, but the impregnation can be carried out under conditions such as about 5 to 35° C. (e.g., about 20 to 25° C.) and about 6 to 24 hours (e.g., about 10 to 15 hours). These conditions can be understood as exemplary conditions.

[0121] As described above, the active metal can be supported on a support (e.g., a porous support containing an inorganic oxide, such as a support containing alumina, such as a γ-alumina support) by impregnation and then dried. For example, drying can be carried out under an oxygen-containing atmosphere (e.g., air), and the drying temperature can be, for example, in the range of about 40 to 150° C., such as about 90 to 110° C. In addition, the drying time can be determined in the range of, for example, about 4 to 24 hours, such as about 6 to 10 hours. Thereafter, the dried catalyst can be heat-treated under the temperature conditions adopted in the above-mentioned solid-state reaction. Here, the heat treatment can be carried out under a hydrogen-containing atmosphere (e.g., hydrogen).

[0122] At the same time, compared with the catalyst prepared by solid phase reaction, the porosity of the catalyst prepared by impregnation method is lower, and its specific surface area (BET) is about 150 to 400 m 2 / g, for example, about 200 to 350 m 2 / g, for example, about 250 to 300 m 2 / g, which is lower than the specific surface area of ​​the catalyst prepared by solid phase reaction (e.g., about 90% or less, e.g., about 80% or less, e.g., about 70% or less). In addition, the pore volume of the catalyst prepared by impregnation method can be, for example, about 0.4 to 1 cm 3 / g, for example, about 0.45 to 0.8 cm 3 / g, for example, about 0.5 to 0.7 cm 3 / g. In addition, the average pore size (diameter) thereof may be in the range of, for example, about 3 to 20 nm, for example, about 5 to 12 nm, for example, about 6 to 10 nm.

[0123] Meanwhile, the size of the active metal in the hydrogenation catalyst manufactured by the impregnation method may be in the range of about 0.4 to 10 nm, such as about 1 to 5 nm, such as about 2 to 4 nm, and thus the size of the supported active metal is larger than that of the catalyst manufactured by the solid-state reaction.

[0124] Furthermore, the catalyst produced by the impregnation method may be reduced before hydrogenation, and the reduction conditions may be set within the above range.

[0125] Dehydrogenation catalyst

[0126] In one embodiment of the present disclosure, the dehydrogenation of LOHC to release hydrogen can be carried out in the presence of a catalyst, which can be the same type as the above-mentioned hydrogenation catalyst or a different type than the above-mentioned hydrogenation catalyst. Alternatively, one of the hydrogenation catalyst and the dehydrogenation catalyst can be made by impregnation, while the other can be made by solid-state reaction, or vice versa.

[0127] Therefore, as described above, it is desirable to suppress the formation of methylfluorene during the dehydrogenation of monobenzyltoluene and maintain the methylfluorene content in LOHC below a predetermined level during repeated hydrogen storage / release cycles, and to perform dehydrogenation using a catalyst having controllable characteristics.

[0128] According to one embodiment, sulfur components can be added to the catalyst to control the catalytic properties, and thus sulfurization can be performed. Here, the dehydrogenation catalyst may include a support containing a porous inorganic oxide, an active metal and sulfur. In the dehydrogenation catalyst, the porous inorganic oxide can be at least one of the types selected from the hydrogenation catalyst, and the active metal can also be as described above. In the dehydrogenation catalyst of a specific embodiment, the porous inorganic oxide support can be aluminum oxide, the active metal can be platinum, and sulfur can be mixed into the catalyst by sulfurization.

[0129] In addition, the content of active metal in the dehydrogenation catalyst can be determined, for example, in the range of about 0.1 to 10 wt%, such as about 0.2 to 5 wt%, such as about 0.5 to 3 wt%. The sulfur content in the catalyst can be determined, for example, in the range of about 0.001 to 2 wt%, such as about 0.002 to 1 wt%, such as about 0.01 to 0.5 wt%.

[0130] In this regard, sulfidation can be carried out by any method known in the art, such as a gaseous method (contacting with hydrogen sulfide or its inert gas mixture) or a liquid method (contacting with a sulfur-containing compound solution). According to a specific embodiment, the thermally treated and / or reduced catalyst can be treated with a sulfur-containing compound solution.

[0131] According to one embodiment, the sulfur compound available in the sulfurization process may be at least one of hydrogen sulfide, hydrogen disulfide, carbon disulfide, alkyl sulfide, etc. Examples of alkyl sulfides may include methyl sulfide, dimethyl sulfide, dimethyl disulfide, diethyl sulfide, and / or dibutyl sulfide. In one embodiment, the sulfurization may be performed at a temperature of room temperature to about 500° C. (e.g., about 100 to 450° C.) for about 0.5 to 100 hours (e.g., about 1 to 48 hours).

[0132] According to one embodiment, the molar ratio of sulfur / active metal in the dehydrogenation catalyst may be, for example, in the range of about 0.1 to 1, for example, about 0.2 to 0.8, for example, about 0.3 to 0.5. If the sulfur content is too high compared to the active metal, the active sites of the metal may be blocked due to the adsorption of sulfur, resulting in excessive reduction in reaction activity; and if the sulfur content is too low, the effect of controlling the catalyst characteristics may be relatively low, so the inhibition of the formation of methylfluorene may be limited. Therefore, the molar ratio thereof may be advantageously adjusted within the above range, but may also vary depending on the type of active metal and support, the amount of active metal and the particle size. In addition, the degree of sulfidation may be adjusted in the range of, for example, about 10% to 70%, for example, about 20% to 60%, for example, about 30% to 50%.

