Polyolefins and films comprising the same
By controlling the molecular weight distribution and crystal structure of polyolefins, the problems of low transparency and poor mechanical properties in the blown film are solved, and polyolefins with high transparency and high impact strength are achieved, which are suitable for high-performance blown films. Production.
Patent Information
- Application Number
- CN202380026766.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-10-16
- Filing Date
- 2023-10-20
- Publication Date
- 2024-11-05
AI Technical Summary
The existing linear low-density polyethylene (LLDPE) has problems of low transparency and poor mechanical properties in blown film processing, which is difficult to meet the needs of high impact strength and excellent haze properties.
A polyolefin with a molecular weight distribution of 2.5 to 4 is developed, and by controlling the crystal structure, it meets specific crystallization difficulty and Avrami parameter to Ozawa parameter ratio, optimizes crystallization behavior and high temperature elution characteristics to achieve high transparency and high impact strength.
The polyolefins have achieved excellent transparency and high impact strength properties in the film, and are suitable for the production of blown films requiring high mechanical properties and excellent transparency.
Smart Images

Figure CN118900855A_ABST
Abstract
Description
Technical Field
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application is based on and claims the benefit of priority of Korean Patent Application Nos. 10-2022-0144766 and 10-2023-0137793, filed on November 2, 2022 and October 16, 2023, respectively, the disclosures of which are hereby incorporated herein in their entirety by reference.
[0003] The present invention relates to a polyolefin exhibiting excellent haze properties and high drop impact strength properties, and a film comprising the polyolefin. Background Art
[0004] Linear low-density polyethylene (LLDPE) is a resin having a narrow molecular weight distribution and short chain branches of a certain length without long chain branches, which is prepared by copolymerizing ethylene and α-olefins under low pressure using a polymerization catalyst. Linear low-density polyethylene films have high breaking strength and elongation, and excellent tear strength and drop impact strength as well as basic polyethylene properties, and therefore, are increasingly used in stretch films, overlapping films, etc., while existing low-density polyethylene (LDPE) or high-density polyethylene (HDPE) are difficult to apply to these films.
[0005] With the recent decarbonization, there is an increasing demand for high-performance linear low-density polyethylene with improved high recyclability, and additionally, there is an increasing demand for linear low-density polyethylene with excellent processability and drop impact strength.
[0006] Drop impact strength is a very important mechanical property that determines the resistance of the resin to various impacts. However, compared with the excellent mechanical properties, linear low-density polyethylene has the disadvantages of poor blown film processability and low transparency. Blown film is a film prepared by blowing air into molten plastic for inflation, also known as inflated film.
[0007] Generally, since linear low-density polyethylene has a lower density, it has the characteristics of better transparency and higher drop impact strength. However, when a large amount of α-olefin comonomer is used to prepare low-density polyethylene, there is a problem that scaling may frequently occur during slurry polymerization, and therefore, in the slurry polymerization process, products with a density of 0.915 g / cc or more are mainly produced.
[0008] Therefore, there is a need to develop a polyolefin capable of achieving excellent transparency and high impact strength properties. Summary of the invention
[0009] Technical issues
[0010] To solve the problems of the prior art, a polyolefin is provided which exhibits excellent transparency and high impact strength properties by controlling the crystal structure.
[0011] Also provided is a film, in particular a blown film, comprising the polyolefin.
[0012] Technical Solution
[0013] According to the present invention, a polyolefin is provided.
[0014] The molecular weight distribution is 2.5 to 4,
[0015] The crystallization difficulty (F(T)) calculated according to the Mo method after differential scanning calorimetry, and the ratio of the Avrami parameter to the Ozawa parameter (a) satisfy the following requirements (i) and (ii) under the condition of 20% relative crystallinity, and
[0016] In the temperature rising elution fractionation (TREF) curve analyzed by cross fraction chromatography (CFC), A H The peak height ratio of / A1 meets the following requirement (iii):
[0017] (i) F(T)≤15
[0018] (ii) a>1.45
[0019] (iii)A H / A1≥1.8
[0020] In (iii),
[0021] A H represents the height of the highest peak in the TREF curve, and
[0022] A1, when the lowest peak in the TREF curve exists in the elution temperature of 40°C to 75°C, it represents the peak height of the lowest peak; and when the lowest peak in the TREF curve does not exist in the elution temperature of 40°C to 75°C, or when the lowest peak does not exist because the TREF curve has a single peak, it represents the height at the elution temperature of 65°C.
[0023] Also provided is a film comprising a polyolefin.
[0024] Beneficial Effects
[0025] The polyolefin according to the present invention exhibits excellent transparency and high impact strength properties. Therefore, it can be used to produce films, in particular, blown films which are required to have high impact strength properties and excellent transparency. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1is a graph showing the relationship between the crystallization completion time and the cooling rate under the condition of 20% relative crystallinity in DSC analysis of the polyolefins of Examples 1 to 4 and Comparative Example 1;
[0027] Figure 2 The TREF curve of the polyolefin of Example 1 shows the relationship between A1 and A H The diagram of the definition of ;
[0028] Figure 3 is a graph showing TREF obtained by CFC analysis of the polyolefin of Example 1 and the molecular weight in each elution region;
[0029] Figure 4 is a graph showing TREF obtained by CFC analysis of the polyolefin of Example 2 and the molecular weight in each elution region;
[0030] Figure 5 is a graph showing TREF obtained by CFC analysis of the polyolefin of Example 3 and the molecular weight in each elution region; and
[0031] Figure 6 is a graph showing TREF obtained by CFC analysis of the polyolefin of Example 4 and the molecular weight in each elution region. DETAILED DESCRIPTION
[0032] As used herein, the terms “first”, “second”, etc. are used to describe various components, and these terms are only used to distinguish a certain component from other components.
[0033] In addition, the terms used in this specification are only used to explain the exemplary embodiments and are not intended to limit the present invention. A singular expression may include a plural expression unless it is expressed differently in the context. It must be understood that the terms "including", "equipped with" or "having" in this specification are only used to specify the presence of effective features, quantities, steps, components or combinations thereof, and do not exclude the presence or possibility of adding one or more different characteristics, quantities, steps, components or combinations thereof in advance.
[0034] In the present invention, room temperature refers to 20°C±5°C.
[0035] The present invention can be modified in various ways and has various forms, and specific embodiments will be described and described in detail as follows. However, it should be understood that this description is not intended to limit the present invention to the specific forms disclosed, but rather, the present invention will cover all modifications, equivalents and alternatives that fall within the spirit and scope of the present invention.
[0036] Hereinafter, the polyolefin of the present invention and a film including the same will be described in detail.
[0037] Regarding the polyolefin according to the present invention,
[0038] The molecular weight distribution is 2.5 to 4,
[0039] The crystallization difficulty (F(T)) calculated according to the Mo method after differential scanning calorimetry (DSC) and the ratio of the Avrami parameter to the Ozawa parameter (a) satisfy the following requirements (i) and (ii) under the condition of 20% relative crystallinity, and
[0040] In the temperature rising elution fractionation (TREF) curve (X axis: elution temperature (°C), Y axis: elution amount (dw / dt)) analyzed by cross fraction chromatography (CFC), A H The peak height ratio of / A1 meets the following requirement (iii):
[0041] (i) F(T)≤15
[0042] (ii) a>1.45
[0043] (iii)A H / A1≥1.8
[0044] In (iii),
[0045] A H represents the height of the highest peak in the TREF curve, and
[0046] A1, when the lowest peak in the TREF curve exists in the elution temperature of 40°C to 75°C, it indicates the peak height of the lowest peak, and when the lowest peak in the TREF curve does not exist in the elution temperature of 40°C to 75°C (that is, when the lowest peak exists in the temperature range other than the elution temperature of 40°C to 75°C), or when the lowest peak does not exist because the TREF curve has a single peak, it indicates the height at the elution temperature of 65°C.
[0047] Blown film extrusion, used to produce packaging materials and various industrial films, is a method for mass-producing films with uniform thickness and surface by generating an airflow to expand the film extruded from a die through a screw. This method is mainly used to produce films with a relatively low melt index (MI) of about 0.5 to 2.0. In the process of expanding the polymer melt with air, uniform orientation can be provided in the machine direction (MD) and in the direction perpendicular to the stretching (transverse direction, TD), thereby ensuring excellent mechanical properties.
[0048] However, due to the method of generating bubble shape and controlling the degree of air cooling, the transparency is not as good as the cast film extrusion method. Therefore, the method of improving the film surface by blending LDPE with LLDPE is mainly adopted. However, in this case, there is a problem that the mechanical properties of the film are greatly reduced.
[0049] Therefore, it is necessary to develop a polyolefin having excellent haze properties even without being blended with LDPE while having excellent basic mechanical properties, and to quantify the corresponding structure.
[0050] Meanwhile, in the case of LLDPE for film production, the optical properties and physical properties are changed by the process of extrusion from the die and cooling. In this process, depending on the polymer structure of LLDPE, it may exhibit different crystallization behaviors even under the same processing conditions.
[0051] Therefore, in the present invention, polyolefin is defined by crystallization behavior parameters analyzed according to the Mo method, specifically, crystallization difficulty (F(T)) and the ratio (a) of Avrami parameter to Ozawa parameter, while its drop weight impact strength and transparency are optimized to excellent ranges.
[0052] The Mo method is a method for analyzing the crystallization characteristics of a polymer by combining the Avrami equation and the Ozawa method, and can be expressed as the following Equation 1 (see literature: Li, Yu et al., Journal of Applied Polymer Science 138.2 (2021): 49652).
[0053] [Equation 1]
[0054] logΦ=log F(T)-a log t
[0055] In equation 1,
[0056] Φ represents the cooling rate, F(T) represents the difficulty of crystallization, a represents the ratio of Avrami parameter to Ozawa parameter (Avrami parameter / Ozawa parameter), and t represents the crystallization completion time, i.e., the time taken to reach 20% relative crystallinity.
[0057] The above equation can be graphed by plotting the time to completion of crystallization (log t) on the x-axis, which is related to the crystallization rate, and the external condition cooling rate (log Φ) on the y-axis.
[0058] Figure 1 It is a graph showing the relationship between the crystallization completion time and the cooling rate under the condition of 20% relative crystallinity in differential scanning calorimeter (DSC) analysis of the polyolefins of Examples 1 to 4 and Comparative Example 1 of the present specification. Figure 1 These are merely examples for explaining the present invention, and the present invention is not limited thereto.
[0059] like Figure 1 As shown, the longer the crystallization completion time is, the slower the crystal formation rate is.
[0060] In addition, F(T) refers to the cooling rate condition corresponding to a specific crystallization time (1 minute). A lower F(T) value means that crystallization can occur smoothly even under moderate cooling conditions. Therefore, it is also defined as the difficulty of crystallization.
[0061] Meanwhile, a is a measure of how much the crystallization behavior is affected when the cooling conditions change. A higher a value means that the crystallization behavior will not change much regardless of the cooling conditions.
[0062] F(T) and a can be obtained from the results of differential scanning calorimetry (DSC) analysis using the Mo method described in the literature (Li, Yu et al., Journal of Applied Polymer Science 138.2 (2021): 49652).
