Two-component thermally conductive structural adhesive
Through the design of two-component thermally conductive adhesive, different proportions of thermally conductive fillers and reactive components are used to solve the problem of insufficient strength and adhesion of traditional adhesives at high temperatures, and high thermal conductivity and good adhesion are achieved. , improves the performance of the battery cooling system.
Patent Information
- Application Number
- CN202380028663.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-22
- Filing Date
- 2023-03-21
- Publication Date
- 2024-11-05
AI Technical Summary
In existing battery cooling systems, thermally conductive adhesives have challenges in achieving high thermal conductivity and good adhesion, especially at high temperatures, where traditional epoxy adhesives affect glass transformation due to the use of high molecular weight polyetheramines. Transition temperature and strength properties.
Using a two-component thermally conductive adhesive, the mixing ratio is adjusted to achieve a thermally conductive filler concentration of 65-85 wt% by using different proportions of thermally conductive filler in the resin component and hardener component and between 0.8:1 and 1.2:1 The adhesive strength and adhesion are improved by mixing at a volume ratio.
High thermal conductivity and good adhesion are achieved, ensuring that the battery unit maintains efficiency at high temperatures and avoids thermal runaway reactions, improving the overall performance of the battery cooling system.
Smart Images

Figure BDA0005049739520000061 
Figure BDA0005049739520000081 
Figure BDA0005049739520000101
Abstract
Description
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims priority to U.S. Provisional Patent Application No. 63 / 322,281, filed on March 22, 2022, which is incorporated by reference into this application. Background Art
[0003] Currently, there is a strong trend towards building electric drive vehicles to reduce fleet CO2 emissions. The combination of a growing car market and a growing market share for electric drive vehicles has led to a strong growth in the number of electric drive vehicles.
[0004] In order to provide a long driving range, a battery with a high energy density is required. Several battery strategies currently follow different detailed concepts, but the common point of all long-range battery concepts is the need to manage the heat generated during battery use. Thermally conductive adhesives are used to thermally connect and fix battery cells or modules in place to the cooling unit. Battery cells generate heat during charging and discharging operations. The battery cells need to be kept at an appropriate operating temperature (preferably 25°C-40°C) without losing efficiency and avoiding overheating that may cause dangerous thermal runaway reactions. For these reasons, active cooling is used. Usually a cooled water-ethylene glycol mixture is pumped through a channel that cools the metal base plate on which the battery cells / modules are placed. In order to connect these battery cell modules to the cooling plate, a thermally conductive adhesive is applied to bond the battery cell modules to the cooling plate. For cooling efficiency, a thermal conductivity of ≥1W / mK is required. In order to bond the battery module to the cooling plate, a high lap shear strength level of greater than 3MPa, more preferably greater than 5MPa, and most preferably greater than 7MPa is typically required.
[0005] Cooling plates and module housings are most often designed using aluminum without additional electrocoating protection. Aluminum is typically passivated by treatments such as by Ti / Zr coating, which results in excellent corrosion protection. Additionally, steel as a substrate is used by selected customers in cells that may be electrocoated in corrosion-prone areas or uncoated in dry areas. On such substrates, polyurethane adhesives typically have the challenge of establishing a strong, durable bond with an excellent failure mode. Optimal adhesion to metals can typically be achieved by applying epoxy adhesives.
[0006] For the easiest application and best mix quality, end users typically want an adhesive with a 1:1 mix ratio for automated applications. This is for a number of reasons, including
[0007] - Minimum impact of feeding errors,
[0008] - In case of the same size of feeder and packaging (bulk) of adhesive in a 1:1 ratio, the refilling time of the feeder and the bulk will occur at the same time, thus reducing downtime.
[0009] Two-component epoxy adhesives are typically prepared by a combination of an epoxide and an amine component. The typically used bisphenol A diglycidyl ether epoxy resin (DGBPA) has an epoxide equivalent weight typically between 170 and 190 g / mol of epoxide, while the typically used amines, such as the frequently used 4,7,10-trioxatridecane-1,13-diamine with a molecular weight of 220 g / mol and two primary amines, result in molecules such as triethylenetetramine with an active NH equivalent weight (NHEW) as low as 55 g / mol or even a NHEW of only 22 g / mol. In order to design an epoxy adhesive with an epoxide:NH ratio of about 1:1 or even a balanced one, a higher amount of very long polyetheramines (commonly known as Jeffamines) is typically used. These are commercially available as diamines with molecular weights up to 2000 g / mol (NH equivalent weight = 500 g / mol). This enables the formulation of adhesives with a mixing ratio of 2:1 or even 1:1. The use of such high molecular weight polyetheramines is not entirely desirable because they negatively affect glass transition temperature and strength properties, especially at high temperatures. In addition, the good electrical properties of epoxy adhesives derive from the specific properties of the epoxy resin within the adhesive. Therefore, the higher the epoxy resin content in the final cured matrix, the better the electrical properties. This is important because for some applications, at least 1.0 x 10 14 Volume resistivity in ohms / cm.
[0010] For most thermally conductive adhesives, to achieve thermal conductivity ≥ 1 W / mK, very high filler loadings of about 70 wt% are required when using aluminum hydroxide ATH. Adhesives are typically designed with symmetrical levels of inorganic filler in both the epoxide and amine components to achieve comparable rheology for both components. Summary of the invention
[0011] In a first aspect, a two-component thermally conductive adhesive is provided, comprising:
[0012] (A) a resin component, the resin component comprising:
[0013] (a1) at least one epoxy resin;
[0014] (a2) at least one reactive toughening agent;
[0015] (a3) at least one reactive silane;
[0016] (a4) at least one thermally conductive filler, in a concentration of [a4] (wt %) based on the total weight of Part A;
[0017] as well as
[0018] (B) a part B hardener component, the hardener component comprising:
[0019] (b1) at least one polyamine;
[0020] (b2) at least one catalyst capable of catalyzing the reaction of an amine with an epoxy group;
[0021] (b3) at least one thermally conductive filler, in a concentration of [b3] (wt %) based on the total weight of Part B;
[0022] Wherein, when used, part A and part B are mixed together in a volume ratio of 0.8:1 to 1.2:1 to form an adhesive mixture, and the concentration of the thermally conductive filler in the adhesive mixture is 65-85wt% based on the total weight of the adhesive mixture, and the ratio of [a4]:[b3] is 0.7 to 0.9.
[0023] In a second aspect, there is provided a method for producing an adhesive, the method comprising the steps of:
[0024] (1) providing a part A resin component, the resin component comprising:
[0025] (a1) at least one epoxy resin;
[0026] (a2) at least one reactive toughening agent;
[0027] (a3) at least one reactive silane;
[0028] (a4) at least one thermally conductive filler, in a concentration of [a4] (wt %) based on the total weight of Part A;
[0029] (2) providing a part B hardener component, the hardener component comprising:
[0030] (b1) at least one polyamine;
[0031] (b2) at least one catalyst capable of catalyzing the reaction of an amine with an epoxy group;
[0032] (b3) at least one thermally conductive filler, in a concentration of [b3] (wt %) based on the total weight of Part B;
[0033] (3) mixing part A and part B in a volume ratio of 0.8:1 to 1.2:1 to form an adhesive mixture to achieve a concentration of the thermally conductive filler in the adhesive mixture of 65-85 wt % based on the total weight of the adhesive mixture;
[0034] The ratio of [a4]:[b3] is 0.7 to 0.9.