[0133] In an alternative embodiment, when the dehydrogenation catalyst is manufactured by solid phase reaction, an effect equivalent to sulfidation can be obtained by adding a sulfur compound (e.g., at least one selected from ammonium sulfate, hydroxylamine sulfate, aluminum sulfate, dimethyl sulfate, diethyl sulfate, tetramethylammonium sulfate, tetrabutylammonium sulfate, dodecylammonium sulfate, etc.) together with the active metal precursor, the inorganic oxide precursor and the base component in the precursor mixture to carry out solid phase reaction, and the amount of the sulfur compound can be determined within the range related to sulfidation.

[0134] In a dehydrogenation catalyst having characteristics controlled in this way, the formation of methylfluorene can be more effectively suppressed by weakening the adsorption strength of the dehydrogenation product and preventing additional reactions from occurring after H0-MBT.

[0135] Hydrogenation / dehydrogenation of a mixture of monobenzyltoluene isomers

[0136] According to one embodiment of the present disclosure, the above-mentioned monobenzyltoluene isomer mixture can be used as a liquid organic hydrogen carrier (LOHC) for hydrogenation / dehydrogenation. Therefore, monobenzyltoluene can store or release hydrogen in a liquid phase or a gas phase in an alternating manner of a hydrogen-rich state and a hydrogen-poor state. In particular, by processing hydrogen in the form of a liquid organic hydrogen carrier, existing fuel facilities can be utilized, and high-purity hydrogen can be produced compared to storing hydrogen by hydrogenating a gas (such as carbon dioxide or nitrogen).

[0137] According to a method of storing and releasing hydrogen in accordance with one embodiment, a benzyltoluene isomer mixture (e.g., liquid) may be contacted with a hydrogenation catalyst or a dehydrogenation catalyst as a liquid organic hydrogen carrier in a reaction system. In one embodiment, the ratio of active metals (M / R) in the catalyst / LOHC may be distinguished between hydrogenation and dehydrogenation, for example, in hydrogenation, the ratio of M / R may be set relatively low, while in dehydrogenation, the ratio of M / R may be set relatively high. In this regard, if the ratio of M / R is too low, insufficient reaction activity may result because the lack of active sites of the active metal will limit the reaction. On the other hand, if the ratio of M / R is too high, the volume of the solid catalyst may be significantly increased compared to the liquid reactant, forming an excessive slurry state, which not only makes it difficult to stir during the reaction, but also causes diffusion restrictions, resulting in the inability to fully utilize the active sites of the catalyst. Therefore, it may be advantageous to appropriately adjust the ratio of M / R within the above range.

[0138] In one embodiment, the M / R ratio in hydrogenation (hydrogen storage) can be, for example, about 0.01 to 0.4 mol% (e.g., about 0.02 to 0.2 mol%, such as about 0.03 to 0.15 mol%, such as about 0.035 to 0.1 mol%), while the M / R ratio in dehydrogenation (hydrogen release) can be adjusted in the range of, for example, about 0.3 to 3 mol% (e.g., about 0.4 to 2.5 mol%, such as about 0.5 to 2 mol%, such as about 0.55 to 1 mol%).

[0139] According to one embodiment, the hydrogenation temperature may be, for example, in the range of about 50 to 200° C., for example, about 70 to 180° C., for example, about 80 to 150° C. Meanwhile, the hydrogenation pressure may be, for example, in the range of about 5 to 100 bar, for example, about 20 to 80 bar, for example, about 30 to 70 bar, for example, about 40 to 60 bar. In addition, the hydrogenation time is not particularly limited, but may be, for example, in the range of about 0.5 to 24 hours, for example, about 1 to 12 hours, for example, 1.5 to 6 hours.

[0140] According to one embodiment, the hydrogenation efficiency (defined as the number of moles of hydrogen actually stored by hydrogenation relative to the number of moles of hydrogen theoretically storable per mole of dehydrogenation reactant) can be, for example, at least about 90%, such as at least about 95%, such as at least about 99%. Therefore, the selectivity of the hydrogenation product corresponding to the hydrogen storage compound can be at least about 90%, such as at least about 95%, such as at least about 99%.

[0141] On the other hand, a dehydrogenation reaction can be performed to release hydrogen from a hydrogen storage material (liquid organic hydrogen carrier). The dehydrogenation reaction is an endothermic reaction and can be performed at a higher reaction temperature (e.g., about 50 to 150°C, e.g., about 60 to 120°C, e.g., about 80 to 100°C) than the hydrogenation (exothermic) of the same hydrogen storage material. According to one embodiment, the dehydrogenation temperature may be, for example, about 100 to 300°C, for example, about 150 to 290°C, for example, in the range of about 180 to 280°C. In addition, unlike the reaction temperature, the dehydrogenation pressure may be, for example, about 0.1 to 10 bar, for example, about 0.5 to 5 bar, such as atmospheric pressure, which is lower than the pressure conditions of hydrogenation. In addition, the dehydrogenation time is not particularly limited and can be set, for example, in the range of about 0.5 to 24 hours, for example, about 2 to 12 hours, for example, about 3 to 8 hours.