[0063] Specifically, F(T) and a can be obtained by a method comprising the following steps:
[0064] A step of DSC analysis, wherein a polyolefin is introduced into a DSC apparatus, cooled to 20°C at a cooling rate of N°C / min (where N=5, 10, 15 and 20), and maintained at 20°C for 5 minutes, and then the cooled polyolefin is heated again to 160°C at a rate of 10°C / min to measure the change in melting enthalpy;
[0065] a step of calculating a crystallization completion time, which is a time taken to reach a temperature corresponding to a relative crystallinity of 20% when cooled from 120°C at a cooling rate of N°C / min (where N=5, 10, 15 or 20), wherein the relative crystallinity of 20% is determined by a point at which the enthalpy value is 20% when a crystallization peak between 30°C and 120°C in a temperature difference curve obtained as a result of DSC analysis is set as an analysis region and a total enthalpy value of the corresponding region is regarded as 100% of the relative crystallinity;
[0066] A step of obtaining a first order linear relationship by plotting the above calculated crystallization completion time (log t) on the X-axis and the cooling rate (log Φ) on the Y-axis and then performing curve fitting; and
[0067] The y-intercept and slope of the resulting first-order linear relationship are determined as F(T) and a, respectively.
[0068] More specifically, the polyolefin was introduced into the DSC apparatus, heated to 160° C. at a rate of 10° C. / min, and then maintained for 5 minutes to remove the thermal history.
[0069] The obtained polyolefin was cooled to 20°C at cooling rates of 5°C / min, 10°C / min, 15°C / min and 20°C / min (N°C / min, where N=5, 10, 15 and 20), respectively, and maintained at 20°C for 5 minutes, and then the cooled polyolefin was heated again to 160°C at a rate of 10°C / min, and the change in melting enthalpy was measured.
[0070] The crystallization peak between 30°C and 120°C in the temperature difference curve obtained as a result of DSC analysis was set as the analysis region, and the total enthalpy value of the corresponding region was regarded as 100% relative crystallinity. Based on the above total enthalpy, the peak point corresponding to the enthalpy value of 20% was determined as the relative crystallinity of 20%, and the time taken to reach the temperature corresponding to the relative crystallinity of 20% when cooled from 120°C at a cooling rate of N°C / min (where N=5, 10, 15 or 20), i.e., the crystallization completion time, was calculated respectively.
[0071] The temperature corresponding to 20% relative crystallinity refers to the temperature at a peak point where the enthalpy value is 20% based on the total enthalpy of the crystallization peak from 30°C to 120°C.
[0072] In addition, the enthalpy value can be obtained by integrating the crystallization peak area within the corresponding range.
[0073] In addition, the crystallization completion time (min) can be specifically determined according to the time at the point corresponding to 120° C. (t 120 ) and the time taken to reach 20% relative crystallinity, i.e., t 120 -t 20 _N, where the time (t 120 ), and the time taken to reach 20% relative crystallinity when cooled at each cooling rate of 5°C / min, 10°C / min, 15°C / min, and 20°C / min (t 20 _N, wherein N is as defined above).
[0074] The crystallization completion time is the log t data (log(t x _5), log(t x _10), log(t x _15) and log(t x_20)), where x is the value of relative crystallinity (%), and is plotted using x=20 and log(Φ) data (where Φ is the cooling rate (°C / min), Φ=5, 10, 15, 20). In this regard, the crystallization completion time, i.e., the time taken to reach 20% relative crystallinity (log t), is plotted on the X-axis, and the cooling rate (logΦ) is plotted on the Y-axis.
[0075] The first-order linear relationship was obtained by curve fitting of the plotted curve using data analysis software (Origin Pro, 9.1).
[0076] The resulting first-order linear relationship can be expressed as, for example, y=mx+b, and in the above relationship, the y-intercept (b) and the slope (m) are represented by F(T) and a, respectively.
[0077] Furthermore, the following Equation 1 in the Mo method can be derived by using the y intercept as log F(T) in a first-order linear relationship and using the absolute value of the slope as a.
[0078] [Equation 1]
[0079] logΦ=log F(T)-a log t
[0080] In equation 1,
[0081] Φ represents the cooling rate, F(T) represents the difficulty of crystallization, a represents the ratio of Avrami parameter to Ozawa parameter (Avrami parameter / Ozawa parameter), and t represents the crystallization completion time, i.e., the time taken to reach 20% relative crystallinity.
[0082] Regarding the polyolefin according to the present invention, the crystallization difficulty (F(T)) calculated according to the Mo method after DSC analysis and the ratio (a) of the Avrami parameter to the Ozawa parameter meet the above requirements (i) and (ii) under the condition of 20% relative crystallinity.
[0083] More specifically, under the condition of 20% relative crystallinity, the F(T) of the polyolefin is 15 or less, or 14.5 or less, or 14.3 or less, or 14 or less, and 10 or more, or 11 or more, or 12 or more, or 13 or more. In addition, a of the polyolefin is greater than 1.45, or 1.46 or more, or 1.48 or more, and 1.6 or less, or 1.58 or less, or 1.55 or less.
[0084] As described, compared with existing polyolefins, the polyolefin according to the present invention has a low F (T) value and a high a value, so that although the average crystallization rate is very fast, the cooling rate conditions have little effect on it. Therefore, even under blown film processing conditions where the cooling rate is considered to be relatively high, the crystallization rate will not change much, and a relatively small crystal structure can be produced. The small crystal structure leads to low surface haze and high transparency.
[0085] To explain this in relation to the crystal structure by CFC analysis, a highly crystalline polymer peak appears at a high elution temperature, and when the content is high, the polyolefin may exhibit a low F(T) due to the highly crystalline polymer chain. However, when the molecular weight of the highly crystalline polymer is too high, the mobility of the chain decreases, resulting in the crystallization behavior being insensitive to temperature changes.
[0086] Generally, when the linear low-density polyethylene film has a BOCD structure, the TREF crystalline region is widely distributed to have more than two peaks, which indicates that a molecular chain containing few short chain branches (SCBs) to show high crystallinity and a molecular chain containing a large number of SCBs coexist to form a macroscopic structure in which sheet molecules and connected molecules are mixed.
[0087] In the present disclosure, after CFC analysis of a polyolefin is performed using 1,2,4-trichlorobenzene as a solvent and separation into a low crystalline region and a high crystalline region based on an elution temperature of 75°C is performed, the content ratio (weight %) of a low crystalline polymer (or fraction) eluted in a region of elution temperature of 75°C or less, for example, in a region of elution temperature of 35°C to 75°C (excluding a soluble fraction (SF) eluted in a region of elution temperature below 35°C), and the weight average molecular weight (g / mol) thereof are respectively defined as W, W, and W. L and M L The content ratio (weight %) and weight average molecular weight (g / mol) of the high crystalline polymer (or fraction) eluted in the region where the elution temperature is higher than 75°C are defined as W H and M H .
[0088] W L and M L Indicates the quantification of the part in which the linking molecule is highly likely to be formed. Only when the molecular weight above an appropriate level is ensured, excellent drop impact strength and impact resistance can be achieved due to the linking molecule. In addition, W H and M HIt refers to a part that is easily impacted due to high crystallinity, but strength and rigidity can be sufficiently enhanced only when 50% by weight or more of it is contained in the polymer. In addition, only when a specific molecular weight range, such as 70,000 g / mol to 110,000 g / mol, is ensured, the relaxation time can be increased during film cooling, thereby suppressing excessive growth of a macromolecular structure having a spherulite morphology, and as a result, transparency can be controlled. However, when W H and M H If W is too high, the physical properties may deteriorate. H is 60 wt % or less, and W H It is 110,000 g / mol or less.
[0089] When the molecular weight and content of the low crystalline region must not be too high, light scattering can be controlled due to the layered-connected molecular structure. In addition, when the molecular weight of the high crystalline region is high, spherulite growth can be suppressed by increasing the relaxation time. However, when the content is too high, transparency may be impaired due to the high crystallinity.
[0090] For example, in the TREF curve, when the peak is not visible or the peak height is low in the low crystalline region with an elution temperature of 35°C to 75°C, even if the content of the high crystalline polymer eluted in the region with an elution temperature of more than 75°C is sufficient, a nucleus for crystallization due to high crystallinity can be quickly generated. In addition, when the molecular weight of the polymer in the corresponding high crystalline region is large or small, the speed at which the molecular chain moves during the crystallization process may be affected. If the polymer in the high crystalline region has a relatively large molecular weight, the chain movement slows down, resulting in insufficient crystal growth at the nucleation site and the formation of small spherulites, which can reduce roughness and scattering, and as a result, the haze properties can be improved. However, when the polymer in the high crystalline region has a relatively small molecular weight, large spherulites are formed due to the growth of the crystal structure, which increases roughness and scattering, resulting in poor haze properties.
[0091] Therefore, regarding the polyolefin according to the present invention, the ratio A H / A1 satisfies the following requirement (iii) in the TREF curve analyzed by CFC:
[0092] (iii)A H / A1≥1.8
[0093] In (iii),
[0094] A H represents the height of the highest peak in the TREF curve, and
[0095] A1 indicates the peak height of the lowest peak when the lowest peak in the TREF curve exists in the elution temperature of 40°C to 75°C, and indicates the height at the elution temperature of 65°C when the lowest peak in the TREF curve does not exist in the elution temperature of 40°C to 75°C (that is, when the lowest peak exists in the temperature range outside the elution temperature of 40°C to 75°C), or when the lowest peak does not exist because the TREF curve has a single peak.
[0096] Figure 2 The TREF curve of the polyolefin of Example 1 below shows A1 and A H . Figure 2 These are merely examples for explaining the present invention, and the present invention is not limited thereto.
[0097] refer to Figure 2 In the TREF curve of the polyolefin of Example 1, the highest peak appears when the elution temperature is 89.4°C, and the lowest peak appears when the elution temperature is 66.1°C. Therefore, the A of the polyolefin of Example 1 H It is the peak height of the highest peak appearing at an elution temperature of 89.4°C, and in A1 it is the peak height of the lowest peak appearing at an elution temperature of 66.1°C.
[0098] A H / A1 defines the relative amount of high crystalline polymer eluted in the high temperature region. The polyolefin of the present invention has a sufficient amount of high crystalline polymer by satisfying the above requirements. Therefore, the crystallized nuclei in the high elution temperature zone are slowly generated or not fully grown, resulting in the formation of small spherulites, which may lead to a reduction in roughness and scattering, thereby showing improved haze properties.
[0099] More specifically, according to the present invention, H / A1 is 1.8 or more, or 1.81 or more, or 2 or more, and 3 or less, or 2.8 or less, or 2.7 or less.
[0100] In addition, in addition to the above-mentioned crystal structure requirements, the polyolefin according to the present invention can also be further L 、M L , W H and M H The optimal required range shows excellent physical properties.
[0101] Specifically, the W of polyolefin L % by weight, which represents the content ratio (weight %) of the low crystalline polymer eluted in a region where the elution temperature is 75° C. or less (for example, in a region where the elution temperature is 35° C. to 75° C., excluding the soluble fraction (SF)) in the TREF curve analyzed by CFC, and M LThe soluble fraction (SF) refers to a fraction eluted in a region where the elution temperature is lower than 35° C. in the TREF curve. In addition, the content ratio (weight %) of the low crystalline polymer is based on the total weight of all eluted fractions.