[0035] In a third aspect, there is provided a method for adhering two substrates, the method comprising the steps of:
[0036] (1) providing a part A resin component, the resin component comprising:
[0037] (a1) at least one epoxy resin;
[0038] (a2) at least one reactive toughening agent;
[0039] (a3) at least one reactive silane;
[0040] (a4) at least one thermally conductive filler, in a concentration of [a4] (wt %) based on the total weight of Part A;
[0041] (2) providing a part B hardener component, the hardener component comprising:
[0042] (b1) at least one polyamine;
[0043] (b2) at least one catalyst capable of catalyzing the reaction of an amine with an epoxy group;
[0044] (b3) at least one thermally conductive filler, in a concentration of [b3] (wt %) based on the total weight of Part B;
[0045] (3) mixing part A and part B in a volume ratio of 0.8:1 to 1.2:1 to form an adhesive mixture to achieve a concentration of the thermally conductive filler in the adhesive mixture of 65-85 wt % based on the total weight of the adhesive mixture;
[0046] The ratio of [a4]:[b3] is 0.7 to 0.9;
[0047] (4) applying the adhesive mixture to at least one substrate;
[0048] (5) placing a second substrate in bonding contact with the adhesive mixture; and
[0049] (6) Allow the adhesive mixture to cure. DETAILED DESCRIPTION
[0050] The inventors have surprisingly found that the epoxy component (A component) and the amine component (B component) of a two-component epoxy adhesive can be filled with significant deviations of more than a 10% by weight difference in filler volume content between the two components. The filler content in part A is reduced to, for example, 60-65% by weight, which enables an increase in the content of the organic epoxy matrix in part A, while the part B filler loading is increased to, for example, 75%-80%. As a result, even if the full adhesive is a 1:1 mixing ratio by weight, the ratio of organic compounds is very close to a 2:1 mixing ratio. The resulting adhesive has very high strength and very good adhesion to metal surfaces.
[0051] Definitions and Abbreviations
[0052] ATH Aluminum Hydroxide
[0053] PTMEG Poly(tetramethylene glycol)
[0054] DGEBA Bisphenol A diglycidyl ether
[0055] polyTHF poly(tetrahydrofuran) glycol
[0056] PBD Poly(butadiene) glycol
[0057] DBTL Dibutyltin dilaurate
[0058] HDI Hexamethylene diisocyanate
[0059] PTHF Poly(tetrahydrofuran)
[0060] MDI Methylene diphenyl diisocyanate
[0061] Molecular weights of polymers as reported herein are reported as number average or weight average molecular weight in Daltons (Da) as determined by size exclusion chromatography (SEC). If not otherwise stated, molecular weight refers to number average molecular weight.
[0062] Two-component adhesives consist of Part A (resin component) and Part B (hardener component). When used, Part A and Part B are mixed in the desired ratio and then applied to one or more substrates.
[0063] Component A
[0064] Component A contains:
[0065] (a1) at least one epoxy resin;
[0066] (a2) at least one reactive toughening agent;
[0067] (a3) at least one reactive silane;
[0068] (a4) at least one thermally conductive filler, in a concentration of [a4] (wt %) based on the total weight of Part A;
[0069] Each of these components will be discussed in turn.
[0070] At least one epoxy resin (a1)
[0071] Part A of the two-component adhesive contains at least one epoxy resin. Epoxy resins useful in the adhesive composition include a variety of curable epoxy compounds and combinations thereof. Useful epoxy resins include liquids, solids and mixtures thereof, and liquids are useful. Typically, the epoxy compound is an epoxy resin (also referred to as a monoepoxide or polyepoxide). The polyepoxide useful herein can be monomeric (e.g., diglycidyl ether of bisphenol A, diglycidyl ether of bisphenol F, diglycidyl ether of tetrabromobisphenol A, epoxy resins based on phenolic formaldehyde, and trifunctional epoxy resins), higher molecular weight resins (e.g., diglycidyl ether of bisphenol A improved with bisphenol A) or polymerized unsaturated monoepoxides (e.g., glycidyl acrylate, glycidyl methacrylate, allyl glycidyl ether, etc.) to homopolymers or copolymers. Most desirably, the epoxy compound contains at least one side-connected or terminal 1,2 epoxy group (i.e., ortho-epoxy group) / molecule on average. The solid epoxy resin that can be used can contain or preferably be mainly based on bisphenol A. Some epoxy resins include, for example, DER 330, DER 331, and DER 671, all commercially available from The Dow Chemical Company. The monoepoxides useful herein may be reactive diluents bearing only one 1,2-epoxy group, such as, for example, p-tert-butylphenyl glycidyl ether (Araldite DY-T), glycidyl ethers of long chain aliphatic alcohols such as the monoglycidyl ether of a mixture of C12 and C14 alcohols (Araldite DY-E), or reactive diluents bearing multiple 1,2-epoxy groups, such as, for example, the reaction product of epichlorohydrin and polypropylene glycol (DER 732).
[0072] A preferred epoxy resin has the general formula:
[0073]
[0074] wherein n is in the range of 0 to about 25.
[0075] Exemplary epoxy resins have an epoxy equivalent weight in the range of about 170 to 195 g / mol.
[0076] The combination of epoxy resins can be used to adjust the characteristics of epoxy adhesives. In compositions and methods, epoxy adhesives can include any amount of epoxy resins. Preferably, liquid and / or solid epoxy resins include epoxy adhesives greater than or about 20wt%, more preferably greater than or about 25wt%, 30wt% or 35wt%. Preferably, liquid and / or solid epoxy resins include epoxy adhesives less than or about 65wt%, more preferably less than or about 55wt% or 45wt%. Other amounts are shown in examples. Also disclosed is the scope formed from these numerical pairs (e.g., 25 to 35wt%, 25 to 65wt%, 30 to 38wt% (adhesive AA)).
[0077] When using the combination of liquid epoxy resin and solid epoxy resin, any ratio can be used, and can be determined by those of ordinary skill in the art. In order to obtain suitable viscosity, it is usually useful that the weight ratio of liquid epoxy resin and solid epoxy resin is greater than 50:50. The epoxy adhesive composition can include liquid epoxy resin and solid epoxy resin in a ratio of or greater than 55:45, 65:35 or 70:30. The epoxy adhesive composition can include liquid epoxy resin and solid epoxy resin in a ratio of or less than 100:0, 99:1, 90:10 or 85:10. Other ratios are shown in the examples. Also disclosed is the scope formed from these numerical pairs (e.g., 50:50 to 100:0, 65:35 to 82:18 (adhesive AU)).
[0078] Preferred epoxy resins include:
[0079] Epoxides 1. Liquid reaction products of epichlorohydrin and bisphenol A, the liquid reaction product having an epoxy equivalent weight of 182-192 g / eq (as measured according to ASTM D-1652), an epoxy percentage of 22.4%-23.6% (as measured according to ASTM D-1652), an epoxy group content of 5200-5500 mmol / kg (as measured according to ASTM D-1652) and a viscosity of 4000-14000 mPas at 25° C. (as measured according to ASTM D-445), for example DER 331;
[0080] Epoxides 2. Solid epoxy resins, which are low molecular weight solid reaction products of epichlorohydrin and bisphenol A, having an epoxy equivalent weight of 475-550 g / eq (as measured according to ASTM D-1652), an epoxy percentage of 7.8%-9.1% (as measured according to ASTM D-1652), an epoxy group content of 1820-2110 mmol / kg (as measured according to ASTM D-1652) and a melt viscosity of 400-950 mPas at 150° C. (as measured according to ASTM D-4287), for example DER671;
[0081] Epoxide 1 is particularly preferred.
[0082] The epoxy resin may be present in the adhesive at 20 to 40 wt %, more preferably 25 to 35 wt %, particularly preferably 26 to 34 wt %, based on the total weight of part A of the adhesive.
[0083] In one embodiment, the epoxy resin is Epoxide 1, which is used at 26 to 29 wt % based on the total weight of Part A of the adhesive.
[0084] In one embodiment, part A has an epoxy equivalent weight per liter of 1.50 to 4.50, more preferably 2.50 to 3.5, particularly preferably 3.00 to 3.30 mmol / l.
[0085] Reactive toughening agent (a2)
[0086] Part A of the two-component adhesive comprises at least one reactive toughening agent.
[0087] Reactive tougheners (sometimes called tougheners) are elastomeric molecules having end groups that react with epoxy resins or epoxy resin hardeners in the presence of a catalyst, or that can be cleaved to reveal end groups that react with epoxy resins or epoxy resin hardeners in the presence of a catalyst.
[0088] Preferred toughening agents for use in the compositions of the present invention are reactive polyurethane based toughening agents prepared by reacting at least one polyol and optionally a poly(butadiene) diol with a polyisocyanate in the presence of a polyurethane catalyst, optionally followed by chain extension with a dihydric phenol, and end-capping with a phenol, an oxime, or a molecule having Formula I:
[0089]
[0090] Where R 1 and R 2 are independently selected from hydrogen and C1 to C6 alkyl, n is an integer from 1 to 2, and R 3 It is a C1 to C6 alkyl group.
[0091] In another preferred embodiment, the terminal group or the end-capping group is a phenol, particularly preferably a dihydric phenol or a monohydric phenol, particularly preferably O,O'-diallylbisphenol A or cardanol.