[0142] According to one embodiment, the dehydrogenation efficiency (defined as the number of moles of hydrogen actually produced by dehydrogenation relative to the number of moles of hydrogen theoretically released from 1 mole of hydrogenation reactant) can be, for example, at least about 50%, such as at least about 60%, such as at least about 70%, such as at least about 80%, and in a certain embodiment, the dehydrogenation efficiency can be as high as, for example, at least about 90%, such as at least about 95%. Therefore, the selectivity of the dehydrogenation product corresponding to the hydrogen storage compound can be, for example, at least about 40%, such as at least about 70%, such as at least about 80%.

[0143] Meanwhile, according to one embodiment, hydrogenation / dehydrogenation can be carried out using a reactor known in the art, such as a batch reactor, a continuous reactor, a semi-continuous reactor, etc., and the reactor can be equipped with an agitator, because hydrogenation and dehydrogenation can be carried out in a liquid phase. According to one embodiment, the reaction can be carried out in a fixed bed reactor using a granular catalyst.

[0144] Mode for carrying out the invention

[0145] The present disclosure may be more clearly understood through the following examples, which are merely used to illustrate the present disclosure and are not to be construed as limiting the scope of the present disclosure. Example

[0146] In the examples and comparative examples, the prepared catalysts were analyzed according to the following analytical methods.

[0147] - Gas chromatography-flame ionization detector (GC-FID) analysis

[0148] The sample recovered after the reaction was filtered with a 0.1 μm syringe filter, and then 1 g of the corresponding material was dissolved in 10 ml of acetone and 100 μl of nonane to prepare a sample for GC-FID analysis. GC-FID analysis was performed on a RT-PCR system connected to a Restek The HPLC-MS analysis was performed on an Agilent Technologies 7890A with a -17Sil MS column (30 m x 0.25 mm x 0.25 μm). For GC-FID analysis, inlet temperature = 300°C, detector temperature = 300°C, flow rate = 0.2 cm 3 / min, split ratio = 1:300, and the oven program was set as 50°C → heating at 50°C / min → maintaining at 140°C for 80 minutes → heating at 50°C / min → maintaining at 250°C.

[0149] - 1 H NMR and 13 C NMR analysis

[0150] NMR analysis was performed using a Bruker DPX-300. All NMR spectra were obtained in CDCl3 and referenced to tetramethylsilane.

[0151] -Adsorption energy analysis based on density functional theory (DFT)

[0152] DFT calculations were performed using the Vienna ab initio simulation package (VASP). The generalized gradient approximation of Perdew-Burke-Ernzerhof was used for the exchange correlation function. In addition, projected augmented waves and regular waveset analogy valence wave functions were used. The cut-off energy for all DFT calculations was set to 500 eV. All geometry optimizations were performed using the conjugate gradient algorithm until the forces acting on each atom converged to The electron work function was determined according to the Methfessel-Paxton method with an energy distribution of 0.2 eV. In order to consider the dispersion effect, the semi-empirical DFT-D3 method was used. For the Pt slab model and the Ru slab model, the Monkhorst-Pack Brillouin zone sampling was 3x 3x 1 (9x 9x 9); for the γ-Al2O3 slab model, the Monkhorst-Pack Brillouin zone sampling was 2x 2x 1 (6x 4x 4). At the same time, the slab models of Pt (111) (5x 4) supercell 3 layers (2 layers relaxed), Ru (0001) (6x 4) supercell 3 layers (2 layers relaxed) and γ-Al2O3 (110) (2x 2) 4 layers (1 layer relaxed) were used respectively.

[0153] Chlorine concentration analysis

[0154] The synthetic material was tested according to KS M 2457:2003 (method for determining the chlorine content of light and heavy fractions by oxidation microcoulometry). The chlorine content was analyzed as follows using the TS / TX analyzer (ECS3000) of Thermo Fisher Scientific according to ASTM D5808 by oxidation microcoulometry. Oxygen and inert gas were continuously injected into the combustion tube to cause the sample to burn, and the resulting combustion products were transferred to the titration cell to react with the silver ions and hydrochloric acid produced by electrolysis. Afterwards, the silver ions consumed by the titration reaction were replaced by coulometric method, and the total current required to replace the silver ions was a measure of chlorine.

[0155] Boiling point, melting point and viscosity analysis

[0156] The boiling point is measured as follows: 1 ml of liquid sample is added to a test tube, and then a melting point capillary is dripped into the test tube with the open end facing down. The test tube is attached to a thermometer with a rubber band and then placed in a TL tube filled with thermal medium oil. Next, the TL tube is heated with a Bunsen burner, and the temperature is increased until bubbles are continuously generated in the capillary. After turning off the Bunsen burner, the speed of gas bubbling slows down and stops. The boiling point is recorded as the temperature when the matrix begins to enter the capillary. Each material is measured three times and the average value is taken.

[0157] Melting points were determined using data stored in Aspen+ software.

[0158] Viscosity was measured using a DV-II+Pro viscometer from Brookfield Engineering Laboratories. For analysis, 6 ml of liquid sample was placed on the sample cup and the shear rate was increased from 100 s -1 Change to 200s-1 The measurements were taken at each temperature for 2 minutes.

[0159] -Thermogravimetric analysis

[0160] For thermogravimetric analysis, each of the three monobenzyltoluene isomers (5 ml) and γ-Al2O3 or Ru / Al2O3 catalyst (500 mg) were stirred at room temperature for 24 hours and then vacuum dried at 80°C for 12 hours to prepare a sample adsorbing monobenzyltoluene. The prepared sample was subjected to thermogravimetric analysis using SDT Q600 of TA Instruments. 5 mg of the sample adsorbing monobenzyltoluene was placed on an alumina pan, heated from 35°C to 600°C at a heating rate of 5°C / min under a nitrogen flow (100 sccm), and then subjected to thermogravimetric analysis.