[0102] More specifically, W L It may be 33 wt % or more, or 37 wt % or more, or 39 wt % or more, and 45 wt % or less, or 43 wt % or less, or 42 wt % or less, M L The molecular weight may be 130,000 g / mol or more, or 132,000 g / mol or more, or 133,000 g / mol or more, and 250,000 g / mol or less, or 230,000 g / mol or less, or 210,000 g / mol or less.
[0103] In addition, the W of polyolefin H 50 wt % to 60 wt %, M H and W are 70,000 g / mol to 110,000 g / mol, which respectively represent the content ratio (wt%) of the high crystalline polymer eluted in the region where the elution temperature is higher than 75° C. in the TREF curve, and the weight average molecular weight (g / mol) of the high crystalline polymer. More specifically, W H It may be 50 wt % or more, or 51 wt % or more, or 54 wt % or more, and 60 wt % or less, or 58 wt % or less, or 56 wt % or less, M H It may be 70,000 g / mol or more, or 70,500 g / mol or more, or 80,000 g / mol or more, and 110,000 g / mol or less, or 109,000 g / mol or less. In this regard, the content ratio (weight %) of the high crystalline polymer is based on the total weight of all eluted fractions.
[0104] Previously, a method of introducing long chain branches (LCBs) into mLLDPE was proposed to improve transparency. In general, mLLDPE with LCBs has significantly low M L and W L , because its crystallization characteristics vary in a unimodal manner. Specifically, the M of the polyolefin of the present invention L is 130,000 g / mol or more, and W L 33 wt% to 45 wt%, while the M of existing mLLDPE with LCBs is L is 20,000 g / mol to 60000 g / mol, or 27,000 g / mol to 28000 g / mol, and W L40 wt % or less, 20 wt % to 40 wt %. Therefore, the existing mLLDPE with LCBs has L and W L The lower the molecular weight, the smaller the area for forming connected molecules, so it is difficult to exhibit sufficient drop weight impact strength.
[0105] Furthermore, the polyolefin according to the present invention has a minimum peak elution temperature (Te L ) is 60℃ to 90℃, the highest peak elution temperature (Te H ) is 80°C to 100°C. More specifically, Te L It can be 60°C or above, or 64°C or above, 90°C or below, or 85°C or below. H It can be 80°C or more, or 85°C or more, or 89°C or more, and 100°C or less, or 95°C or less. These peak characteristics and high A H The / A1 value indicates that there is a high probability of participation of highly crystalline molecules in the film fabrication process, and when Te L and Te H and A H When the / A1 value appears within the above elution temperature range, the polyolefin can show a more improved effect in terms of haze.
[0106] More specifically, with regard to polyolefin, the content ratio of the soluble fraction (SF) eluted in a region where the elution temperature is lower than 35° C. in a TREF curve analyzed by CFC may be 1% by weight or more, or 4% by weight or more, and 15% by weight or less, or 12% by weight or less, based on the total weight of all eluted fractions.
[0107] Furthermore, regarding polyolefins, the content ratio of the fraction or polymer eluting in the region where the elution temperature is 35° C. or higher and lower than 55° C. may be 5% by weight or higher, or 6% by weight or higher, and 15% by weight or lower, or 10% by weight or lower, based on the total weight of all eluted fractions.
[0108] Furthermore, regarding polyolefins, the content ratio of the fraction or polymer eluting in the region where the elution temperature is 55° C. or higher and 75° C. or lower can be 20% by weight or higher, or 25% by weight or higher, and 40% by weight or lower, or 35% by weight or lower, based on the total weight of all eluted fractions.
[0109] In addition, regarding polyolefin, as described above, the content ratio of the fraction eluted in the region where the elution temperature is higher than 75°C or the high crystalline polymer can be 50% by weight or more, 51% by weight or more, and 60% by weight or less, 56% by weight or less based on the total weight of all eluted fractions.
[0110] Meanwhile, in the present invention, the content ratio of the fraction or polymer eluted within a certain elution temperature range is calculated as a percentage (weight % or wt %) of the content ratio of the fraction or polymer eluted in the corresponding elution temperature range based on the total weight of all eluted fractions obtained by CFC analysis.
[0111] Furthermore, in the present invention, the crystal structure characteristics of the polyolefin can be determined by CFC analysis. The specific measurement method and measurement conditions are described in the following experimental examples.
[0112] In addition to the above-mentioned crystal structure characteristics, the molecular weight distribution exhibited by the polyolefin according to the present invention is 2.5 to 4. More specifically, the molecular weight distribution of the polyolefin according to the present invention is 2.5 or more, or 2.8 or more, or 2.85 or more, or 2.87 or more, and 4 or less, or 3.8 or less. The polyolefin can exhibit excellent mechanical strength properties by having a molecular weight distribution in the above range. When the molecular weight distribution of the polyolefin is less than 2.5, it is considered that the mechanical properties are deteriorated, and when it exceeds 4, it is considered that the haze properties are deteriorated.
[0113] Meanwhile, in the present invention, regarding the molecular weight distribution of polyolefin, MWD is determined by measuring Mw and Mn respectively using gel permeation chromatography and then calculating the ratio of Mw to Mn (Mw / Mn) therefrom. The specific measurement method and conditions are described in the following experimental examples.
[0114] In addition, the polyolefin according to the present invention exhibits a density of 0.915 g / cc to 0.925 g / cc, more specifically, 0.915 g / cc or more, or 0.917 g / cc or more, and 0.925 g / cc or less, or 0.920 g / cc or less, as measured according to ASTM D1505.
[0115] When the polyolefin exhibits the above-mentioned density range, it can exhibit excellent mechanical properties.
[0116] In addition, the melt index (MI) of the polyolefin according to the present invention is measured at a temperature of 190° C. under a load of 2.16 kg according to ASTM D1238. 2.16 ) can be 0.5 g / 10min to 1.5 g / 10min, more specifically, 0.5 g / 10min or more, or 0.9 g / 10min or more, or 0.95 g / 10min or more, and 1.5 g / 10min or less, or 1.2 g / 10min or less, or 1.05 g / 10min or less.
[0117] In addition, the melt index (MI) of polyolefins is measured at a temperature of 190° C. under a load of 21.6 kg according to ASTM D1238. 21.6) can be 10 g / 10min to 50 g / 10min, more specifically, 10 g / 10min or more, or 20 g / 10min or more, or 25 g / 10min or more, and 50 g / 10min or less, or 40 g / 10min or less, or 35 g / 10min or less.
[0118] In addition, the MFRR (MI 21.6 / MI 2.16 ) may be 20 to 30, more specifically, 20 or more, or 25 or more, or 26 or more, and 30 or less, or 29.5 or less, which is a melt index (MI) measured at a temperature of 190° C. under a load of 21.6 kg according to ASTM D1238 standard. 21.6 ) divided by the melt index (MI) measured at 190°C under a load of 2.16 kg according to ASTM D1238 2.16 ) obtained.
[0119] The polyolefin according to the present invention has the above-mentioned crystal structure characteristics and the optimal ranges of density and melt index, thereby showing significantly improved impact strength properties and transparency as well as excellent processability.
[0120] The polyolefin of the present invention is specifically a copolymer of ethylene and an olefin monomer.
[0121] The olefin monomer may be ethylene, an α-olefin, a cycloolefin, a diene or a triene olefin having two or more double bonds.
[0122] Specific examples of the olefin monomers may include ethylene, propylene, 1-butene, 1-pentene, 4-methyl-1-pentene, 1-hexene, 1-heptene, 1-octene, 1-decene, 1-undecene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-eicosene, norbornene, norbornadiene, ethylidene norbornene, phenyl norbornene, vinyl norbornene, dicyclopentadiene, 1,4-butadiene, 1,5-pentadiene, 1,6-hexadiene, styrene, α-methylstyrene, divinylbenzene, 3-chloromethylstyrene, and the like, and two or more of these monomers may be mixed and copolymerized.
[0123] More specifically, the polyolefin is a copolymer of ethylene / C4-C10 alpha-olefin, and more specifically, the copolymer is ethylene / 1-hexene.
[0124] The polyolefin according to the present invention having the above-mentioned characteristics can be prepared by, for example, a preparation method comprising the following steps: a step of subjecting ethylene and an olefin monomer to a slurry polymerization reaction while introducing hydrogen in the presence of a catalyst composition comprising a first transition metal compound represented by the following formula 1 and a second transition metal compound represented by the following formula 2 in a molar ratio of 1:1 to 1:3:
[0125] [Formula 1]
[0126]
[0127] In formula 1,
[0128] R1 to R8, and R1' to R4' are the same or different from each other, and each independently represents hydrogen, halogen, C 1-20 Alkyl group, C 2-20 Alkenyl group, C 6-20 Aryl group, C 7-20 Alkyl aryl group or C 7-20 Arylalkyl groups;
[0129] R9 and R 10 are the same or different from each other and are each independently hydrogen, C 1-20 Alkyl group, C 2-20 Alkenyl group, C 6-20 Aryl group, C 7-20 Alkyl aryl group or C 7-20 An arylalkyl group, or R 10 and R 11 may be connected to each other to form one or more aliphatic rings, aromatic rings or heterocyclic rings;
[0130] R 11 is hydrogen, halogen, C 1-20 Alkyl group, C 2-20 Alkenyl group, C 6-20 Aryl group, C 7-20 Alkyl aryl group or C 7-20 Arylalkyl groups;
[0131] L is C 1-10 a straight or branched chain alkylene group;
[0132] D is -O-, -S-, -N(R)- or -Si(R)(R')-, wherein R and R' are the same or different from each other and are each independently hydrogen, halogen, C 1-20 Alkyl group, C 2-20 Alkenyl group or C 6-20 Aryl groups;
[0133] A is hydrogen, C 1-20 Alkyl group, C 2-20Alkenyl group, C 6-20 Aryl group, C 7-20 Alkyl aryl group or C 7-20 Arylalkyl groups;
[0134] M1 is a Group 4 transition metal;
[0135] X1 and X2 are the same or different from each other and are each independently halogen, C 1-20 Alkyl group, C 2-20 Alkenyl group, C 6-20 Aryl group, nitro group, amide group, C 1-20 Alkylsilyl group, C 1-20 Alkoxy groups or C 1-20 Sulfonate groups;
[0136] [Formula 2]
[0137]
[0138] In formula 2,
[0139] R 11 To R 21 are the same or different from each other and are each independently hydrogen, halogen, C 1-20 Alkyl group, C 2-20 Alkenyl group, C 6-20 Aryl group, C 7-20 Alkyl aryl group or C 7-20 Arylalkyl groups;
[0140] R 31 To R 35 are independently hydrogen, C 1-20 Alkyl group, C 2-20 Alkenyl group, C 6-20 Aryl group, C 7-20 Alkyl aryl group, C 7-20 Arylalkyl group, C 1-20 Alkoxy group, C 2-20 Alkoxyalkyl group or C 7-30 Aryloxyalkyl, where R 31 To R 35 At least one of them is C 1-20 Alkyl group, C 1-20 Alkoxy group, C 2-20 Alkoxyalkyl group or C 7-30 Aryloxyalkyl,
[0141] M2 is a Group 4 transition metal; and
[0142] X3 and X4 are the same or different from each other and are each independently halogen, C 1-20Alkyl group, C 2-20 Alkenyl group, C 6-20 Aryl group, nitro group, amide group, C 1-20 Alkylsilyl group, C 1-20 Alkoxy groups or C 1-20 Sulfonate group.