[0092] If the terminal group is a molecule of formula I, then preferably, R 1 and R 2 are independently selected from H and C1 to C4 alkyl, more preferably H and C1 to C2 alkyl, particularly preferably, R 1 and R 2 It's H.
[0093] In a preferred embodiment, R 3 It is a C1 to C4 alkyl group, more preferably a C1 to C2 alkyl group.
[0094] In a preferred embodiment, n is 1.
[0095] In another preferred embodiment, R 1 and R 2 Yes H, R 3 is ethyl or methyl, especially ethyl, and n is 1. In a particularly preferred embodiment, the end-capping molecule is CPEE.
[0096] At least one polyol is preferably a diol or a triol or a mixture of the two. Diols are particularly preferred. In a preferred embodiment, at least one polyol is a poly(alkylene oxide) glycol. Preferred poly(alkylene oxide) glycols are selected from poly(C2-C6 alkylene oxide) glycols, in particular poly(tetramethylene oxide) glycol ("PTMEG"), poly(oxetane) glycol ("PO3G"), and mixtures of these. Poly(alkylene oxide) glycols preferably have a molecular weight in the range of 1,000 to 2,500 Da, more preferably 1,000 to 2,000 Da. PTMEG is particularly preferred. Preferably, PTMEG has a molecular weight in the range of 1,000 to 2,500 Da, more preferably 1,000 to 2,000 Da.
[0097] In a preferred embodiment, the PBD is contained within the toughening agent backbone.
[0098] In another preferred embodiment, chain extension is performed using dihydric phenols.
[0099] In another preferred embodiment, PBD is included and a dihydric phenol is used for chain extension.
[0100] In another preferred embodiment, no PBD is included.
[0101] In another preferred embodiment, no chain extension is performed.
[0102] In another preferred embodiment, no PBD is included and no chain extension is performed.
[0103] If used, PBD preferably has a molecular weight in the range of 1,000 to 3,500 Da, more preferably 2,800 Da.
[0104] The polyisocyanate is not particularly limited. It may be aromatic or aliphatic. Examples of suitable polyisocyanates include toluene diisocyanate, 1,6-hexamethylene diisocyanate ("HMDI" or "HDI"), methylene diphenyl diisocyanate ("MDI"), 2,2,4-trimethylhexamethylene diisocyanate (TMDI) and isophorone diisocyanate (IPDI). HMDI is particularly preferred.
[0105] The polyurethane catalyst is not particularly limited. Dibutyltin dilaurate ("DBTL") and metal carboxylates such as bismuth carboxylates and / or zinc carboxylates are particularly preferred. The catalyst is preferably used at 0.01 to 0.5 wt%, more preferably 0.1 wt%, based on the total weight of the toughening agent. In a preferred embodiment, the catalyst is a mixture of bismuth carboxylates and zinc carboxylates, which is used at 0.1 wt% based on the total weight of the toughening agent.
[0106] Optional chain extension is performed with a dihydric phenol. O,O'-diallyl bisphenol A ("ODBA") is particularly preferred. The dihydric phenol is preferably used at 2 to 10 wt%, more preferably 5 to 8 wt%, particularly preferably 7 wt%, based on the total weight of the toughening agent. Alternatively, the chain extender can be used with the polyol in a molar ratio of 0:1 to 1:1, more preferably 0:1 to 0.8:1, particularly preferably 0.6:1 to 0.8:1.
[0107] The reaction of the diol, polyisocyanate and diphenol chain extender (if used) results in the molecules before end-capping being end-capped with NCO groups. End-capping is then carried out with phenol, diphenol or a molecule of formula I. If a molecule of formula I is used as end-capping group, a catalyst is used, such as, for example, at least one metal carboxylate, in particular a zinc carboxylate and / or a bismuth carboxylate.
[0108] Based on the total weight of the toughener, the toughener preferably contains 40 to 90 wt% of a polyol, in particular a poly(alkylene oxide) glycol, more preferably 45 to 85 wt%, more particularly preferably 50 to 85 wt%. Particularly preferably, based on the total weight of the toughener, the toughener contains 40 to 90 wt% of PTMEG, more preferably 45 to 85 wt%, more particularly preferably 50 to 85 wt%.
[0109] If present, PBD is preferably present in the toughening agent at 10 to 25 wt% PBD, more preferably 12 to 18 wt% based on the total weight of the toughening agent, with PBD having a molecular weight of 2,800 Da being particularly preferred.
[0110] In a preferred embodiment, the toughening agent comprises toluene diisocyanate as the polyisocyanate, poly(propylene oxide) diol as the polyol, and cardanol as the capping group.
[0111] In another preferred embodiment, the toughening agent comprises hexamethylene diisocyanate as polyisocyanate, poly(tetramethylene furan)diol as polyol, and O,O'-diallylbisphenol A as chain extender and end-capping group.
[0112] The preferred method for preparing the toughening agent is the following process:
[0113] 1. First reaction step: Heat the polyol, preferably poly(alkylene oxide) glycol (more preferably PTMEG) and PBD (if used) to 120°C-130°C. Heat the mixture under vacuum for 25-35 minutes. Cool the mixture to 50°C-70°C. When the temperature reaches 50°C-70°C, add the diisocyanate (preferably HDI) and mix the mixture for 2-5 minutes. Then add a polyurethane catalyst (e.g., an organic tin compound) and react the mixture at 75°C-90°C (bath temperature) for 40-50 minutes under a neutral atmosphere (e.g., nitrogen, argon).
[0114] 2. Second reaction step: Add chain extender (if used) and stir the mixture under neutral atmosphere (eg nitrogen, argon) at 85-95° C. (bath temperature) for 50-70 minutes.
[0115] 3a. Third reaction step (if using a molecule having formula I as an end group): Add a capping molecule having formula I (e.g., CPEE) and stir the mixture under a neutral atmosphere (e.g., nitrogen, argon) at 85° C.-95° C. (bath temperature) for 80-95 minutes. Stir the mixture at 95° C. for 10 minutes under vacuum to degas.
[0116] 3b. Third reaction step (if using dihydric phenol or monohydric phenol as end group): add monohydric phenol or dihydric phenol and stir the mixture under neutral atmosphere (e.g. nitrogen, argon) at 85°C-95°C (bath temperature) for 80-95 minutes. Stir the mixture at 95°C for 10 minutes under vacuum to degas.
[0117] The reactive toughening agent is preferably present in part A at 2-10 wt %, based on the total weight of part A, more preferably 3-8 wt %, particularly preferably 4-6 wt %.
[0118] In a preferred embodiment, the reactive toughening agent is a polyurethane-based toughening agent and is present in an amount of 2-10 wt %, based on the total weight of Part A, more preferably 3-8 wt %, particularly preferably 4-6 wt %.
[0119] In another preferred embodiment, the reactive toughening agent is prepared by reacting at least one polyol and optionally a poly(butadiene) diol with a polyisocyanate in the presence of a polyurethane catalyst, optionally followed by chain extension with a dihydric phenol, and end-capping with a phenol, an oxime, or a molecule having Formula I:
[0120]
[0121] Where R 1 and R 2 are independently selected from hydrogen and C1 to C6 alkyl, n is an integer from 1 to 2, and R 3 is a C1 to C6 alkyl group, and the reactive toughening agent is present in an amount of 2-10 wt %, more preferably 3-8 wt %, particularly preferably 4-6 wt %, based on the total weight of part A.
[0122] Reactive silane (a3)
[0123] Component A comprises at least one reactive silane.
[0124] A reactive silane is any silane comprising a hydrolyzable silylalkoxy group covalently bonded to a mercapto group, a primary or secondary amine group, or an epoxy group.
[0125] In a preferred embodiment, the reactive silane is a mercaptosilane. Preferably, the mercaptosilane is selected from mercaptoalkyl (trialkoxy) silanes and mercaptoalkyl (methyl-dialkoxy) silanes. Examples of suitable mercaptosilanes include γ-mercaptopropyl trimethoxy silane, γ-mercaptopropyl (methyl-dimethoxy) silane, wherein γ-mercaptopropyl trimethoxy silane is particularly preferred.