[0161] Example

[0162] Preparation of hydrogenation catalyst (Ru / Al2O3)

[0163] Al2O3 was added to Ru3(CO) dissolved in tetrahydrofuran (purity: 99.5%; Daejung Chemicals & Metals, Korea) 12 (purity: 99%, Sigma-Aldrich) solution, stirred at 25°C for 13 hours. Then, the solvent was removed under reduced pressure at 45°C, and then dried in an oven at 105°C for 8 hours. Finally, the recovered sample was heat-treated at 500°C for 6 hours under a hydrogen flow (100 sccm) to obtain a hydrogenation catalyst (Ru / Al2O3).

[0164] Preparation of dehydrogenation catalyst (Pt-S / Al2O3) Aluminum nitrate hydrate (purity: 98.0%; Junsei Co., Ltd.), ammonium bicarbonate (purity: 97.0%; Korea Ooi Chemical Co., Ltd.), ammonium sulfate (purity: 99.0%; Sigma-Aldrich Trading Co., Ltd.) and [Pt(NH3)4](NO3)2 (purity: 99.0%; Alfa Aesar Chemical Co., Ltd.) were crushed (or ground) with a mortar and pestle for 20 minutes to prepare a gel-type catalytic solid. Then, the gel-type catalytic solid was calcined at 600°C for 5 hours in an oxygen-containing environment (e.g., an air environment). Finally, the recovered sample was heat-treated at 500°C for 3 hours under a hydrogen flow (100 sccm) to prepare a dehydrogenation catalyst (Pt-S / Al2O3).

[0165] Synthesis of a Single Isomer of Benzyltoluene

[0166] refer to Figure 1 Three monobenzyltoluene isomers (o-MBT, m-MBT and p-MBT) were synthesized from 2-methylbenzyl chloride, 3-methylbenzyl chloride and 4-methylbenzyl chloride and excess benzene in the presence of a homogeneous catalyst.

[0167] Specifically, 2-methylbenzyl halide, 3-methylbenzyl halide and 4-methylbenzyl halide (purity: >98.0%; TCI) were prepared and added to a stirrer together with 20 molar equivalents of benzene (purity: 99.5%; Duksan Chemical) and 0.01 molar equivalents of FeCl3 (purity: 99.5%; Alfa Aesar Chemical Co., Ltd.). The added mixture was stirred at room temperature (800 rpm) for 2 hours. After the reaction was completed, distilled water was added and stirred at a speed of 1000 rpm for 10 minutes to deactivate the catalyst. Then, ethyl acetate (purity: 99.0%; Samchun Chemicals) was added, extracted, and the aqueous layer and the organic layer were separated to obtain only the organic layer. In addition, excess brine and excess MgSO4 (purity: 99.5%; Samchun Chemical Co., Ltd.) were added and extracted with ethyl acetate to remove as much water as possible. Finally, the recovered organic product is purified by vacuum distillation to recover o-MBT, m-MBT and p-MBT. Thus, the yield is about 40% to 48% of the theoretical yield.

[0168] When removing trace amounts of chlorine contained in each of the three MBT isomers as products, 200 molar equivalents of sodium methoxide (purity: 95%; Sigma-Aldrich Trading Co., Ltd.) were added for purification treatment according to the measured chlorine content. The added mixture was heated to 270° C. under stirring (750 rpm) while nitrogen was supplied at a rate of 0.03 L / min for 12 hours and then cooled. Then, distillation was carried out under reduced pressure (vacuum) conditions of 0.85 bar to recover materials with a boiling point in the range of 250 to 260° C., thereby obtaining three monobenzyltoluene isomers free of chlorine.

[0169] Preparation of a mixture of monobenzyltoluene isomers

[0170] The H0-MBT-p55 isomer mixture (ortho:meta:para=36:9:55) and the H0-MBT-p72 isomer mixture with increased p-MBT content (ortho:meta:para=19:9:72) were prepared according to the following steps.

[0171] Toluene (purity: 99.8%; Sanzen Chemical Co., Ltd.) and benzyl chloride (purity: 99.0%; Sanzen Chemical Co., Ltd.) were prepared as reactants. In addition, beta zeolite (Zeolyst Co.) and USY zeolite (Zeolyst Co.) were prepared as catalysts, and then heat-treated at 450° C. for 2 hours.

[0172] First, toluene and a catalyst are added to a reactor and heated to a set reaction temperature. Then, an appropriate amount of benzyl chloride is added according to the amount of toluene, and the mixture is stirred (1000 rpm) at 110°C for 3 hours for reaction. After the reaction is completed, the solid catalyst is separated from the mixture and then distilled to obtain high-purity monobenzyltoluene.

[0173] In addition, as a comparative example, an MBT isomer mixture (MLH-sim) was prepared by physically mixing the three single isomers so that it corresponded to the composition of Marlotherm LH commercially available from Sasol (ortho: meta: para = 46:5:49).