[0143] In the transition metal compounds of Formulae 1 and 2, the substituents will be described in more detail below.
[0144] C 1-20 The alkyl group may include a straight chain or branched chain alkyl group, and specifically may include but is not limited to a methyl group, an ethyl group, a propyl group, an isopropyl group, an n-butyl group, a tert-butyl group, a pentyl group, a hexyl group, a heptyl group, an octyl group, etc.
[0145] C 2-20 The alkenyl group may include a straight chain or branched alkenyl group, and specifically may include but is not limited to an allyl group, a vinyl group, a propenyl group, a butenyl group, a pentenyl group, and the like.
[0146] C 6-20 The aryl group may include a monocyclic or condensed-ring aryl group, and specifically may include but is not limited to a phenyl group, a biphenyl group, a naphthyl group, a phenanthrenyl group, a fluorenyl group, and the like.
[0147] C 7-20 The alkylaryl group (in which one or more hydrogens of the aryl group are replaced by an alkyl group) may specifically include methylphenyl, ethylphenyl, n-propylphenyl, isopropylphenyl, n-butylphenyl, isobutylphenyl, tert-butylphenyl, cyclohexylphenyl and the like.
[0148] C 7-20 An arylalkyl group is a substituent in which one or more hydrogen atoms of an alkyl group are replaced by an aryl group. Specifically, C 7-40 Arylalkyl groups may include benzyl groups, phenylpropyl groups, phenylhexyl groups, and the like.
[0149] C 1-20 The alkoxy group may include, but is not limited to, a methoxy group, an ethoxy group, a phenoxy group, a cyclohexyloxy group, and the like.
[0150] C 2-20 The alkoxyalkyl group (in which one or more hydrogen atoms of the alkyl group as described above are replaced by an alkoxy group) may specifically include, but are not limited to, alkoxyalkyl groups such as a methoxymethyl group, a methoxyethyl group, an ethoxymethyl group, an isopropoxymethyl group, an isopropoxyethyl group, an isopropoxyhexyl group, a tert-butoxymethyl group, a tert-butoxyethyl group, a tert-butoxyhexyl group, etc.; or an aryloxyalkyl group such as a phenoxyhexyl group, etc.
[0151] C 6-20 The aryloxy group may specifically include, but is not limited to, phenoxy, biphenyloxy, naphthoxy, and the like.
[0152] In addition, C 5-20 The heteroaryl group may include, but is not limited to, a monocyclic or condensed-ring heteroaryl group, and may include, but is not limited to, a carbazolyl group, a pyridyl group, a quinolyl group, an isoquinolyl group, a thiophenyl group, a furanyl group, an imidazolyl group, an oxazolyl group, a thiazolyl group, a triazine group, a tetrahydropyranyl group, a tetrahydrofuranyl group, and the like.
[0153] The halogen may be fluorine (F), chlorine (Cl), bromine (Br) or iodine (I).
[0154] The above substituents are optionally substituted with one or more substituents selected from the group consisting of a hydroxyl group; a halogen; an alkyl group or an alkenyl group, an aryl group, an alkoxy group; an alkyl group or an alkenyl group, an aryl group, an alkoxy group containing one or more heteroatoms of Groups 14 to 16; a silyl group; an alkylsilyl group or an alkoxysilyl group; a phosphine group; a phosphide group; a sulfonate group; and a sulfonic acid, within the range of achieving the same or similar effects as the desired effect.
[0155] In addition, the Group 4 transition metal may include, but is not limited to, titanium (Ti), zirconium (Zr), hafnium (Hf), and the like.
[0156] Specifically, the first transition metal compound of Formula 1 forms a structure in which a fluorene derivative is cross-linked by a bridge, and has an unshared electron pair that can act as a Lewis base in the structure of the ligand. Therefore, when loaded on the surface of the carrier having Lewis acid characteristics, it exhibits high polymerization activity even when loaded. In addition, since the first transition metal compound contains an electron-rich fluorene group, it has high activity, thereby polymerizing a high molecular weight olefin polymer.
[0157] Specifically, in the first transition metal compound, R1 to R4, and R1' to R4' in Formula 1 are each independently hydrogen; 1-12 Alkyl groups, such as methyl group, ethyl group, propyl group, isopropyl group, n-butyl group, tert-butyl group, pentyl group, hexyl group, heptyl group, octyl group, etc.; C 6-12 Aryl groups, such as phenyl groups, etc.; C 7-13 Alkyl aryl groups, such as 3,5-dimethylphenyl group, tert-butylphenyl group, etc.; C 7-13 Arylalkyl groups, such as benzyl groups, etc. More specifically, R1 to R4, and R1' to R4' of Formula 1 may all be hydrogen.
[0158] In addition, in Formula 1, R5 to R8 may each independently be hydrogen; 1-12Alkyl groups, such as methyl group, ethyl group, propyl group, isopropyl group, n-butyl group, tert-butyl group, pentyl group, hexyl group, heptyl group, octyl group, etc.; C 6-12 Aryl groups, such as phenyl groups, etc.; C 7-13 Alkyl aryl groups, such as 3,5-dimethylphenyl groups, tert-butylphenyl groups, etc.; or C 7-13 Arylalkyl groups, such as benzyl groups, etc. More specifically, R5 to R7 may all be hydrogen, and R8 may be hydrogen; C 1-12 Alkyl groups, such as methyl group, ethyl group, propyl group, isopropyl group, n-butyl group, tert-butyl group, pentyl group, hexyl group, heptyl group, octyl group, etc.; C 6-12 Aryl groups, such as phenyl groups, etc.; C 7-13 Alkyl aryl groups, such as 3,5-dimethylphenyl groups, tert-butylphenyl groups, etc.; or C 7-13 Arylalkyl groups, such as benzyl groups, and the like.
[0159] In addition, in Formula 1, R9 and R 10 can be independently hydrogen, C 1-12 Alkyl group, C 2-12 Alkenyl group, C 6-12 Aryl group, C 7-13 Alkyl aryl group or C 7-13 Arylalkyl group, or R9 and R 10 can be connected to each other to form one or more aromatic rings. More specifically, in Formula 1, R9 can be hydrogen, and R 10 Can be C 1-12 or C 1-6 an alkyl group, such as a methyl group, an ethyl group, a propyl group, an isopropyl group, an n-butyl group, a tert-butyl group, etc.; or R9 and R 10 May be connected to each other to form a benzene ring.
[0160] More specifically, R5 to R7, and R9 may all be hydrogen, and R8 may be hydrogen; C 6-12 Aryl group, such as phenyl group, etc.; or C 7-13 Alkyl aryl group, such as 3,5-dimethylphenyl group, tert-butylphenyl group, etc.; R 10 Can be C 1-6 an alkyl group, such as a methyl group, an ethyl group, a propyl group, an isopropyl group, an n-butyl group, a tert-butyl group, etc.; R5 to R8 may all be hydrogen, and R9 and R 10 May be connected to each other to form a benzene ring.
[0161] In addition, in Formula 1, R 11 More specifically, C 1-12 or C 1-6An alkyl group such as a methyl group, an ethyl group, a propyl group, an isopropyl group, an n-butyl group, a tert-butyl group, etc. More specifically, R 11 It may be a methyl group or an ethyl group.
[0162] In addition, in Formula 1, L can be specifically C 4-8 A straight or branched alkylene group. More specifically, L may be butene, pentene or hexene.
[0163] In addition, in Formula 1, D may specifically be -O-.
[0164] In addition, in Formula 1, A can be specifically hydrogen; C 1-12 Alkyl groups, such as methyl group, ethyl group, propyl group, isopropyl group, n-butyl group, tert-butyl group, pentyl group, hexyl group, heptyl group, octyl group, etc.; C 6-12 Aryl group, such as phenyl group, etc.; or C 7-13 Alkyl aryl groups, such as 3,5-dimethylphenyl groups, tert-butylphenyl groups, etc.; or C 7-13 Arylalkyl groups, such as benzyl groups, more specifically, A can be hydrogen, methyl groups, ethyl groups, propyl groups, isopropyl groups, n-butyl groups, tert-butyl groups.
[0165] In addition, in Formula 1, M1 may specifically be zirconium (Zr) or hafnium (Hf), and more specifically zirconium (Zr).
[0166] In addition, in Formula 1, X1 and X2 may each independently be a halogen, more specifically chlorine.
[0167] More specifically, the first transition metal compound represented by Formula 1 may be any one selected from the group consisting of the following compounds, but is not limited thereto:
[0168]
[0169] At the same time, the uncross-linked second transition metal compound represented by Formula 2 has a tetrahydroindene structure in which indene is reduced and cyclopentadiene as a ligand, so its hydrogen reactivity is relatively relaxed, and it is easy to reduce the weight average molecular weight and control PDI according to hydrogen input compared to the existing indene structure-based transition metal compounds for preparing low molecular weight polymers.
[0170] In addition, in these two ligands, regarding the tetrahydroindene structure ligand, the cyclohexane structure of the tetrahydroindene structure is not substituted, that is, R 14 To R 21 In addition, the cyclopentadiene structure in the tetrahydroindene structure is not substituted, that is, R 11 , R 12 and R 13are all hydrogen, or at least one of the carbons in positions 1 to 3, i.e., R 11 , R 12 and R 13 At least one of them is C 1-12 Alkyl group, C 2-12 Alkenyl group, C 6-12 Aryl group, C 7-13 Alkyl aryl group or C 7-13 In view of the excellent improvement effect according to the optimization of the substituents, the ligands of the tetrahydroindene structure may all be unsubstituted, that is, R 11 To R 21 It may be entirely hydrogen.
[0171] Meanwhile, in Formula 2, regarding the ligand of the cyclopentadiene structure, R 31 To R 35 At least one of the substituents of may be substituted. Specifically, R 31 To R 35 At least one of them is C 1-12 Alkyl group, C 1-12 Alkoxy group, C 2-12 Alkoxyalkyl group, or C 7-18 aryloxyalkyl group, the remainder of which may be hydrogen. More specifically, R 31 To R 35 One of them is C 1-12 Alkyl group, C 1-12 Alkoxy groups, or C 2-12 an alkoxyalkyl group, the remainder of which may be hydrogen; or R 31 To R 35 Two of them are C 1-12 alkyl group, the rest may be hydrogen; or R 31 To R 35 Can be C 1-12 Alkyl group.
[0172] More specifically, R 31 To R 35 One of them is C 1-6 Alkyl groups such as methyl, ethyl, propyl or butyl; C 1-6 an alkoxy group, such as methoxy, ethoxy, propoxy or butoxy; or C 2-12 Alkoxyalkyl groups, such as tert-butoxyhexyl, the remainder may be hydrogen. 31 To R 35 Two of them are C 1-6 alkyl groups, such as methyl, ethyl, propyl or butyl, and the remainder may be hydrogen. 31 To R 35 Both C 1-4Alkyl groups, such as methyl and ethyl.
[0173] In addition, in Formula 2, M2 may specifically be zirconium (Zr) or hafnium (Hf), more specifically zirconium (Zr).
[0174] Furthermore, in Formula 2, X3 and X4 may each independently be a halogen, more specifically chlorine.
[0175] More specifically, the second transition metal compound may be any one of the compounds represented by the following formulae, but is not limited thereto:
[0176]
[0177]
[0178] The above-mentioned first and second transition metal compounds can be synthesized by applying known reactions, and for more detailed synthesis methods, the Examples can be used as reference.