[0126] In another preferred embodiment, the reactive silane is an aminosilane. Preferably, the aminosilane is selected from aminoalkyl (trialkoxy) silanes and aminoalkyl (methyl-dialkoxy) silanes. The example of suitable aminosilanes includes bis-(trimethoxysilyl propyl) amine, (3-aminopropyl) trimethoxysilane, (3-aminopropyl) triethoxysilane, N-(2-aminoethyl)-3-aminopropyl trimethoxysilane, trimethoxysilyl propyl diethylenetriamine, wherein bis-(trimethoxysilyl propyl) amine, (3-aminopropyl) trimethoxysilane are particularly preferred.
[0127] In another preferred embodiment, the reactive silane is an epoxy silane. Preferably, the epoxy silane is selected from glycidyloxyalkyl (trialkoxy) silanes and glycidyloxyalkyl (methyl-dialkoxy) silanes. Examples of suitable epoxy silanes include tris (diethylene glycol methyl ether) silyl propylene glycidyl ether, (3-glycidyloxypropyl) trimethoxysilane, (3-glycidyloxypropyl) triethoxysilane, 3-glycidyloxypropyl methyl dimethoxysilane, 3-glycidyloxypropyl methyl diethyl silane, 2- (3,4-epoxycyclohexyl) -ethyl trimethoxysilane, 2- (3,4-epoxycyclohexyl) -ethyl triethoxysilane, wherein tris (diethylene glycol methyl ether) silyl propylene glycidyl ether is particularly preferred.
[0128] The reactive silane is preferably present in component A in an amount of 0.25-2.25 wt %, based on the total weight of component A, more preferably 0.5 to 1.75 wt %, particularly preferably 0.75 to 1.5 wt %.
[0129] In a preferred embodiment, the reactive silane is selected from glycidyloxyalkyl(trialkoxy)silanes and glycidyloxyalkyl(methyl-dialkoxy)silanes and is present at 0.25-2.25 wt %, more preferably 0.5 to 1.75 wt %, particularly preferably 0.75 to 1.5 wt %, based on the total weight of component A.
[0130] In a preferred embodiment, the reactive silane is tri(diethylene glycol methyl ether) silyl propylene glycidyl ether and is present at 0.25-2.25 wt %, based on the total weight of component A, more preferably 0.5 to 1.75 wt %, particularly preferably 0.75 to 1.5 wt %.
[0131] Thermally conductive filler (a4, b3)
[0132] The thermally conductive fillers used as a4 and b3 are not particularly limited. Suitable thermally conductive fillers are those having a thermal conductivity greater than 5 W / m°K, greater than 10 W / m°K, or greater than 15 W / m°K. Examples of thermally conductive fillers include alumina, alumina trihydrate or aluminum hydroxide, silicon carbide, boron nitride, diamond and graphite, or mixtures thereof. Particularly preferred are aluminum hydroxide (ATH) and aluminum oxide, with ATH being most preferred.
[0133] In a preferred embodiment, the thermally conductive filler has a broad particle size distribution characterized by a D90 / D50 ratio of 3 or about 3 or more. Particularly preferably, the thermally conductive filler is ATH or alumina having a broad particle size distribution characterized by a D90 / D50 ratio of 3 or about 3 or more, most preferably ATH.
[0134] Also preferred are thermally conductive fillers having a bimodal particle size distribution. A bimodal distribution is when, for example, the ratio D 90 / D 50 When the particle size is 3 or about 3 or more, more preferably 5 or about 5 or more, and more particularly preferably 9 or about 9 or more. For example, the particle has a D of 5 to 20 microns. 50 and 70 to 90 μm D 90 , especially 7-9 micron D 50 and D of 78-82 μm 90 The particle size can be determined using laser diffraction. For ATH, a suitable solvent is deionized water containing a dispersing aid such as Na4P2O7×10H2O, preferably containing the dispersing aid at 1 g / l. Alumina and ATH having a bimodal distribution, especially ATH, are preferred.
[0135] The thermally conductive filler is present in the final adhesive at a concentration of 65-85 wt % based on the total weight of the adhesive.The thermally conductive filler is preferably present in the final adhesive at a concentration that yields a thermal conductivity of at or about 1.1 W / mK or greater.
[0136] The thermally conductive filler is present in both part A (a4) and part B (b3), and the ratio of [a4]: [b3] is 0.7 to 0.9. In preferred embodiments, the ratio of [a4]: [b3] is 0.72 to 0.87, 0.7 to 0.8, or more preferably between 0.73 and 0.87.
[0137] In a preferred embodiment, the thermally conductive filler is used in part (A) at a concentration of 50-80 wt %, more preferably 55-65 wt %, based on the total weight of part A.
[0138] In another preferred embodiment, the thermally conductive filler is used in part (B) at 70-90 wt%, more preferably 75 to 85 wt%, based on the total weight of part (B).
[0139] In another preferred embodiment, the thermally conductive filler is ATH and is used in part (A) at a concentration of 50-80 wt %, more preferably 55-65 wt %, based on the total weight of part A.
[0140] In another preferred embodiment, the thermally conductive filler is ATH and is used in part (B) at 70-90 wt%, more preferably 75 to 85 wt%, based on the total weight of part (B).
[0141] In a preferred embodiment, the thermally conductive filler is used in part (A) at a concentration of 50-80 wt%, more preferably 55-65 wt%, based on the total weight of part A, and in part (B) at 70-90 wt%, more preferably 75 to 85 wt%, based on the total weight of part (B). In a particularly preferred embodiment, the thermally conductive filler is used in part A at 60 wt%, based on the total weight of part A, and in part B at 80 wt%, based on the total weight of part B.
[0142] In a particularly preferred embodiment, the thermally conductive filler is a material having a D of 8 or about 8 or greater. 90 / D 50 ATH of the ratio is used in part (A) at a concentration of 50-80 wt %, more preferably 55-65 wt %, based on the total weight of part A.
[0143] In another preferred embodiment, the thermally conductive filler has a D of 8 or about 8 or more. 90 / D 50 The ATH is preferably used in part (B) at a ratio of 70 to 90 wt%, more preferably 75 to 85 wt%, based on the total weight of part (B).
[0144] In a particularly preferred embodiment, the thermally conductive filler is a material having a D of 8 or about 8 or greater. 90 / D 50 The ratio of ATH is 60 wt % based on the total weight of part A and 80 wt % based on the total weight of part B in part A.
[0145] In a particularly preferred embodiment, the thermally conductive filler is a material having a D of 8 or about 8 or greater. 90 / D 50 The ATH of the ratio is used in part (A) at a concentration of 50-80 wt%, more preferably 55-65 wt%, based on the total weight of part A, and in part (B) at a concentration of 70-90 wt%, more preferably 75 to 85 wt%, based on the total weight of part (B). In a particularly preferred embodiment, the thermally conductive filler is a thermally conductive filler having a D of 8 or about 8 or more. 90 / D 50 The ratio of ATH is 60 wt % based on the total weight of part A and 80 wt % based on the total weight of part B in part A.
[0146] Other ingredients of component A
[0147] Component A may contain additional optional ingredients such as, for example:
[0148] Additional impact modifiers such as:
[0149] Rubber modifier, such as an adduct formed by the reaction of an epoxy resin and a carboxyl-terminated butadiene acrylonitrile rubber, preferably 0-30 wt% based on the total weight of Part A
[0150] Silicone toughening agent, preferably 0-30w% based on the total weight of Part A
[0151] Core-shell rubber toughener, preferably 0-30w% based on the total weight of Part A
[0152] The phosphoric acid-modified epoxy resin preferably comprises 0-15 wt % based on the total weight of Part A.
[0153] One or more silane adhesion promoters, such as tri(diethylene glycol methyl ether) silyl acrylic glycidyl ether.
[0154] Monofunctional, difunctional and trifunctional epoxy reactive diluents such as dihydric phenols, monohydric phenols such as cardanol, C 12-14 -monoglycidyl ether of alcohol, (trimethylolpropane triglycidyl ether) resin and diglycidyl ether of cyclohexanedimethanol.
[0155] Plasticizers, such as phthalates and dialkylnaphthalenes, in particular dialkyl phthalates, for example diisononyl phthalate, and dialkylnaphthalenes, such as diisopropylnaphthalene.
[0156] Reinforcers, and fillers, such as glass (fibers, flakes, microspheres), carbon fibers, graphite, carbon black, wollastonite (especially high aspect ratio wollastonite), calcium carbonate, TiO2, fumed silica, and mixtures of any of these. Reinforcers and / or fillers are preferably used in an amount of 0-15 wt% based on the total weight of Part A excluding the above-mentioned thermally conductive fillers.