[0174] Analyze the results

[0175] Characterization of the Single Isomer of Monobenzyltoluene

[0176] Figure 2 It shows that in the case of hydrogen-rich (H 12 Figure 1 shows the GC analysis results of three monomer isomers (o-MBT, m-MBT and p-MBT) of monobenzyltoluene in the hydrogen-poor (H0-MBT) and hydrogen-poor (H0-MBT) states, as well as an isomer mixture corresponding to the commercially available Marlotherm LH (comparative example). As can be seen from the figure, the hydrogen-poor state seems to have one peak for each isomer, while the hydrogen-rich state seems to have two peaks for each isomer. These peaks correspond to the peaks of commercial Marlotherm LH, especially the peaks of the hydrogen-rich orthorhombic isomer and meta-isomer are detected in almost the same area and seem to overlap.

[0177] The three single isomers of para-benzyltoluene (o-MBT, m-MBT and p-MBT) were 1 H NMR (left) and 13 C NMR (right), the analysis results are as follows Figure 3 a to Figure 3 c. In which, in a single isomer of monobenzyltoluene, methyl groups as substituents are respectively present at the ortho position, meta position and para position, which confirms that each material is an isomer of monobenzyltoluene.

[0178] Analysis of the influence of chlorine on the single isomer of -monobenzyltoluene

[0179] The results of hydrogenation and dehydrogenation of the three single isomers of monobenzyltoluene (o-MBT, m-MBT and p-MBT) depend on the concentration of Cl, as shown in Tables 1 and Figure 4 , Figure 5 .

[0180] Table 1

[0181]

[0182] a : GC analysis and calculation results.

[0183] b :Hydrogen release efficiency = (full dehydrogenation product [mol] x 6H2 + single ring dehydrogenation product [mol] x 3H2) / (reactant [mol] x 6H2) x 100%

[0184] Referring to the table and the attached figure, as the Cl concentration in each isomer decreases, the time required to complete the hydrogenation (t full ) also decreased, which confirmed the increase in reaction activity. In addition, similar to hydrogenation, in the dehydrogenation process, the release efficiency of hydrogen (H2) also increased with the decrease in Cl concentration. Therefore, the activity of both hydrogenation and dehydrogenation increased until the residual Cl concentration in monobenzyltoluene decreased to below 10 ppm.

[0185] The boiling points, melting points and viscosities of the three single isomers (o-MBT, m-MBT and p-MBT) of the dechlorinated purified monobenzyltoluene were compared with those of the corresponding commercial Marlotherm LH in the comparative example, as shown in Table 2 below.

[0186] Table 2

[0187] category Material <![CDATA[Boiling point [°C] a > <![CDATA[Melting point [°C] b > <![CDATA[Viscosity [cP] c > Example 1 <![CDATA[o-H0-MBT]]> 284.7 6.6 5.26 Example 2 <![CDATA[meta-H0-MBT]]> 278.3 -27.8 6.41 Example 3 <![CDATA[para-H0-MBT]]> 288.3 4.6 5.19 Example 4 <![CDATA[o-H 12 -MBT]]> 261.3 - 6.67 Example 5 <![CDATA[meta-H 12 -MBT]]> 266.3 - 4.92 Example 6 <![CDATA[para-H 12 -MBT]]> 272.0 - 5.62 Comparative Example 1 Marlotherm LH 282.7 - 4.36 Comparative Example 2 <![CDATA[Marlotherm H 12 -LH]]> 271.0 - 6.59

[0188] a : Experimental measurement results.

[0189] b :Based on Aspen+ software data.

[0190] c : The results of measurement using a DV-II+Pro viscometer at 20°C.

[0191] It can be clearly seen from the table above that the boiling point of the hydrogen-poor isomer is higher than that of the hydrogen-rich isomer, especially the boiling point of the para-isomer is higher than that of the other isomers. As for the melting point, since it is difficult to measure, we quoted the data of the ASPEN+ program and found that the melting point of the hydrogen-poor meta-isomer is particularly low. In addition, the viscosity tends to decrease with increasing temperature. The viscosity of the synthetic isomer at 20°C is measured to be about 4.92 to 6.67 cP.

[0192] Evaluation of the activity of the single isomers of -monobenzyltoluene and their physical mixtures

[0193] Figure 6 and Figure 7 The results of hydrogenation and dehydrogenation of three monobenzyltoluene isomers (o-MBT, m-MBT, and p-MBT) after removal of Cl are shown. Figure 6 a to Figure 6 c shows the hydrogenation results of purified monobenzyltoluene at reaction temperatures of 130°C, 110°C and 90°C, respectively. These figures show the H2 consumption efficiency as a function of time. full The hydrogenation activity is arranged in the order of ortho < meta < para-benzyltoluene. Figure 7 a to Figure 7 c shows the results of dehydrogenation of purified monobenzyltoluene at reaction temperatures of 260°C, 250°C, and 240°C, respectively. These figures show the efficiency of hydrogen release over time, and the dehydrogenation activity also follows the order of ortho < meta < para monobenzyltoluene, similar to hydrogenation.

[0194] Figure 8 a and Figure 8 b shows the Arrhenius plots of the hydrogenation and dehydrogenation of three monobenzyltoluene isomers (o-MBT, m-MBT, and p-MBT) after removal of Cl. Figure 8 In a, the Arrhenius plot of hydrogenation is drawn based on the initial reaction rate constants calculated at 90°C, 110°C, and 130°C, and the activation energy is also arranged in the order of ortho>meta>para-benzyltoluene, which shows a trend consistent with the reactivity. Figure 8 In b, the Arrhenius plot of dehydrogenation is depicted based on the initial reaction rate constants calculated at 240 °C, 250 °C, and 260 °C, and the activation energy is consistent with the trend of hydrogenation.