[0179] Meanwhile, in the present invention, the first transition metal compound may be in the form of a meso isomer, a racemic isomer or a mixed form thereof. On the contrary, the second transition metal compound may not include a meso isomer and does not include a racemic isomer.
[0180] As used herein, the term "racemic form" or "racemate" or "racemic isomer" refers to a form in which the same substituents on two ligands are located on opposite sides of the center of the plane containing the transition metal represented by M1 in Formula 1, for example, a transition metal such as zirconium (Zr) or hafnium (Hf), and the ligand portion.
[0181] In addition, as used herein, the term "meso form" or "meso isomer" is a stereoisomer of the above-mentioned racemic isomer, and refers to a form in which the same substituents on the two ligands are located on the same side of the plane containing the transition metal represented by M1 in Formula 1, for example, a transition metal such as zirconium (Zr) or hafnium (Hf) and the center of the ligand portion.
[0182] In the mixed supported catalyst according to one embodiment of the present disclosure, considering excellent catalytic activity and polymerizability, the first transition metal compound and the second transition metal compound may be supported in a molar ratio of 1:1 to 1:3 based on the first transition metal compound.
[0183] When they are included in the above molar ratio, the catalyst exhibits high activity in olefin polymerization, thereby preparing a polyolefin having improved falling weight impact strength and haze properties and excellent processability. More specifically, the molar ratio may be 1:1 to 1:2, or 1:1 to 1:1.5, or 1:1.1 to 1:1.2.
[0184] Meanwhile, the first and second transition metal compounds may be used in the form of a supported catalyst supported on a silica support.
[0185] As a carrier, a carrier containing hydroxyl groups on the surface can be used, and preferably, it can contain highly reactive hydroxyl groups and siloxane groups on the surface, which are dried to remove water on the surface. For example, silica, silica-alumina and silica-magnesia dried at high temperature can be used. These carriers can generally include oxide, carbonate, sulfate and nitrate components, such as Na2O, K2CO3, BaSO4 and Mg(NO3)2, etc.
[0186] When used as a supported catalyst, the prepared polymer has excellent particle shape and bulk density, and the catalyst can be appropriately used in conventional slurry polymerization, bulk polymerization and gas phase polymerization processes. In addition, among various carriers, the silica carrier supports the transition metal compound by chemically bonding the functional groups of the transition metal compound, and therefore, almost no catalyst is released from the carrier surface during the polymerization process, and as a result, when polyolefin is prepared by slurry polymerization or gas phase polymerization, the fouling phenomenon of adhering to the wall surface of the reactor or adhering to the reactor itself can be minimized.
[0187] In addition, when loaded on a carrier, the first and second transition metal compounds can be loaded in a content range of 0.01 mmol to 100 mmol, more specifically, 0.01 mmol or more, or 0.1 mmol or more, or 1 mmol or more, or 10 mmol or more, or 20 mmol or more, and 100 mmol or less, or 85 mmol or less, or 60 mmol or less, based on 1000 g of the carrier. When loaded within the above content range, the loaded catalyst can exhibit appropriate catalytic activity, which may be advantageous in maintaining catalytic activity and economic efficiency.
[0188] In addition, in terms of improving high activity and process stability, the catalyst may further include a promoter.
[0189] The co-catalyst may include one or more compounds selected from the group consisting of compounds represented by the following Formula 3:
[0190] [Formula 3]
[0191] -[Al(R a )-O] m -
[0192] In formula 3,
[0193] R a are the same as or different from each other and are each independently halogen; C 1-20 Hydrocarbyl group; or C substituted by halogen1-20 a hydrocarbyl group; and
[0194] m is an integer greater than or equal to 2.
[0195] Examples of the compound represented by Formula 3 may include alkylaluminoxane-based compounds such as methylaluminoxane, ethylaluminoxane, isobutylaluminoxane, butylaluminoxane, and the like, and any one of them or a mixture of two or more thereof may be used.
[0196] Among the above compounds, the cocatalyst may more specifically be an alkylaluminoxane type cocatalyst, for example methylaluminoxane.
[0197] The alkylaluminoxane-based cocatalyst stabilizes the transition metal compound and functions as a Lewis acid, thereby further improving the catalytic activity by including a metal element capable of forming a bond with a functional group introduced into the bridging group of the transition metal compound through Lewis acid-base interaction.
[0198] In addition, the amount of the co-catalyst can be appropriately adjusted according to the physical properties or effects of the desired catalyst and polymer and the polyolefin containing them. For example, when silica is used as a carrier, based on the weight of the carrier, for example, 1,000 g of silica, the amount of the co-catalyst loaded can be 100 g or more, or 500 g or more, or 700 g or more, and 1,000 g or less, or 900 g or less, or 800 g or less.
[0199] The catalyst having the above structure can be prepared by a preparation method comprising the steps of: a step of loading a co-catalyst compound on a carrier, and a step of loading a transition metal compound on a carrier, wherein the loading order of the co-catalyst and the transition metal compound can be changed as required.
[0200] Consider the effect of the supported catalyst with the structure determined according to the loading sequence, after the co-catalyst is loaded on the carrier, the loaded transition metal compound is loaded to ensure that the prepared supported catalyst has high catalytic activity and excellent process stability in the polymer preparation process. In addition, the loading sequence of the first transition metal compound and the second transition metal compound is not particularly limited yet, and the second transition metal compound can be loaded after loading the first transition metal mixture, or they can be loaded in reverse order. As a selection, the first and second transition metal compounds can be loaded simultaneously.
[0201] Meanwhile, the polymerization reaction for preparing polyolefin is carried out under the condition of introducing hydrogen.
[0202] Specifically, the amount of hydrogen introduced can be 5 ppm to 30 ppm based on the total weight of the olefin monomers. More specifically, the amount of hydrogen introduced can be 5 ppm or more, or 10 ppm or more, or 15 ppm or more, and 30 ppm or less, or 28 ppm or less, based on the total weight of the olefin monomers.
[0203] Hydrogen activates the inactive sites of the metallocene catalyst and causes a chain transfer reaction to control the molecular weight. The transition metal compound used in the present invention has excellent hydrogen reactivity, and therefore, by controlling the amount of hydrogen used during the polymerization process, a polyolefin having a desired molecular weight and melt index level can be effectively obtained.
[0204] The polymerization process may be carried out by a continuous polymerization process, for example, various polymerization processes known as polymerization reactions of olefin monomers may be used, such as a continuous solution polymerization process, a bulk polymerization process, a suspension polymerization process, a slurry polymerization process or an emulsion polymerization process, a gas phase polymerization process, etc. Specifically, in the present invention, a slurry polymerization process is carried out to achieve the above-mentioned physical properties of the polyolefin.
[0205] In addition, the polymerization reaction can be carried out at a temperature of 60° C. or more, or 70° C. or more, or 80° C. or more, 90° C. or less, or 85° C. or less. In addition, the polymerization reaction can be carried out at a pressure of 10 bar or more, or 20 bar or more, and 50 bar or less, or 40 bar or less. When polymerization is allowed at such a temperature and pressure, the desired physical properties of the polyolefin can be more easily achieved.
[0206] The polyolefin prepared by the above-mentioned preparation method has a crystal structure capable of ensuring excellent transparency and BOCD structure, as described above, thereby showing transparency and excellent drop weight impact strength properties. Therefore, the polyolefin can be used to produce films, in particular, blown films, which require high mechanical properties and excellent transparency.
[0207] Therefore, the present invention provides a resin composition comprising a polyolefin, in particular, a composition for producing a film.
[0208] Furthermore, the present invention provides a film, specifically, a blown film produced by using the polyolefin or the resin composition.
[0209] Film according to the present invention can be produced according to common film production methods, except that the polyolefin is used. For example, a composition for producing film can be prepared by mixing polyolefin and optional additives such as antioxidants and processing aids, and the composition is extruded into a film using an extruder to produce the film.
[0210] In addition, by including polyolefin, the film can express excellent transparency and mechanical properties.
[0211] Specifically, as measured under the conditions of Blown-Up ratio (BUR) of 2.3 to 3, more specifically 2.5 to 3, more specifically 2.5, and film thickness of 50 μm to 65 μm according to method A of ASTM D 1709, the film has a drop weight impact strength of 1600 gf or more, or 1800 gf or more, as measured according to ISO 13468 standard, and the film has a haze of 15% or less, or 14% or less. The higher the drop weight impact strength, the better the film, and therefore, the upper limit is not particularly limited. However, the drop weight impact strength can be, for example, 3000 gf or less. In addition, the lower the haze, the better the film, and therefore, the lower limit is not particularly limited. However, the haze can be, for example, 1% or more.
[0212] Example
[0213] Hereinafter, preferred exemplary embodiments will be provided to better understand the present invention. However, the following exemplary embodiments are provided only to more easily understand the present invention, but the content of the present invention is not limited thereby.
[0214] Synthesis example 1
[0215]
[0216] Preparation of ligand compounds
[0217] 100 mL of tert-butoxyhexyl magnesium chloride solution (about 0.14 mol, ether) was slowly added dropwise to 100 mL of trichloromethylsilane solution (about 0.21 mol, hexane) at -100°C over 3 hours, followed by stirring at room temperature for 3 hours. After separating the transparent organic layer from the mixed solution, the separated transparent organic layer was vacuum dried to remove excess trichloromethylsilane. As a result, a transparent liquid (6-tert-butoxyhexyl)dichloromethylsilane (yield 84%) was obtained.
[0218] 1H NMR (500MHz, CDCl3, 7.24ppm): 0.76(3H,s),1.11(2H,t),1.18(9H,s),1.32~1.55(8H,m),3.33(2H,t)
[0219] Fluorene (100 mmol) and methyl tert-butyl ether (MTBE, 0.3 M) were placed in a reactor at -20°C, and then n-BuLi (1.05 equiv., 2.5 M, in hexane) was slowly added, and stirred at room temperature for 6 hours to prepare a fluorenyl lithium solution. After the stirring was completed, the temperature of the reactor was cooled to -30°C, and tert-Bu-O-(CH2)6SiMeCl2 (0.505 equiv.) was added to the prepared fluorenyl lithium solution at -30°C, and washed with MTBE (50 mL). After stirring at room temperature for more than 8 hours, the solution was extracted by adding water, and dried (evaporated) to obtain (tert-Bu-O-(CH2)6)MeSi(9-C 13 H 10 The structure of the ligand was identified by 1H-NMR.
[0220] 1H NMR (500MHz, CDCl3): -0.35(3H,s),0.25(2H,m),0.59(2H,m),0.95(4H,m),1.17(9H,s),1 .31(2H,m),3.23(2H,t),4.11(2H,s),7.25(4H,m),7.37(4H,m),7.42(4H,m),7.86(4H,d).
[0221] Preparation of transition metal compounds
[0222] n-BuLi (2.05 equiv., 2.5 M in hexane) was slowly added to (tert-Bu-O-(CH2)6)MeSi(9-C 13 H 10 )2(100mmol) / MTBE(0.4M) solution, and the solution was reacted for more than 8 hours, while the temperature was raised to room temperature to prepare a dilithium salt slurry solution. At -20°C, the prepared dilithium salt slurry solution was slowly added to a ZrCl4(THF)2(1 equivalent, 100mmol) / hexane (1M) slurry solution, and further reacted at room temperature for 8 hours. The resulting reaction product was vacuum dried to completely remove the solvent. DCM (0.43M) was added to the resulting dry product, and then hexane (0.32M) was further added. The resulting precipitate (LiCl) was filtered, and the filtrate was vacuum dried. Hexane (0.3M) was added to the resulting dry product to prepare a slurry, which was then filtered. The resulting filtrate was washed several times with hexane to obtain tert-Bu-O-(CH2)6)MeSi(9-C 13 H9) 2ZrCl2 compound (A-1) (52.1 g, yield 75.4%).