[0157] Flame retardants and synergists, such as phosphorus-based and nitrogen-based flame retardants. Examples include melamine polyphosphate, melamine pyrophosphate, melamine cyanurate, aluminum dialkylphosphinates such as aluminum diethylphosphinate. If used, flame retardants and synergists are present in 0 to 10 wt% based on the total weight of component A.
[0158] Component B
[0159] Component B contains:
[0160] (b1) at least one polyamine;
[0161] (b2) at least one catalyst capable of catalyzing the reaction of an amine with an epoxy group;
[0162] (b3) at least one thermally conductive filler, in a concentration of [b3] (wt %) based on the total weight of Part B;
[0163] Each of these components will be discussed in turn.
[0164] At least one polyamine (b1)
[0165] Component B includes at least one polyamine capable of crosslinking with epoxy groups on the epoxy resin. Polyamines include molecules having two or more amine groups.
[0166] Preferred polyamines include secondary and primary amines, particularly polymeric amines, low molecular weight amines, and combinations thereof.
[0167] In a preferred embodiment, the polyamine comprises a polyetheramine, i.e. a molecule having a polyether backbone with terminal amine groups. Also preferred is the reaction product of a stoichiometric excess of an amine prepolymer and an epoxy resin. The amine prepolymer can be any amine prepolymer having at least two amine groups to allow crosslinking to occur. The amine prepolymer comprises primary and / or secondary amine groups, and preferably comprises primary amine groups. Suitable amine prepolymers include polyether diamines and polyether triamines, and mixtures thereof.
[0168] The polyetheramine can be linear, branched, or a mixture. Branched polyetheramines are preferred. Polyetheramines of any molecular weight can be used, and molecular weights in the range of 200-6000 or higher are suitable. The molecular weight can be higher than 1000, or more preferably higher than 3000. Molecular weights of 3000 or 5000 are preferred.
[0169] Examples of suitable commercially available polyamines include:
[0170]
[0171]
[0172] In a preferred embodiment, the polyamine of component B comprises a mixture of TETA and a difunctional primary amine having an average molecular weight of about 2000 and having the following general structure:
[0173] Where X≈33.
[0174] The concentration of the polyamine in component B will depend on the desired degree of cure in the cured adhesive and also on the desired mixing ratio of component A to component B. In a preferred embodiment, in which the mixing ratio (volume) of component A to component B is 0.8:1 to 1.2:1, in particular 1:1, the NH equivalent / liter component B is in the range of 1.5 to 4.50 mol / l, more preferably in the range of 2.50 to 3.75 mol / l, particularly preferably in the range of 3.00-3.40 mol / l.
[0175] In a preferred embodiment, the total amine content in component B is 5 to 18 wt %, based on the total weight of component B, more preferably 7 to 15 wt %, particularly preferably 9 to 13 wt %.
[0176] Catalyst (b2) capable of catalyzing the reaction between amine and epoxy group
[0177] Component B contains a catalyst capable of catalyzing the reaction of amines with epoxy groups. Suitable catalysts may be Lewis acids or Lewis bases.
[0178] Examples of suitable catalysts are ureas and / or tertiary amines, for example p-chlorophenyl-N,N-dimethylurea (monuron), 3-phenyl-1,1-dimethylurea (benzalkonium), 3,4-dichlorophenyl N,N-dimethylurea (diuron), N-(3-chloro-4-methylphenyl)-N',N'-dimethylurea 25 (chlorotoluron), tertiary acrylamides or alkyleneamines such as benzyldimethylamine, 2,4,6-tris(dimethylaminomethyl)phenol, piperidine or its derivatives, various aliphatic urea compounds (as described in EP1916272); C1-C 12 Alkylene imidazoles or N-aryl imidazoles are suitable, such as 2-ethyl-2-methyl imidazole, or N-butyl imidazole and 6-caprolactam, especially 2,4,6-tris(dimethylaminomethyl)phenol incorporated into a poly(p-vinylphenol) matrix (as described in European Patent EP0197892), or 2,4,6-tris(dimethylaminomethyl)phenol incorporated into a phenolic resin, including those described in US 4,701,378. Particularly preferred are tertiary amines, especially tris-2,4,6-tris(dimethylaminomethyl)phenol.
[0179] The catalyst is preferably used in an amount of 0.1 to 6 wt %, based on the total weight of component B, more preferably 2 to 5 wt %, particularly preferably 3 wt % or 4 wt %.
[0180] In a preferred embodiment, the epoxy curing catalyst is 2,4,6-tris(dimethylaminomethyl)phenol, which is used at 2 to 5 wt % based on the total weight of component B.
[0181] Other ingredients of component B
[0182] Component B may contain additional optional ingredients such as:
[0183] One or more silane adhesion promoters, such as N-(n-butyl)-3-aminopropyltrimethoxysilane.
[0184] Plasticizers, such as phthalates and dialkylnaphthalenes, in particular dialkyl phthalates, for example diisononyl phthalate, and dialkylnaphthalenes, such as diisopropylnaphthalene.
[0185] Reinforcement agents, and fillers, such as glass (fibers, flakes, microspheres), carbon fibers, graphite, carbon black, wollastonite (especially high aspect ratio wollastonite), calcium carbonate, TiO2, fumed silica, and mixtures of any of these. Reinforcement agents and / or fillers are preferably used in an amount of 0-15 wt%, more preferably 0-10 wt%, based on the total weight of Part B.
[0186] Curing accelerators, such as p-chlorophenyl-N,N-dimethylurea (monuron), 3-phenyl-1,1-dimethylurea (benzalkonium), 3,4-dichlorophenyl N,N-dimethylurea (diuron), N-(3-chloro-4-methylphenyl)-N',N'-dimethylurea 25 (chlorotoluron), tertiary acrylamide or alkylene amines such as benzyldimethylamine, 2,4,6-tris(dimethylaminomethyl)phenol, piperidine or its derivatives, various aliphatic urea compounds (such as described in EP1916272); C1-C 12 Alkylene imidazoles or N-aryl imidazoles are suitable, such as 2-ethyl-2-methyl imidazole, or N-butyl imidazole and 6-caprolactam, especially 2,4,6-tris(dimethylaminomethyl)phenol incorporated into a poly(p-vinylphenol) matrix (as described in European Patent EP0197892), or 2,4,6-tris(dimethylaminomethyl)phenol incorporated into a phenolic resin, including those described in US 4,701,378. Particularly preferred are tertiary amines, especially tris-2,4,6-tris(dimethylaminomethyl)phenol. If used, the curing accelerator is preferably present in an amount of 0 to 10 wt % based on the total weight of component B.
[0187] Flame retardants and synergists, such as phosphorus-based and nitrogen-based flame retardants. Examples include melamine polyphosphate, melamine pyrophosphate, melamine cyanurate, aluminum dialkylphosphinates such as aluminum diethylphosphinate. If used, flame retardants and synergists are present in 0 to 10 wt% based on the total weight of component B.
[0188] Curing adhesive
[0189] In one aspect, there is provided a cured adhesive obtained by mixing components A and B as described herein and curing the resulting mixture.
[0190] Components A and B may be mixed by any method that provides a homogeneous mixture relatively quickly. In a preferred embodiment, mixing is achieved using a static mixer when dispensing component A and component B through a nozzle.
[0191] The mixing ratio A:B of component A and component B is 0.8:1 to 1.2:1, more preferably 1:1.
[0192] Method for producing an adhesive
[0193] In another aspect, there is provided a method for producing an adhesive, the method comprising the steps of:
[0194] (1) providing a part A resin component, the resin component comprising:
[0195] (a1) at least one epoxy resin;
[0196] (a2) at least one reactive toughening agent;
[0197] (a3) at least one reactive silane;
[0198] (a4) at least one thermally conductive filler, in a concentration of [a4] (wt %) based on the total weight of Part A;
[0199] (2) providing a part B hardener component, the hardener component comprising:
[0200] (b1) at least one polyamine;
[0201] (b2) at least one catalyst capable of catalyzing the reaction of an amine with an epoxy group;
[0202] (b3) at least one thermally conductive filler, in a concentration of [b3] (wt %) based on the total weight of Part B;
[0203] (3) mixing part A and part B in a volume ratio of 0.8:1 to 1.2:1 to form an adhesive mixture to achieve a concentration of the thermally conductive filler in the adhesive mixture of 65-85 wt % based on the total weight of the adhesive mixture;
[0204] The ratio of [a4]:[b3] is 0.7 to 0.9.