[0195] Fig. 9 a to Fig. 9 c shows the GC-FID analysis results of dehydrogenation after removal of Cl from three monobenzyltoluene isomers (o-MBT, m-MBT, and p-MBT). 12 -When the MBT conversion rate exceeds 95%, a new peak appears after 80 minutes. According to the GC-MS analysis results, it was found that the components corresponding to the new peaks were 1-methylfluorene (MF), 2-methylfluorene (MF) and 3-methylfluorene (MF). According to the results of GC analysis, the order of the number of methylfluorenes formed was p-benzyltoluene > m-benzyltoluene > o-benzyltoluene, which is similar to the hydrogenation and dehydrogenation activities. Although the use of a single p-benzyltoluene isomer seems to be more conducive to maximizing the hydrogen storage / release efficiency, the amount of methylfluorene formed also increased, which confirms the reduction in dehydrogenation selectivity.

[0196] In order to analyze the difference in hydrogen charging and dehydration rates with isomer types, the density functional theory (DFT) was used to calculate the effects of Pt (111), Ru (0001) and γ-Al2O3 (110) sites on H0-MBT, cis-H 12 -MBT and trans-H 12 -MBT adsorption energy, the results are as follows Fig.10 a to Fig.10 c. Among them, H0-MBT, cis-H 12 -MBT and trans-H 12 -MBT has the lowest adsorption energy for the para-isomer, which indicates that its adsorption strength is the strongest.

[0197] Three monobenzyltoluene isomers (hydrogen-poor state) were adsorbed on γ-alumina (γ-Al2O3) and Ru / Al2O3 catalysts, and thermogravimetric analysis was performed. The results are as follows: Fig.11 a to Fig.11 c. Among them, the para-isomer has the lowest adsorption energy and the strongest adsorption strength at all sites. On the other hand, the ortho-isomer is the least stable during the adsorption process, so the adsorption strength is weaker. Fig.11 In a, the adsorption intensity and adsorption amount on γ-alumina are arranged in the order of o-benzyltoluene < m-benzyltoluene < p-benzyltoluene. Fig.11 b shows the adsorption intensity and adsorption amount on the commercial Ru / Al2O3 catalyst, showing a similar trend to that of γ-alumina. In short, the order of adsorption intensity is p-benzyltoluene > m-benzyltoluene > o-benzyltoluene, which should be due to the difference in initial reaction rate caused by the adsorption intensity and adsorption amount, resulting in the above hydrogenation trend.

[0198] The physical mixture of monobenzyltoluene isomers is hydrogenated and dehydrogenated, and the result is as follows Figure 12 to Figure 14 In this regard, the results of hydrogenation and dehydrogenation of a binary physical mixture of two monobenzyltoluene isomers (para and meta) and a binary physical mixture of two monobenzyltoluene isomers (para and ortho) are shown in FIG. Fig.12 and Fig.13 The results of hydrogenation and dehydrogenation of a ternary physical mixture of three monobenzyltoluene isomers (ortho, meta and para) are shown in Fig.14 As shown. Among them, the activity of monobenzyltoluene isomers appears in the order of ortho-benzyltoluene < meta-benzyltoluene < para-benzyltoluene. As the number of isomers with good activity increases, the corresponding reaction activity also increases. In addition, as Fig.12 As shown in FIG. 1 , when the content of the para-isomer reaches or exceeds 90 mol %, the content of the meta-isomer has no significant effect on the hydrogenation and dehydrogenation results. Fig.13As shown in Figure 2, the ortho isomer has a greater impact on the hydrogenation and dehydrogenation results than the meta isomer. Therefore, it is desirable to reduce the amount of ortho-benzyltoluene used in the hydrogenation / dehydrogenation process.

[0199] -Evaluation of activity and stability of selective isomer combinations

[0200] In the hydrogen-rich state (H 12 The selective isomer compositions (p72 and p55) obtained by adding the synthesis step of the p-benzyltoluene component were analyzed by GC under the hydrogen-deficient state (H0-MBT) and the hydrogen-deficient state (H0-MBT). The physical properties and gas chromatography analysis results of the isomer compositions are shown in Tables 3 and Fig.15 .

[0201] Table 3

[0202] category Material <![CDATA[Boiling point [°C] a > <![CDATA[Melting point [°C] b > <![CDATA[Viscosity [cP] c > Example 1 <![CDATA[H0-MBT-p55]]> 282.9 - 4.08 Example 2 <![CDATA[H0-MBT-p72]]> 282.9 -5.2 3.87 Example 3 <![CDATA[H 12 -MBT-p55]]> 265.0 - 6.92 Example 4 <![CDATA[H 12 -MBT-p72]]> 266.0 - 6.73 Comparative Example 1 <![CDATA[SIM H0-LH]]> 282.8 - 4.15 Comparative Example 2 <![CDATA[SIM H 12 -LH]]> 266.9 - 7.15

[0203] a : Experimental measurement results.

[0204] b :Based on Aspen+ software data.

[0205] c : The results of measurement using a DV-II+Pro viscometer at 20°C.

[0206] As shown, when the selective isomer composition is converted from a hydrogen-deficient state to a hydrogen-rich state by hydrogenation, the composition of ortho-benzyltoluene, meta-benzyltoluene, and para-benzyltoluene does not change.