[0223] 1H NMR (500MHz, C6D6): 1.16(9H,s),1.27(3H,s),1.59(2H,m),1.68(4H,m),1.93(4H, m),3.33(2H,t),6.90(4H,m),7.15(4H,m),7.60(4H,dd),7.65(2H,d),7.78(2H,d)
[0224] Synthesis example 2
[0225]
[0226] Preparation of ligand compounds
[0227] Fluorene (100 mmol) and methyl tert-butyl ether (MTBE, 0.3 M) were placed in a reactor at -20°C, and then n-BuLi (1.05 equivalents, 2.5 M, in hexane) was slowly added, and stirred at room temperature for 6 hours to prepare a fluorenyl lithium solution. After the stirring was completed, the temperature of the reactor was cooled to -30°C, and tert-Bu-O-(CH2)6SiMeCl2 (1.0 equivalent) was added to the prepared fluorenyl lithium solution at -30°C, and washed with MTBE (50 mL), and then introduced again. As a result, tert-Bu-O-(CH2)6SiMeCl (9-C 13 H 10 ).
[0228] 2-Methyl-4-phenyl-indene (1.0 eq., 100 mmol) and MTBE (0.3 M) were placed in a separate reactor at -20°C, and n-BuLi (1.05 eq., 2.5 M in hexane) was slowly added, followed by stirring at room temperature for 6 hours to prepare lithiated 2-methyl-4-phenyl-indene.
[0229] The prepared tert-Bu-O-(CH2)6SiMeCl(9-C 13 H 10 ) was cooled to -30°C, and then lithiated 2-methyl-4-phenyl-indene was introduced and reacted at room temperature for more than 8 hours under stirring. The obtained product was extracted by adding water and dried (evaporated) to obtain a ligand compound (tert-Bu-O-(CH2)6)MeSi(9-C 13 H 10 )(2-Me-4-Ph-indene). The structure of the ligand was identified by 1H-NMR.
[0230] 1H NMR (500MHz, CDCl3): -0.10(3H,s),0.58(2H,m),1.08(2H,m),1.23(9H,s),1.38(4H,m),1.62(2H,m),2.26(3H,s),3.28(2H ,t),3.81(1H,s),4.11(1H,s),6.87(1H,s),7.24(3H,m),7.36(3H,m),7.44(4H,m),7.53(2H,t),7.61(2H,d),7.86(2H,d).
[0231] Preparation of transition metal compounds
[0232] n-BuLi (2.05 equiv., 2.5 M in hexane) was slowly added to (tert-Bu-O-(CH2)6)MeSi(9-C 13 H 10 )(2-Me-4-Ph-indene)(100 mmol) / MTBE (0.4 M) solution, and the solution was allowed to react for more than 8 hours while the temperature was raised to room temperature to prepare a dilithium salt slurry solution.
[0233] At -20 ° C, the prepared dilithium salt slurry solution was slowly added to the ZrCl4(THF)2 (1 equivalent, 100 mmol) / hexane (1M) slurry solution, and further reacted at room temperature for 8 hours. The resulting reaction product was vacuum dried to completely remove the solvent. DCM (0.43M) was added to the resulting dried product, and then hexane (0.32M) was further added. The resulting precipitate (LiCl) was filtered and the filtrate was vacuum dried. Hexane (0.3M) was added to the resulting dried product to prepare a slurry, which was then filtered. The filtrate was washed several times with hexane to obtain (tert-Bu-O-(CH2)6)MeSi(9-C 13 H9) (2-Me-4-Ph-indene)ZrCl2 compound (A-2) (37.8 g, yield 64.0%).
[0234] 1H NMR (500MHz, C6D6): 1.17(9H,s),1.30(3H,s),1.57(2H,m),1.66(4H,m),1.86(4H,m),2.26(3H,s),3.32(2H ,t),6.90(2H,m),6.95(1H,s),7.14(3H,m),7.36(1H,d),7.45(3H,t),7.61(4H,m),7.65(1H,d),7.78(1H,d)
[0235] Synthesis example 3
[0236]
[0237] n-BuLi (1.05 eq.) was slowly added to a solution in which indene (1 eq.) was dissolved in THF (0.3 M) at -25°C, and stirred at room temperature for 3 hours. TMSCl((CH3)3SiCl) (1.05 eq.) was added to the resulting reaction product at -25°C, followed by stirring at room temperature overnight. The resulting reaction product was dried to completely remove the solvent, and ZrCl4 (1 eq.) was added, toluene (0.5 M) was introduced, and stirred under reflux overnight. The resulting reaction product was cooled to room temperature, and then hexane (0.5 M) was introduced, and filtered to obtain indene-ZrCl3 solid.
[0238] In a separate reactor, n-BuLi (1.05 equivalents) was slowly added dropwise to a solution in which n-butylcyclopentadiene (1 equivalent) was dissolved in THF (0.3 M) at -25°C, followed by stirring at room temperature for 3 hours. Indene-ZrCl3 (1 equivalent) prepared as above was introduced into the resulting reaction product at -25°C, followed by stirring at room temperature overnight. The resulting reaction product was dried to completely remove the solvent, and then hexane was introduced, and the solid was filtered to obtain n-BuCp-ZrCl2-indene intermediate.
[0239] The obtained intermediate and Pd / C (based on the total weight of C, Pd content = 10 wt %, corresponding to 0.1 mol based on 1 mol of the intermediate) were introduced into a parr reactor (600 ml) using DCM (0.3 M), and then 15 bar of hydrogen was introduced and reacted at 40 ° C overnight under stirring. After the reaction was completed, the hydrogen remaining in the reactor was discharged, and the final product and Pd / C in the parr reactor were filtered out using a cannula and washed with DCM. The filtrate was dried in vacuo, hexane was added, and then filtered to obtain the compound (B-1) of the above structure in the solid phase.
[0240] 1H NMR (500MHz, CDCl3): 1.11(3H,t),1.50(2H,m),1.62(2H,m),1.70(2H,m),1.90(2H,m),2 .53(2H,m),2.78(2H,t),2.90(2H,m),5.48(2H,s),5.93(1H,s),6.22(2H,d),6.35(2H,d)
[0241] Synthesis example 4
[0242]
[0243] The compound (B-2) of the above structure was obtained in a solid phase in the same manner as in Synthesis Example 3 except that tert-butoxyhexylcyclopentadiene was used instead of n-butylcyclopentadiene.
[0244] 1H NMR (500MHz, CDCl3): 1.23(9H,s),1.40(4H,m),1.64(6H,m),1.88(2H,m),2.52(2H,m),2 .68(2H,t),2.91(2H,m),3.34(2H,t),5.49(2H,s),5.94(1H,s),6.18(2H,d),6.28(2H,d)
[0245] Synthesis example 5
[0246]
[0247] The compound (B-3) of the above structure was obtained in a solid phase in the same manner as in Synthesis Example 3 except that 1-methyl-3-propyl-1,3-cyclopentadiene was used instead of n-butylcyclopentadiene.
[0248] 1H NMR (500MHz, CDCl3): 0.93(3H,t),1.350(2H,m),1.49(2H,m),1.63(2H,m),1.89(2H,m),2.22(3 H,s),2.47(1H,m),2.55(3H,m),2.90(2H,m),5.48(2H,s),5.93(2H,m),5.98(1H,m),6.09(1H,m)
[0249] Comparative Synthesis Example 1
[0250]
[0251] The transition metal compound (C-1) of the above structure was prepared in the same manner as in Preparation Examples 2 to 6 in Korean Patent Publication No. 10-2016-0029718.
[0252] Comparative Synthesis Example 2
[0253]
[0254] The 1,2-ethylenebis(indenyl)ZrCl2 compound was synthesized as disclosed in J.AM.CHEM.SOC.VOL.126, No.46, 2004, pp.15231-15244.
[0255] Comparative Synthesis Example 3
[0256]
[0257] The transition metal compound (D) of the above structure is prepared in the same manner as in Preparation Example 2 in Korean Patent Publication No. 10-2016-0029718.
[0258] Preparation Example 1
[0259] 2.0 kg of toluene and 700 g of silica (SYLOPOL 952X, manufactured by Grace Davision) were introduced into a 20 Lsus autoclave and stirred while raising the temperature of the reactor to 40° C. 5.4 kg of a methylaluminoxane solution (10 wt % in toluene, manufactured by Albemarle) was introduced into the reactor, and the temperature was raised to 70° C., followed by stirring at about 200 rpm for about 12 hours.
[0260] After that, the temperature of the reactor was lowered to 40°C and stirring was stopped. The reaction product was allowed to settle for about 10 minutes and then decanted. 2.0 kg of toluene was added to the reaction product and stirred for 10 minutes, stirring was stopped, and then the solution was allowed to settle for about 30 minutes and then decanted.
[0261] 2.0kg toluene is introduced into the reactor, and then, the compound (A-1) (20mmol) prepared in Synthesis Example 1 and the compound (B-1) (40mmol) prepared in Synthesis Example 3 are introduced as the first transition metal compound and the second transition metal compound, and 1000mL toluene is introduced. The temperature of the reactor is raised to 85°C, followed by stirring for about 90 minutes. Then, the temperature of the reactor is reduced to room temperature, stirring is stopped, and the reaction product is precipitated for about 30 minutes, and then the reaction product is decanted. Subsequently, 3kg hexane is introduced into the reactor, and the hexane slurry solution is transferred to a 20L filter dryer to filter the solution, and dried at 50°C under reduced pressure for about 4 hours to obtain 1.05kg mixed metallocene catalyst.
[0262] Preparation Examples 2 to 4 and Comparative Preparation Examples 1 to 3
[0263] Each mixed metallocene catalyst was prepared in the same manner as in Preparation Example 1, except that the kinds and input amounts of the first and second transition metal compounds were changed as shown in Table 1 below.
[0264] Table 1
[0265]
[0266] <Production of Polyolefin>
[0267] Examples 1 to 4 and Comparative Examples 1 to 3
[0268] As a polymerization reactor, a 140L continuous polymerization reactor operated at a reaction flow rate of about 7m / s was prepared, in which an isobutylene slurry circulation process was feasible. In addition, in the reactor, the reactants required for olefin polymerization as described in Table 2 were continuously introduced. As catalysts for each polymerization reaction, those prepared in the preparation examples or comparative preparation examples described in Table 1 were used, and the catalysts were introduced after mixing with the isobutylene slurry. The polymerization reaction was carried out at a pressure of about 40bar and a temperature of about 85°C. In addition, other main conditions for the polymerization reaction are described in Table 2 below.
[0269] Comparative Example 4
[0270] BO1801EN (manufactured by DAELIM) was commercially purchased and used.
[0271] Comparative Example 5
[0272] XP8318ML (manufactured by Exxon chemical) was commercially purchased and used.
[0273] Comparative Example 6
[0274] XP8656ML (manufactured by Exxon chemical) was commercially purchased and used.