[0205] The preferred embodiments of the adhesive described herein are equally applicable to the method of making the adhesive.
[0206] The mixing in step (3) can be performed by any method that provides a homogeneous mixture relatively quickly. In a preferred embodiment, mixing is achieved using a static mixer when dispensing component A and component B through a nozzle.
[0207] In a preferred embodiment, the epoxy equivalents per liter of fraction A and the NH equivalents per liter of fraction B are in the range of 0.8:1 to 1.2:1.
[0208] In an embodiment, the volume ratio in step (3) is 1:1.
[0209] In another embodiment, the ratio of [a4]:[b3] is 0.60 to 0.90.
[0210] In an embodiment of the method, the volume ratio in step (3) is 1:1, and the ratio of [a4]:[b3] is 0.65 to 0.85.
[0211] In an embodiment of the method, the volume ratio in step (3) is 1:1, the ratio of [a4]:[b3] is 0.65 to 0.85, and the ratio of the epoxy equivalent of part A to the NH equivalent of part B is in the range of 0.8:1 to 1.2:1.
[0212] Method for bonding two substrates
[0213] In another aspect, a method for adhering two substrates is provided, the method comprising the steps of:
[0214] (1) providing a part A resin component, the resin component comprising:
[0215] (a1) at least one epoxy resin;
[0216] (a2) at least one reactive toughening agent;
[0217] (a3) at least one reactive silane;
[0218] (a4) at least one thermally conductive filler, in a concentration of [a4] (wt %) based on the total weight of Part A;
[0219] (2) providing a part B hardener component, the hardener component comprising:
[0220] (b1) at least one polyamine;
[0221] (b2) at least one catalyst capable of catalyzing the reaction of an amine with an epoxy group;
[0222] (b3) at least one thermally conductive filler, in a concentration of [b3] (wt %) based on the total weight of Part B;
[0223] (3) mixing part A and part B in a volume ratio of 0.8:1 to 1.2:1 to form an adhesive mixture to achieve a concentration of the thermally conductive filler in the adhesive mixture of 65-85 wt % based on the total weight of the adhesive mixture;
[0224] The ratio of [a4]:[b3] is 0.7 to 0.9;
[0225] (4) applying the adhesive mixture to at least one substrate;
[0226] (5) placing a second substrate in bonding contact with the adhesive mixture; and
[0227] (6) Allow the adhesive mixture to cure.
[0228] Preferred embodiments of the adhesives described herein are also applicable to methods of adhering substrates.
[0229] The adhesive is particularly suitable for bonding metal to metal, in particular steel, aluminum, magnesium, titanium, nickel-plated steel, stainless steel, coated steels typically used in the automotive industry such as zinc-coated steel and zinc-magnesium-coated steel, metal surfaces coated with organic coatings such as epoxy powder coatings, PET foils, plastic surfaces.
[0230] In a preferred embodiment, both the first substrate and the second substrate are metal, in particular steel or aluminium.
[0231] Curing is carried out by simply leaving the mixture to stand, preferably at room temperature. Functionally useful curing is typically achieved after 7 days at room temperature. Acceleration of curing can be achieved by heating. Functionally useful curing can also be achieved after 2 h at 60° C.
[0232] Effects of the disclosed adhesive
[0233] The cured (7 days, room temperature) adhesive preferably has a thermal conductivity greater than or equal to 1.0 W / Km, more preferably greater than or equal to 1.1 W / km, when measured according to ASTM 5470-12 according to the examples described herein.
[0234] As described in the examples herein, the cured (7 days, room temperature) adhesive preferably has an E modulus of 1,00 MPa or more, more preferably 1000 MPa or more, particularly preferably 4,000 MPa or more, when measured according to DIN ISO EN-527-1:2012-06.
[0235] As described in the Examples herein, the cured (7 days, room temperature) adhesive preferably has a lap shear strength of 12 MPa or greater when measured on DX 56Z 0.7 mm steel.
[0236] The cured (7 days, room temperature) adhesive preferably has a T-peel strength of 1.1 N / mm or greater at 23°C when measured on DX 56Z 0.7 mm steel in accordance with ISO 11339:2010.
[0237] As described in the Examples herein, the cured (7 days, room temperature) adhesive preferably has a T-peel failure mode of at least 80% cohesive failure, more preferably at least 90% cohesive failure, and even more preferably at least 95% cohesive failure at 23°C when measured on DX 56Z 0.7mm steel.
[0238] The cured (7 days, room temperature) adhesive preferably has a volume resistivity of at least 10 Ω-m when measured as described in the Examples herein.
[0239] In particularly preferred embodiments, the cured (7 days, room temperature) adhesive has a thermal conductivity greater than or equal to 1.0 W / Km, more preferably greater than or equal to 1.1 W / km, when measured according to ASTM 5470-12 according to the examples described herein, and an E modulus of 100 MPa or more, more preferably 1000 MPa or more, particularly preferably 4,000 MPa or more when measured according to DIN ISO EN-527-1:2012-06 as described in the examples herein, and a lap shear strength of 12 MPa or more when measured on DX56Z 0.7 mm steel as described in the examples herein, and a T-peel strength of 1.1 N / mm or more at 23° C. when measured on DX56Z 0.7 mm steel according to ISO 11339:2010, and a T-peel strength of 1.1 N / mm or more when measured on DX56Z 0.7 mm steel as described in the examples herein. A T-peel failure mode of at least 80% cohesive failure, more preferably at least 90% cohesive failure, and even more preferably at least 95% cohesive failure at 23°C when measured with 0.7 mm steel, and a volume resistivity of at least 10 Ω-m when measured as described in the Examples herein.
[0240] application
[0241] The adhesive is particularly suitable for bonding components of battery assemblies where thermal conductivity and good structural properties are required, especially in electric vehicles. Specific examples include bonding battery cells to module plates or cooling plates, bonding battery modules to cooling plates, or the like.
[0242] Examples of specific embodiments
[0243] 1. A two-component thermally conductive adhesive comprising:
[0244] (A) a resin component, the resin component comprising:
[0245] (a1) at least one epoxy resin;
[0246] (a2) at least one reactive toughening agent;
[0247] (a3) at least one reactive silane;
[0248] (a4) at least one thermally conductive filler, in a concentration of [a4] (wt %) based on the total weight of Part A;
[0249] as well as
[0250] (B) a part B hardener component, the hardener component comprising:
[0251] (b1) at least one polyamine;
[0252] (b2) at least one catalyst capable of catalyzing the reaction of an amine with an epoxy group;
[0253] (b3) at least one thermally conductive filler, in a concentration of [b3] (wt %) based on the total weight of Part B;
[0254] Wherein, when used, part A and part B are mixed together in a volume ratio of 0.8:1 to 1.2:1 to form an adhesive mixture, and the concentration of the thermally conductive filler in the adhesive mixture is 65-85wt% based on the total weight of the adhesive mixture, and the ratio of [a4]:[b3] is 0.7 to 0.9.
[0255] 2. An adhesive made by mixing part A and part B of Example 1 in a volume ratio of 0.8:1 to 1.2:1 to form an adhesive mixture, and the concentration of the thermally conductive filler in the adhesive mixture is 65-85 wt% based on the total weight of the adhesive mixture, and the ratio of [a4]:[b3] is 0.7 to 0.9.
[0256] 3. A method for producing an adhesive, the method comprising the following steps:
[0257] (1) providing a part A resin component, the resin component comprising:
[0258] (a1) at least one epoxy resin;
[0259] (a2) at least one reactive toughening agent;
[0260] (a3) at least one reactive silane;
[0261] (a4) at least one thermally conductive filler, in a concentration of [a4] (wt %) based on the total weight of Part A;
[0262] (2) providing a part B hardener component, the hardener component comprising:
[0263] (b1) at least one polyamine;
[0264] (b2) at least one catalyst capable of catalyzing the reaction of an amine with an epoxy group;
[0265] (b3) at least one thermally conductive filler, in a concentration of [b3] (wt %) based on the total weight of Part B;
[0266] (3) mixing part A and part B in a volume ratio of 0.8:1 to 1.2:1 to form an adhesive mixture to achieve a concentration of the thermally conductive filler in the adhesive mixture of 65-85 wt % based on the total weight of the adhesive mixture;
[0267] The ratio of [a4]:[b3] is 0.7 to 0.9.