[0207] Fig.16 a and Fig.16 c shows the hydrogen storage and release results of the selective isomer compositions (p72 and p55) obtained by increasing the synthesis step of the p-benzyltoluene component and the comparative example MLH-sim, Fig.16 b and Fig.16 d also shows the Arrhenius plots for hydrogenation and dehydrogenation. The Arrhenius plots are drawn based on the initial reaction rate constants at 90°C, 110°C, and 130°C for hydrogenation and 240°C, 250°C, and 260°C for dehydrogenation. As the amount of p-benzyltoluene increases, the reactivity of the individual components also increases, and the order is evaluated as MBT-p72>MBT-p55>MLH-sim. And, the order of activation energy is MBT-p72>MBT-p55>MLH-sim. <MBT-p55<MLH-sim。

[0208] The product obtained by dehydrogenation of para-benzyltoluene was analyzed by GC, and the results are as follows: Fig.17 a and Fig.17 b. Therefore, Fig.17a corresponds to the hydrogen-rich state (pH 12 -MBT), Fig.17 b corresponds to the hydrogen-poor state (p-H0-MBT). Fig.17 a, with pH 12 With the increase of the dehydrogenation time of p-H0-MBT, the molar concentration of methylfluorene increased to 13.3 mol%, 19.6 mol% and 25.4 mol%, respectively. However, when p-H0-MBT was used as the reactant, the amount of methylfluorene generated in the same reaction time was very small. From the above results, it can be confirmed that hydrogen adsorbed on the catalyst surface or the intermediate (H6-MBT) participates in the formation of methylfluorene, and in the case where the reaction proceeds to 90% or more, methylfluorene is inevitably formed as the reaction proceeds further.

[0209] The apparent colors of the p-benzyltoluene and the product obtained by dehydrogenation of the same reactants for 215 minutes and 1200 minutes are as follows: Fig.18 Thus, according to the comparison results of the apparent color of p-benzyltoluene before the reaction and the apparent color of the dehydrogenation product, it can be confirmed that p-benzyltoluene is colorless in the hydrogen-rich state, and then as it is dehydrogenated to generate methylfluorene (MF), p-benzyltoluene gradually changes from yellow to reddish yellow.

[0210] At the same time, when p-benzyltoluene was dehydrogenated and then hydrogenated again, the effect of methylfluorene (MF) concentration in the dehydrogenation product on hydrogenation was evaluated. Fig.19 As shown. According to this, compared with pure p-H0-MBT, when the concentration of methylfluorene is 13.3 mol% and 25.4 mol%, the hydrogenation activity is reduced to the time required for hydrogen storage (charging) (t full ) increased by about 30 to 90 times. However, for the reactant with a methylfluorene concentration of 13.3 mol%, by adding 10 times the commercial Ru / Al2O3 catalyst, t full The value is 93 minutes. In conclusion, when the dehydrogenation efficiency is improved, the 12 When the MBT conversion rate reaches 90% or more, methylfluorene is formed, which has a significant negative impact on hydrogenation when it is greater than or equal to a predetermined concentration, so that effective hydrogen storage / release cannot be achieved.

[0211] The dehydrogenation reaction of p-benzyltoluene was carried out in the presence of Pt / Al2O3 catalyst and Pt-S / Al2O3 catalyst respectively, and the obtained products were analyzed by GC. The results are as follows: Fig. 20 a and Fig. 20b. Accordingly, when using the Pt-S / Al2O3 catalyst, the amount of methylfluorene formed under the same reaction time and the same hydrogen release efficiency (90%) was reduced from 13.3 mol% to 4.1 mol%. Therefore, in order to utilize monobenzyltoluene as a reversible and efficient hydrogen storage material, it is best to reduce the amount of methylfluorene formed during the dehydrogenation process as much as possible. For this purpose, the use of a dehydrogenation catalyst with controllable characteristics has been proven to be effective.

[0212] The stability of the selective isomer composition (p72) obtained by the synthesis process with increasing p-benzyltoluene content was evaluated in the dehydrogenation process by replacing the Pt / Al2O3 catalyst with the Pt-S / Al2O3 catalyst. For this purpose, the hydrogenation-dehydrogenation cycle was repeated. Here, in order to suppress the influence of a small amount of methylfluorene, the M / R was adjusted to 0.035 mol% in the first hydrogenation run, and to 0.14 mol% in the subsequent hydrogenation runs. The results are shown in Figure 2. Fig.21 As shown. Accordingly, when a catalyst that inhibits the formation of methylfluorene is used, hydrogenation is completed in about 40 minutes, and after 4 hours of reaction, the hydrogen release efficiency of dehydrogenation also reaches 97%, so that the weight storage density of H2 is maintained at 6.0wt% or higher in 10 experiments.

[0213] Hydrogen storage and hydrogen release tests were conducted using p-benzyltoluene, a selective isomer composition (p72 and p55) obtained by a synthetic process with increased p-benzyltoluene content, MLH-sim, and commercially available Marlotherm LH as comparative examples. The results are shown in FIG. Fig. 22 As shown (hydrogenation; Fig. 22 a; dehydrogenation; Fig. 22 b) Based on this, MBT-p72 is the material with the highest hydrogen storage / release efficiency. Under the same reaction conditions, the hydrogenated t full It was reduced by about 57% and dehydrogenation was increased by about 19%.