[0275] Table 2
[0276]
[0277] In Table 2,
[0278] Input amount of 1-hexene 1 (wt%) is expressed as a percentage of the relative content based on the total weight of the olefin monomers comprising ethylene and 1-hexene, and
[0279] Hydrogen input 2 (ppm) based on the total weight of olefin monomers including ethylene and 1-hexene.
[0280] Experimental Example 1
[0281] F(T) and a
[0282] The polyolefin of Example 1 was subjected to differential scanning calorimetry (DSC) analysis, and the crystallization difficulty (F(T)) and the ratio (a) of the Avrami parameter to the Ozawa parameter (Avrami parameter / Ozawa parameter) of the polyolefin were calculated according to the DSC analysis results using the Mo method described in the literature (Li, Yu et al., Journal of Applied Polymer Science 138.2 (2021): 49652). At this time, for comparison, commercially available polyolefins EP2010 (manufactured by LG Chem) and XP6056 (manufactured by Exxon Chemical) were also subjected to DSC analysis in the same manner, and F(T) and a were calculated, respectively (referred to as Reference Comparative Examples 1 and 2, respectively).
[0283] In detail, the polyolefin prepared in Example 1 and the polyolefin of the reference comparative example were equally divided into aluminum pans in an amount of 5 mg each, introduced into a DSC apparatus (DSC Q20 / RCS90 (manufactured by TA)), and heated to 160°C at a rate of 10°C / min and maintained for 5 minutes to remove the thermal history.
[0284] The obtained polyolefin was cooled to 20°C at cooling rates of 5°C / min, 10°C / min, 15°C / min and 20°C / min (N°C / min, where N=5, 10, 15 and 20) and maintained at 20°C for 5 minutes, and then the cooled polyolefin was heated again to 160°C at 10°C / min, and the change in melting enthalpy was measured.
[0285] In the temperature difference curve obtained as a result of DSC analysis, the crystallization peak of 30°C to 120°C was set as the analysis region, the total enthalpy value of the corresponding region was regarded as 100% relative crystallinity, and the peak points of the enthalpy values corresponding to 20%, 40%, 60%, 80% and 100% of the total enthalpy were respectively determined as 20% relative crystallinity, 40% relative crystallinity, 60% relative crystallinity, 80% relative crystallinity and 100% relative crystallinity. The time (min) taken to reach the temperature corresponding to each relative crystallinity of 20%, 40%, 60%, 80% and 100% when cooled from 120°C at a cooling rate of N°C / min (where N=5, 10, 15 or 20) was calculated respectively and determined as the crystallization completion time.
[0286] Specifically, in the temperature difference curve, the time (t 120 ), and each time t taken to reach a relative crystallinity of 20%, 40%, 60%, 80% or 100% when cooled at each cooling rate of 5°C / min, 10°C / min, 15°C / min and 20°C / min 20 _N, t40 _N, t 60 _N, t 80 _N or t 100 _N (where N is 5, 10, 15 or 20, which is the value corresponding to the cooling rate). The crystallization completion time (min) is determined by the time corresponding to the point of 120°C (t 120 ) and the time taken to reach a relative crystallinity of 20%, 40%, 60%, 80% or 100%. For example, the crystallization completion time of 20% relative crystallinity is calculated by the time corresponding to the point of 120°C (t 120 ), and the time taken to reach a relative crystallinity of 20% when cooled at cooling rates of 5°C / min, 10°C / min, 15°C / min, and 20°C / min (t 20 _N, N is the same as the above definition), that is, t 120 -t 20 The value of _N.
[0287] The Log(t) data of the time taken to reach a relative crystallinity of 20%, 40%, 60%, 80% or 100% when cooled at a cooling rate of N°C / min (where N=5, 10, 15 or 20), specifically corresponding to log(t x _5), log(t x _10), log(t x _15), log(t x The data of log(Φ) (Φ is the cooling rate (°C / min) value, Φ=5, 10, 15 and 20) and log(_20) (wherein x is the relative crystallinity (%) value, x=20, 40, 60, 80 or 100) are plotted. When plotting, the crystallization completion time, for example, the time taken to reach 20% relative crystallinity (log t) is plotted on the X-axis, and the cooling rate (logΦ) is plotted on the Y-axis.
[0288] The plotted graph was fitted to a first-order linear relationship using data analysis software (Origin Pro, 9.1). In the obtained first-order linear relationship, the y intercept and slope were determined as F(T) and a, respectively.
[0289] Furthermore, the following Equation 1 in the Mo method is derived by using the y intercept as log F(T) in the first-order linear relationship and using the absolute value of the slope as a.
[0290] [Equation 1]
[0291] logΦ=log F(T)-a log t
[0292] In equation 1,
[0293] Φ represents the cooling rate, F(T) represents the difficulty of crystallization, a represents the ratio of Avrami parameter to Ozawa parameter (Avrami parameter / Ozawa parameter), and t represents the crystallization completion time (min), specifically, the time taken to reach 20%, 40%, 60%, 80% or 100% relative crystallinity.
[0294] Based on the fitting equation, the a value and log F(T) value corresponding to each relative crystallinity (20%, 40%, 60%, 80%, 100%) were calculated, and the results are shown in Tables 3 to 5.
[0295] Tables 3 to 5 are the results of the polyolefins of Example 1 and Reference Comparative Examples 1 and 2, respectively. i represents the crystallization rate (min / °C) determined by the value of 1000 / F(T), Indicates that at each relative crystallinity C i The average of the values.
[0296] Table 3
[0297]
[0298] Table 4
[0299]
[0300] Table 5
[0301]
[0302] Typically, the region corresponding to 20% relative crystallinity is where crystals begin to form and is the point where the greatest thermal variation occurs, and is sensitive to cooling rate conditions. Therefore, in extrusion processes that require cooling with low temperature external air, such as blown film processes, the region corresponding to 20% relative crystallinity is very important. As demonstrated by the results of Tables 3 to 5, the region where the F(T) and a values vary the most depending on the type of polyolefin is the region corresponding to 20% relative crystallinity.
[0303] As shown in Table 3, since the polyolefin of Example 1 has a relatively low F(T) value, crystallization is easy to occur. However, since the a value is high, the change of the crystallization characteristics caused by the change of the cooling rate is not significant. On the contrary, as shown in Tables 4 and 5, since the polyolefin of Reference Comparative Examples 1 and 2 has a high F(T) value, crystallization itself is difficult to occur. However, since the a value is low, the crystallization characteristics can be more easily changed according to the change of the cooling rate. In other words, when the cooling rate slows down during film processing, the polyolefin of Reference Comparative Examples 1 and 2 takes a long time to reach a specific relative crystallinity, for example, a relative crystallinity of 20%, and therefore, there is a high possibility that crystal growth is relatively suppressed. However, when the cooling rate is fast enough, compared with the polyolefin of Example 1 with a high a value, the time to reach crystallinity due to the low a value changes more, so there is a possibility that the crystallization completion time becomes similar to or even faster than the crystallization completion time of the polyolefin of Example 1.
[0304] Experimental Example 2
[0305] The physical properties of the polyolefins prepared in Examples and Comparative Examples were measured as described below, and the results are shown in Tables 6 and 7, respectively.
[0306] (1) Melt index (MI) 2.16 ): measured according to ASTM D1238 (Condition E, 190°C, 2.16 kg load) standard.
[0307] (2) Melt index (MI) 21.6 ): measured according to ASTM D1238 (Condition E, 190°C, 21.6 kg load) standard.
[0308] (3) MFRR(MI 21.6 / MI 2.16 ): By using MI 21.6 (ASTM D1238, 190°C, 21.6 kg load) divided by MI 2.16 (ASTM D1238, 190°C, 2.16 kg load) ratio obtained.
[0309] (4) Density: measured according to ASTM D1505.
[0310] (5) Molecular weight distribution
[0311] The weight average molecular weight (Mw) and the number average molecular weight (Mn) were respectively measured using gel permeation chromatography (GPC, manufactured by Waters), and the molecular weight distribution (Mw / Mn) was calculated from the measured values.
[0312] In detail, the measured samples were evaluated using a Polymer Laboratories PLgel MIX-B 300 mm long column and a Waters PL-GPC220 device. The measuring temperature was 160 ° C, 1,2,4-trichlorobenzene was used as a solvent, and the flow rate was 1 mL / min. The sample was prepared at a concentration of 10 mg / 10 mL and then provided in an amount of 200 μL. Mw and Mn values were determined using a calibration curve formed using polystyrene standards. Nine polystyrene standard samples were used, each with a molecular weight (g / mol) of 2,000 / 10,000 / 30,000 / 70,000 / 200,000 / 700,000 / 2,000,000 / 4,000,000 / 10,000,000.
[0313] (6) CFC analysis
[0314] The polyolefins prepared in the examples and comparative examples were subjected to cross fraction chromatography (CFC) analysis by the following method, and A was calculated based on the results: H / A1.
[0315] [Cross-fraction chromatography analysis conditions (including TREF and GPC analysis)]
[0316] -Analysis equipment: Polymer Char CFC-7890B (G3440D)
[0317] (Detector: Integrated Detector IR5 MCT)
[0318] -Sample preparation and injection: 32 mg of the polyolefin prepared in the examples or comparative examples was placed in a 10 mL vial and placed in an autosampler, 8 mL of 1,2,4-trichlorobenzene (TCB) was introduced, and dissolved at 160° C. for 90 minutes and stabilized at 140° C. for 20 minutes. After nitrogen purging, the sample was extracted and loaded onto a temperature rising elution fractionation column (TREF column).
[0319] - Crystallization: The temperature of the sample previously loaded in the TREF column was set to 140°C and cooled from 140°C to 35°C at a rate of 0.5°C / min and held for 15 minutes.
[0320] The detailed conditions for stability and crystallization are as follows:
[0321]
[0322] - Temperature Rising Elution Fractionation (TREF) analysis: A previously crystallized sample was heated from 35°C to 120°C at a rate of 1°C / min to below the fraction temperature, then fixed, and the concentration of the fraction eluted at this temperature for 5 minutes was measured. A TREF curve was derived from the results of the concentration measurements.
[0323] From the TREF curve, based on the total weight of all eluted fractions, the content ratio of the soluble fraction (SF) eluted in the region where the elution temperature is below 35°C (<35°C), the content ratio of the fraction eluted in the region where the elution temperature is above 35°C and below 55°C (35°C to 55°C), the content ratio of the fraction eluted in the region where the elution temperature is above 55°C and below 75°C (55°C to 75°C), and the content ratio of the fraction eluted in the region where the elution temperature is above 75°C (>75°C) were calculated (weight %).
[0324] Furthermore, from the TREF curve, the content ratio (W % by weight) of the low crystalline polymer (excluding SF) eluted in the region of elution temperature of 75° C. or less, specifically, in the region of elution temperature of 35° C. to 75° C., was calculated based on the total weight of all eluted fractions. L ), and the content ratio of the high crystalline polymer eluted in the region where the elution temperature is higher than 75°C (W H ).
[0325] In addition, determine the elution temperature (Te L ) and the elution temperature of the highest peak (Te H ).
[0326] In addition, the peak height of the highest peak in the TREF curve is determined as A H , when the lowest peak in the TREF curve exists in the elution temperature of 40°C to 75°C, the peak height of the lowest peak is determined as A1, however, when the lowest peak exists outside the elution temperature range of 40°C to 75°C, or when the TREF curve has a single peak, the height at the elution temperature of 65°C is determined as A1 to obtain each value, and then calculate A H / A1.