[0268] 4. A method for adhering two substrates, the method comprising the steps of:
[0269] (1) providing a part A resin component, the resin component comprising:
[0270] (a1) at least one epoxy resin;
[0271] (a2) at least one reactive toughening agent;
[0272] (a3) at least one reactive silane;
[0273] (a4) at least one thermally conductive filler, in a concentration of [a4] (wt %) based on the total weight of Part A;
[0274] (2) providing a part B hardener component, the hardener component comprising:
[0275] (b1) at least one polyamine;
[0276] (b2) at least one catalyst capable of catalyzing the reaction of an amine with an epoxy group;
[0277] (b3) at least one thermally conductive filler, in a concentration of [b3] (wt %) based on the total weight of Part B;
[0278] (3) mixing part A and part B in a volume ratio of 0.8:1 to 1.2:1 to form an adhesive mixture to achieve a concentration of the thermally conductive filler in the adhesive mixture of 65-85 wt % based on the total weight of the adhesive mixture;
[0279] The ratio of [a4]:[b3] is 0.7 to 0.9;
[0280] (4) applying the adhesive mixture to at least one substrate;
[0281] (5) placing a second substrate in bonding contact with the adhesive mixture; and
[0282] (6) Allow the adhesive mixture to cure.
[0283] 5. As described in embodiment 1, 2 or 3, wherein the reactive toughening agent is a polyurethane-based toughening agent.
[0284] 6. As described in any preceding embodiment, wherein the reactive silane comprises a hydrolyzable silylalkoxy group covalently bonded to a mercapto group, a primary or secondary amine group, or an epoxy group.
[0285] 7. As described in any preceding embodiment, wherein the reactive silane comprises mercaptosilane.
[0286] 8. As described in Example 7, wherein the mercaptosilane is selected from mercaptoalkyl(trialkoxy)silane and mercaptoalkyl(methyl-dialkoxy)silane.
[0287] 9. As described in Example 7, wherein the mercaptosilane is selected from γ-mercaptopropyltrimethoxysilane and γ-mercaptopropyl(methyl-dimethoxy)silane.
[0288] 10. As described in any preceding embodiment, wherein the reactive silane comprises an aminosilane.
[0289] 11. As described in embodiment 10, wherein the aminosilane is selected from aminoalkyl(trialkoxy)silane and aminoalkyl(methyl-dialkoxy)silane.
[0290] 12. As described in Example 10, wherein the aminosilane is selected from bis-(trimethoxysilylpropyl)amine, (3-aminopropyl)trimethoxysilane, (3-aminopropyl)triethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, trimethoxysilylpropyldiethylenetriamine, among which bis-(trimethoxysilylpropyl)amine.
[0291] 13. As described in embodiment 10, wherein the aminosilane is (3-aminopropyl)trimethoxysilane.
[0292] 14. As described in any preceding embodiment, wherein the reactive silane comprises epoxy silane.
[0293] 15. As described in embodiment 14, wherein the epoxy silane is selected from glycidyloxyalkyl(trialkoxy)silane and glycidyloxyalkyl(methyl-dialkoxy)silane.
[0294] 16. As described in Example 14, the epoxy silane is selected from tri(diethylene glycol methyl ether) silyl propylene glycidyl ether, (3-glycidyloxypropyl) trimethoxysilane, (3-glycidyloxypropyl) triethoxysilane, 3-glycidyloxypropyl methyl dimethoxysilane, 3-glycidyloxypropyl methyl diethoxysilane, 2-(3,4-epoxycyclohexyl)-ethyl trimethoxysilane and 2-(3,4-epoxycyclohexyl)-ethyl triethoxysilane.
[0295] 17. As described in embodiment 14, wherein the epoxy silane is tri(diethylene glycol methyl ether) silyl propylene glycidyl ether.
[0296] 18. As described in any preceding embodiment, wherein the volume ratio for mixing is 1:1.
[0297] 19. As described in any preceding embodiment, wherein the ratio of [a4]:[b3] is 0.72 to 0.87.
[0298] 20. As described in any preceding embodiment, wherein the ratio of [a4]:[b3] is 0.72 to 0.8.
[0299] 21. As described in any preceding embodiment, wherein the ratio of [a4]:[b3] is 0.75.
[0300] 22. As described in any preceding embodiment, wherein the epoxy equivalent / liter in part A is 1.50 to 4.50 mol / l.
[0301] 23. As described in any preceding embodiment, wherein the epoxy equivalent / liter in part A is 2.50 to 3.50 mol / l.
[0302] 24. As described in any preceding embodiment, wherein the epoxy equivalent / liter in part A is 3.00 to 3.30 mmol / l.
[0303] 25. As described in any preceding embodiment, wherein the NH equivalent / liter of component B is in the range of 1.50 to 4.50 mol / l.
[0304] 26. As described in any preceding embodiment, wherein the NH equivalent / liter of component B is in the range of 2.50 to 3.75 mol / l.
[0305] 27. As described in any preceding embodiment, wherein the NH equivalent / liter of component B is in the range of 3.00-3.40 mol / l.
[0306] 28. As described in any preceding embodiment, wherein the ratio of epoxy equivalent weight of part A to NH equivalent weight of part B is in the range of 0.8:1 to 1.2:1.
[0307] 29. As described in any preceding embodiment, wherein the thermally conductive filler is used in a concentration of 50-80 wt % based on the total weight of Part A.
[0308] 30. As described in any preceding embodiment, wherein the thermally conductive filler is used in part (A) at a concentration of 55-65 wt % based on the total weight of part A.
[0309] 31. As described in any preceding embodiment, the thermally conductive filler is used in part (B) at 70-90 wt % based on the total weight of part (B).
[0310] 32. As described in any preceding embodiment, the thermally conductive filler is used in part (B) at 75 to 85 wt % based on the total weight of part (B).
[0311] 33. As described in any preceding embodiment, the thermally conductive filler is used in part (A) at 55-65 wt % based on the total weight of part A, and in part (B) at 75 to 85 wt % based on the total weight of part (B).
[0312] 34. As described in any preceding embodiment, wherein the thermally conductive filler is aluminum hydroxide.
[0313] 35. As described in any preceding embodiment, wherein the thermally conductive filler is ATH having a D90 / D50 ratio of 8 or about 8 or greater.
[0314] 36. As described in any preceding embodiment, the at least one epoxy resin (a1) is based on bisphenol A, bisphenol F.
[0315] 37. As described in any of the preceding embodiments, wherein the at least one epoxy resin (a1) has the following general formula:
[0316]
[0317] wherein n is in the range of 0 to about 25.
[0318] 38. As described in any preceding embodiment, wherein the at least one epoxy resin (a1) has an epoxy equivalent weight in the range of about 155 to 195 g / mol.
[0319] 39. As described in any preceding embodiment, wherein the at least one epoxy resin (a1) is a liquid reaction product of epichlorohydrin and bisphenol A, the liquid reaction product having an epoxy equivalent weight of 182-192 g / eq (as measured according to ASTM D-1652), an epoxy percentage of 22.4%-23.6% (as measured according to ASTM D-1652), an epoxy group content of 5200-5500 mmol / kg (as measured according to ASTM D-1652) and a viscosity of 4000-14000 mPas at 25° C. (as measured according to ASTM D-445), for example DER 331.
[0320] 40. As described in any preceding embodiment, wherein the at least one epoxy resin (a1) is a solid epoxy resin which is a low molecular weight solid reaction product of epichlorohydrin and bisphenol A, the solid epoxy resin having an epoxy equivalent weight of 475-550 g / eq (as measured according to ASTM D-1652), an epoxy percentage of 7.8%-9.1% (as measured according to ASTM D-1652), an epoxy group content of 1820-2110 mmol / kg (as measured according to ASTM D-1652) and a melt viscosity of 400-950 mPas at 150° C. (as measured according to ASTM D-4287), for example DER 671.
[0321] 41. As described in any preceding embodiment, the at least one epoxy resin (a1) is present in 20 to 40 wt%, more preferably 25 to 35 wt%, particularly preferably 25 to 30 wt%, based on the total weight of part A of the adhesive.