[0214] The products obtained by repeated hydrogen storage / dehydrogenation of para-benzyltoluene were analyzed by GC. Fig.23 As shown. According to this, in the dehydrogenation process, the use of p-benzyltoluene generates a large amount of methylfluorene compared with the use of other isomers, so even if the amount of catalyst is increased four times compared with the second hydrogenation, the hydrogen storage time increases from 44 minutes to 82 minutes. Therefore, the use of MBT-p72 that selectively increases the content of the p-isomer rather than using p-benzyltoluene alone as LOHC is advantageous from the perspective of reducing the manufacturing cost and saving the cost of the hydrogenation catalyst for the formation of methylfluorene.

[0215] The products obtained by repeated hydrogen storage / release of the selective isomer composition (p72) prepared by the synthesis process with increasing p-benzyltoluene content were analyzed by GC. Fig.24 As shown. Accordingly, when the selective isomer composition (MBT-p72) is used, the amount of methylfluorene formed during hydrogen release is 3.0 mol%, which is lower than the amount (4.0 mol%) when para-benzyltoluene is used alone. It is particularly noteworthy that during the hydrogenation process, under the same reaction conditions, the second hydrogenation of the para-isomer takes 82 minutes, while when MBT-p72 is used, it is greatly shortened to 40 minutes, indicating excellent hydrogen storage / release efficiency.

[0216] A person skilled in the art may easily make simple modifications or changes to the present disclosure, and all such modifications or changes may be deemed to be included within the scope of the present disclosure.

Claims

1. A method for reversibly storing and releasing hydrogen, comprising: a) providing a monobenzyltoluene (MBT) isomer mixture having a para-isomer content of at least 50 wt %; b) hydrogenating the monobenzyltoluene (MBT) isomer mixture to store hydrogen; as well as c) dehydrogenating the hydrogenated monobenzyltoluene (MBT) isomer mixture to release hydrogen therefrom, wherein hydrogen is stored or released by alternating hydrogenation and dehydrogenation, and During the dehydrogenation process, the methylfluorene content in the hydrogenated monobenzyltoluene (MBT) isomer mixture is maintained below 10 mol%.

2. The method according to claim 1, wherein: The halogen content in the monobenzyltoluene (MBT) isomer mixture is maintained below 30 ppm (w / w).

3. The method according to claim 1, wherein: The monobenzyltoluene (MBT) isomer mixture includes 42 mol % or less of o-benzyltoluene (o-MBT), 15 mol % or less of m-benzyltoluene (m-MBT), and 55 to 90 mol % of p-benzyltoluene (p-MBT).

4. The method according to claim 1, wherein: The step b) is carried out in the presence of a catalyst, which comprises a support containing a porous inorganic oxide and at least one active metal, and the active metal is selected from the group consisting of nickel, cobalt, palladium, platinum, iridium, ruthenium, rhodium, copper, gold, rhenium, zinc, molybdenum, tin, manganese, tungsten and germanium.

5. The method according to claim 4, wherein: The content of the active metal in the catalyst used in the step b) is determined to be in the range of 0.1 to 50 wt%.

6. The method according to claim 4, wherein: The porous inorganic oxide in the catalyst used in step b) is at least one selected from the group consisting of alumina, silica, silica-alumina, aluminum phosphate, zirconia, titania, cerium and yttrium.

7. The method according to claim 1, wherein: The step c) is carried out in the presence of a catalyst, which comprises a support containing a porous inorganic oxide, an active metal and sulfur.

8. The method according to claim 7, wherein: The content of the active metal in the catalyst used in step c) is determined to be 0.1 to 10 wt %, and the content of the sulfur is determined to be 0.001 to 2 wt %.

9. The method according to claim 8, wherein: The molar ratio of sulfur to active metal in the catalyst used in step c) is determined to be in the range of 0.1 to 1.

10. The method according to claim 7, wherein: In the catalyst used in step c), the porous inorganic oxide is alumina, and the active metal is platinum.

11. The method according to claim 1, wherein: The monobenzyltoluene (MBT) isomer mixture has a boiling point (1 atm) of 250 to 300° C. and a melting point of 10° C. or less.

12. The method according to claim 11, wherein: The monobenzyltoluene (MBT) isomer mixture has a viscosity (20° C.) of 3 to 8 cP and a density (20° C.) of 0.94 to 1.02 g / cm 3 .

13. The method according to claim 11, wherein: During hydrogenation, the ratio of active metals in catalyst / LOHC (M / R) was adjusted within the range of 0.01 to 0.4 mol %; during dehydrogenation, the ratio of active metals in catalyst / LOHC was adjusted within the range of 0.3 to 3 mol %.

14. The method according to claim 1, wherein: During the hydrogenation process, the reaction temperature is between 50 and 200°C and the reaction pressure is between 5 and 100 bar; during the dehydrogenation process, the reaction temperature is between 100 and 300°C and the reaction pressure is between 0.1 and 10 bar.

15. A liquid organic hydrogen carrier composition for reversible hydrogen storage / release, comprising: 42 mol% or less of o-benzyltoluene (o-MBT); 15 mol% or less of meta-benzyltoluene (m-MBT); as well as 55 to 90 mol% of p-benzyltoluene (p-MBT), The methylfluorene content is controlled below 10 mol %, and the halogen content is controlled below 30 ppm (w / w).

16. The liquid organic hydrogen carrier composition according to claim 15, wherein: The halogen is chlorine.

Citation Information

Patent Citations

  • Liquid Compounds and Method for the Use Thereof as Hydrogen Stores

    US20150266731A1

  • Hydrogen storage by reversible hydrogenation of pi-conjugated substrates

    US7351395B1

  • Hydrogen storage material and related system

    US7901491B2

  • KR2015-97558