[0327] <Fractometry Temperature>
[0328] 35℃ / 40℃ / 43℃ / 46℃ / 49℃ / 52℃ / 55℃ / 58℃ / 61℃ / 64℃ / 67℃ / 70℃ / 73℃ / 76℃ / 79℃ / 82℃ / 85℃ / 88℃ / 91℃ / 94℃ / 97℃ / 100℃ / 105℃ / 120℃
[0329] <Measurement conditions>
[0330]
[0331] -GPC analysis: The fraction eluted at each temperature in the previous TREF analysis was transferred to a GPC column of a GPC apparatus provided in a CFC apparatus, and then the molecular weight of the eluted molecules was measured according to the following measurement conditions.
[0332] Furthermore, from the measurement results, the weight average molecular weight (M) of the low crystalline polymer (excluding the soluble fraction (SF)) eluted in the region below 75° C., that is, in the region of elution temperature from 35° C. to 75° C. in the TREF curve was calculated. L ), and the weight average molecular weight (M) of the high crystalline polymer eluted in the region where the elution temperature is higher than 75°C H ).
[0333] <Measurement conditions>
[0334]
[0335] (7) F(T) and a
[0336] The polyolefins of the embodiments and comparative examples were subjected to DSC analysis in the same manner as in Experimental Example 1, and based on the DSC analysis results, F(T) and a were calculated respectively using the Mo method described in the literature (Li, Yu et al., Journal of Applied Polymer Science 138.2(2021):49652).
[0337] Specifically, the polyolefins prepared in Examples 1 to 4 and Comparative Example 1 were aliquoted into aluminum pans in amounts of 5 mg each, introduced into a DSC apparatus (DSC Q20 / RCS90 (manufactured by TA)), and heated to 160° C. at a rate of 10° C. / min and maintained for 5 minutes to remove the thermal history.
[0338] The obtained polyolefin was cooled to 20°C at cooling rates of 5°C / min, 10°C / min, 15°C / min and 20°C / min (N°C / min, where N=5, 10, 15 and 20) and maintained at 20°C for 5 minutes, and then the cooled polyolefin was heated again to 160°C at 10°C / min, and the change in melting enthalpy was measured.
[0339] In the temperature difference curve obtained as a result of DSC analysis, the crystallization peak between 30°C and 120°C was set as the analysis region, the total enthalpy value of the corresponding region was regarded as 100% relative crystallinity, and the peak point corresponding to 20% enthalpy value of the total enthalpy was determined as 20% relative crystallinity. The time (min) taken to reach the temperature corresponding to 20% relative crystallinity when cooled from 120°C at a cooling rate of N°C / min (where N=5, 10, 15 or 20) was calculated and determined as the crystallization completion time.
[0340] Specifically, in the temperature difference curve, the time (t 120 ), and the time taken to reach 20% relative crystallinity when cooled at each of 5°C / min, 10°C / min, 15°C / min and 20°C / min cooling rates (t 20 _N, where N = 5, 10, 15 or 20). The crystallization completion time (min) is determined by the time corresponding to the point of 120°C (t 120 ) and the time taken to reach 20% relative crystallinity, i.e., t 120 -t 20 _N value calculation.
[0341] A graph is prepared using the Log(t) data of the time taken to reach 20% relative crystallinity when cooled at a cooling rate of N°C / min (where N=5, 10, 15 or 20), and the log(Φ) data (Φ is the cooling rate (°C / min) value, Φ=5, 10, 15 and 20). When the graph is prepared, the crystallization completion time, e.g., the time taken to reach 20% relative crystallinity (log t) is plotted on the X-axis, and the cooling rate (logΦ) is plotted on the Y-axis. Figure 1 It is a graph showing the relationship between the time taken to reach 20% relative crystallinity, ie, crystallization completion time, and the cooling rate in differential scanning calorimeter (DSC) analysis of the polyolefins of Examples 1 to 4 and Comparative Example 1.
[0342] The plotted graph was fitted to a first-order linear relationship using data analysis software (Origin Pro, 9.1). In the obtained first-order linear relationship, the y intercept and slope were determined as F(T) and a, respectively.
[0343] Table 6
[0344]
[0345] Table 7
[0346]
[0347] As a result of the experiment, the polyolefins of Examples 1 to 4 showed low F(T) values and high a values compared to the polyolefins of Comparative Examples 1 to 6. From these results, it can be expected that the polyolefins of Examples 1 to 4 have no significant change in crystallization rate even under blown film processing conditions, and their relatively small sizes can form a crystalline structure resulting in low surface haze, resulting in excellent transparency.
[0348] In contrast, Comparative Example 1 exhibits a high F(T) due to the lack of fraction content in the high crystalline region, and Comparative Example 2 exhibits a high F(T) due to the low M LHowever, it has reduced drop impact strength.
[0349] Experimental Example 3
[0350] Films were produced using each of the polyolefins prepared in Examples and Comparative Examples, and then evaluated for drop weight impact strength and haze properties. The results are shown in Table 8 below.
[0351] (1) Film production
[0352] Based on the total weight of the polyolefin prepared in the embodiment or comparative example, 1500 ppm of an antioxidant (weight ratio of Songnox 1076 (Songwon): Songnox 1680 (Songwon) = 1:2) and 300 ppm of 3M Dynamar polymer processing additive FX5929 were added and mixed, and then extruded using a twin-screw extruder (TEK 30MHS, manufactured by SMPLATECH CO., with a diameter of 32 pi, L / D = 40) at an extrusion temperature of 190° C. and an extrusion rate of 35 kg / hr to prepare about 18 mg of a granular composition for producing a film.
[0353] The composition for producing a film prepared as above was extruded under the following film extrusion conditions to produce a film.
[0354] <Film extrusion conditions>
[0355] Single screw extruder (YOOJIN ENGINEERING, Blown Film M / C, 50pi)
[0356] Melting temperature (or extrusion temperature): 170℃
[0357] Die gap: 2.0mm
[0358] Mould diameter: 120mm
[0359] Blowing ratio: 2.5
[0360] Frost line height: maintained at 250mm to 260mm
[0361] Sample extrusion rate: 300g / min to 500g / min
[0362] Film thickness: 50μm
[0363] (2) Drop hammer impact strength
[0364] For the 50 μm thick film produced as described above, the drop weight impact strength was measured according to the ASTM D1709 [Method A] standard, repeated 20 times or more for each film sample, and then the average value was taken.
[0365] (3) Haze
[0366] The haze of the film was measured according to ISO 13468 standard for a 50 μm thick film produced as described above.
[0367] Table 8
[0368]
Claims
1. A polyolefin, The molecular weight distribution is 2.5 to 4, The crystallization difficulty (F(T)) calculated according to the Mo method after differential scanning calorimetry, and the ratio of the Avrami parameter to the Ozawa parameter (a) satisfy the following requirements (i) and (ii) under the condition of 20% relative crystallinity, and In the temperature-elution fractionation curve analyzed by cross-fraction chromatography, A H The peak height ratio of / A1 meets the following requirement (iii): (i) F(T)≤15 (ii) a>1.45 (iii)A H / A1≥1.8 In (iii), A H represents the peak height of the highest peak in the temperature-elution fractionation curve, and A1, when the lowest peak in the temperature increasing elution fractionation curve exists in the elution temperature range of 40°C to 75°C, it indicates the peak height of the lowest peak; and when the lowest peak in the temperature increasing elution fractionation curve does not exist in the elution temperature range of 40°C to 75°C, or when the lowest peak does not exist because the temperature increasing elution fractionation curve has a single peak, it indicates the height at the elution temperature of 65°C.
2. The polyolefin of claim 1, wherein F(T) and a are obtained by a process comprising the steps of: A step of differential scanning calorimetry analysis, wherein the polyolefin is introduced into a differential scanning calorimeter, cooled to 20°C at a cooling rate of N°C / min (where N=5, 10, 15 and 20), and maintained at 20°C for 5 minutes, and then the cooled polyolefin is heated again to 160°C at a rate of 10°C / min to measure the change in melting enthalpy; a step of calculating a crystallization completion time, which is a time taken to reach a temperature corresponding to a relative crystallinity of 20% when cooled from 120°C at a cooling rate of N°C / min (where N=5, 10, 15 or 20), wherein the relative crystallinity of 20% is determined by a point at which the enthalpy value is 20% when a crystallization peak between 30°C and 120°C in a temperature difference curve obtained as a result of differential scanning calorimetry analysis is set as an analysis region and a total enthalpy value of the corresponding region is regarded as 100% of the relative crystallinity; A step of obtaining a first order linear relationship by plotting the crystallization completion time (log t) calculated above on the X-axis and the cooling rate (log Φ) on the Y-axis and then performing curve fitting; and The y-intercept and slope of the resulting first-order linear relationship are determined as F(T) and a, respectively.
3. The polyolefin of claim 1, wherein F(T) is from 10 to 15, and a is from 1.46 to 1.
6.
4. The polyolefin according to claim 1, wherein A H / A1 is 1.8 to 3.
5. The polyolefin according to claim 1, wherein M L 130000 g / mol or more, which is the weight average molecular weight of the polymer eluted in the elution temperature region of 35°C to 75°C in the temperature rising elution fractionation curve by cross fraction chromatography, and the content ratio W is based on the total weight of all eluted fractions. L 35 wt % to 45 wt % or more, and M H is 70000 g / mol to 110000 g / mol, which is the weight average molecular weight of the polymer eluted in the elution temperature region above 75° C., and the content ratio W is based on the total weight of all eluted fractions. H 50 wt % to 60 wt %.
6. The polyolefin according to claim 1, wherein In the temperature-elution fractionation curve analyzed by cross-fraction chromatography, Te L is 60°C to 90°C, which is the elution temperature of the lowest peak, and Te H It is 80°C to 100°C, which is the elution temperature of the highest peak.
7. The polyolefin of claim 1, wherein the polyolefin has a density of 0.915 g / cc to 0.925 g / cc as measured according to ASTM D1505.
8. The polyolefin of claim 1, wherein the MI of the polyolefin is 2.16 0.5 g / 10 min to 1.5 g / 10 min, which is a melt index measured at a temperature of 190° C. under a load of 2.16 kg according to ASTM D 1238, and MI 21.6 The melt index is 10 to 50 g / 10 min, which is a melt index measured at a temperature of 190° C. under a load of 21.6 kg.
9. The polyolefin as claimed in claim 1, wherein the MFRR of the polyolefin is 20 to 30, which is obtained by measuring the melt index (MI) according to ASTM D1238 standard at a temperature of 190° C. under a load of 21.6 kg. 21.6 ) divided by the melt index (MI) measured at a temperature of 190°C under a load of 2.16 kg 2.16 ) obtained.
10. The polyolefin of claim 1, wherein the polyolefin is an ethylene / 1-hexene copolymer.
11. A film comprising the polyolefin of claim 1.
12. The film of claim 11, wherein the film has a dart impact strength of 1600 gf or more measured according to ASTM D 1709 Method A at a BUR of 2.3 to 3 and a film thickness of 50 μm and 65 μm, and a haze of 15% or less measured according to ISO 13468.
13. The film of claim 11, wherein the film is a blown film.