[0322] 42. As described in any preceding embodiment, wherein the epoxy resin (a1) is Epoxide 1, which is used at 26 to 29 wt % based on the total weight of Part A of the adhesive.
[0323] 43. As described in any of the preceding embodiments, wherein the reactive toughening agent (a2) is prepared by reacting at least one polyol and optionally poly(butadiene) diol with a polyisocyanate in the presence of a polyurethane catalyst, optionally followed by chain extension with a dihydric phenol, and end-capping with a phenol, an oxime, or a molecule having formula I:
[0324]
[0325] Where R 1 and R 2 are independently selected from hydrogen and C1 to C6 alkyl, n is an integer from 1 to 2, and R 3 It is a C1 to C6 alkyl group.
[0326] 44. As described in embodiment 43, wherein the end-capping is carried out with phenol.
[0327] 45. As described in embodiment 43 or 44, wherein the end-capping is carried out with O,O'-diallylbisphenol A or cardanol.
[0328] 46. As described in any of embodiments 43-45, wherein the at least one polyol is a poly(alkylene oxide) glycol.
[0329] 47. As described in embodiment 46, wherein the poly(alkylene oxide) glycol is selected from poly(C2-C6 alkylene oxide) glycols, in particular poly(tetramethylene oxide) glycol ("PTMEG"), poly(oxetane) glycol ("PO3G"), and mixtures of these.
[0330] 48. As described in any of embodiments 43-47, the polyisocyanate is selected from toluene diisocyanate, 1,6-hexamethylene diisocyanate ("HMDI" or "HDI"), methylene diphenyl diisocyanate ("MDI"), 2,2,4-trimethylhexamethylene diisocyanate (TMDI) and isophorone diisocyanate (IPDI).
[0331] 49. As described in any one of embodiments 43-48, wherein the reactive toughening agent (a2) comprises toluene diisocyanate as the polyisocyanate, poly(propylene oxide) glycol or poly(tetramethylene oxide) glycol ("PTMEG") as the polyol [I think this describes DESMODUR E15] and cardanol as the capping group.
[0332] 50. As described in any one of embodiments 43-48, wherein the reactive toughening agent (a2) comprises hexamethylene diisocyanate as polyisocyanate, poly(tetramethylene furan)diol as polyol, and O,O'-diallylbisphenol A as chain extender and end-capping group.
[0333] 51. As described in any preceding embodiment, wherein the at least one polyamine (b1) has 2 or 3 or more primary and / or secondary amine functionalities.
[0334] 52. As described in any preceding embodiment, the at least one polyamine (b1) is a polyetheramine.
[0335] 53. As described in any preceding embodiment, the at least one polyamine (b1) is a diamine or triamine having a molecular weight of 200-6,000 Da.
[0336] 54. As described in any preceding embodiment, the at least one polyamine (b1) is a diamine or triamine having a molecular weight of 1,000 to 2,000 Da.
[0337] 55. As described in any preceding embodiment, wherein the at least one polyamine (b1) is selected from:
[0338]
[0339]
[0340] 56. As described in any preceding embodiment, wherein the at least one polyamine (b1) comprises a mixture of TETA and a difunctional primary amine having an average molecular weight of about 2000 and having the following general structure:
[0341] Where X≈33.
[0342] 57. As described in any preceding embodiment, wherein the NH equivalent / liter of fraction B is in the range of 1.5 to 4.50 mol / l.
[0343] 58. As described in any preceding embodiment, wherein the NH equivalent / liter of fraction B is in the range of 2.50 to 3.75 mol / l.
[0344] 59. As described in any preceding embodiment, wherein the NH equivalent / liter of fraction B is in the range of 3.00 to 3.40 mol / l.
[0345] 60. As described in any preceding embodiment, wherein the catalyst (b2) is selected from urea, tertiary amines and mixtures of these.
[0346] 61. As described in any of the preceding embodiments, wherein the catalyst (b2) is selected from p-chlorophenyl-N,N-dimethylurea (monuron), 3-phenyl-1,1-dimethylurea (benzalkonium), 3,4-dichlorophenyl N,N-dimethylurea (diuron), N-(3-chloro-4-methylphenyl)-N',N'-dimethylurea 25 (chlorotoluron), tertiary acrylamide or alkylene amines such as benzyldimethylamine, 2,4,6-tris(dimethylaminomethyl)phenol, piperidine or its derivatives, various aliphatic urea compounds (as described in EP1916272); C1-C 12 Alkylene or N-aryl imidazoles, such as 2-ethyl-2-methyl imidazole, or N-butyl imidazole and 6-caprolactam, in particular 2,4,6-tris(dimethylaminomethyl)phenol incorporated into a poly(p-vinylphenol) matrix (as described in European Patent EP0197892), or 2,4,6-tris(dimethylaminomethyl)phenol incorporated into a phenolic resin, including those described in US 4,701.378.
[0347] 62. As described in any preceding embodiment, wherein the catalyst (b2) is tris-2,4,6-tris(dimethylaminomethyl)phenol.
[0348] 63. As described in any preceding embodiment, wherein the catalyst (b2) is used in an amount of 1 to 6 wt % based on the total weight of component B.
[0349] 64. As described in any preceding embodiment, wherein the catalyst (b2) is used in an amount of 2 to 5 wt% based on the total weight of component B.
[0350] 65. As described in any preceding embodiment, wherein the catalyst (b2) is used at 3 or 4 wt% based on the total weight of component B.
[0351] Examples
[0352]
[0353]
[0354]
[0355] DER TM 331 TM A liquid epoxy resin, which is a liquid reaction product of epichlorohydrin and bisphenol A, the liquid reaction product having an epoxy equivalent weight of 182-192 g / eq (as measured according to ASTM D-1652), an epoxy percentage of 22.4%-23.6% (as measured according to ASTM D-1652), an epoxy group content of 5200-5500 mmol / kg (as measured according to ASTM D-1652) and a viscosity of 11000-14000 mPas at 25°C (as measured according to ASTM D-445).
[0356] Production of toughening agent GF200
[0357] GF200 was produced from the ingredients in Table 2.
[0358] GF200 is the reaction product of Desmodur E15 and Cardolite NX-2026. Reaction procedure: Cardolite NX-2026 and Desmodur E15 are heated to 60°C in a reactor. DABCO T-12N (catalyst) is then added. The reaction mixture is stirred at 80°C under a nitrogen atmosphere for 45 min, and then stirred under vacuum for 10 min. The colorless reaction product is then cooled to room temperature and transferred to a container.
[0359]
[0360] Preparation of epoxy adhesives
[0361] The components of component A (epoxy resin component) for the comparative examples and the inventive examples are shown in Table 3. These ingredients were compounded by mixing the ingredients listed in Table 3 on a planetary mixer or on a dual asymmetric centrifuge. In the first stage, the solid materials were added to the formulation after mixing the liquid phase. After the formulation was mixed under vacuum for about 30 minutes, it was filled into drums, barrels, or vats.
[0362] The components of component B (amine or hardener component) for the comparative examples and the inventive examples are shown in Table 4. These ingredients were compounded by mixing the ingredients listed in Table 4 on a planetary mixer or on a dual asymmetric centrifuge. In the first stage, the solid materials were added to the formulation after mixing the liquid phase. After the formulation was mixed under vacuum for about 30 minutes, it was filled into drums, barrels, or vats.
[0363]
[0364]
[0365]
[0366] The epoxy resin components are summarized in Table 3. Comparative resins 1 and 2 contain 70 wt% thermally conductive filler and only about 18% epoxy resin. Inventive resins 3 and 4 contain only 60 wt% thermally conductive filler.
[0367] Comparative Resin 1 and Inventive Resin 3 used the same toughening agent (RAM 965), while Comparative Resin 2 and Inventive Resin 4 used the same toughening agent (GF 200).
[0368] Table 4 shows the amine hardener components used to cure the different adhesives. Comparative amine hardener 1 was designed for a 1:1 mix ratio using a uniformly distributed thermally conductive filler level in both the resin component and the hardener component. The filler level was 70 wt% thermally conductive filler. It was used to mix with Comparative Resin 1 and Comparative Resin 2.
[0369] Inventive amine hardener 2 is designed for a 1:1 mixing ratio and has a higher filler content than its corresponding resin component, at 80 wt% of thermally conductive filler. It is used for mixing with Inventive Resins 3 and 4.
[0370] The amine functionality of the two amine hardener components is adjusted to match the epoxy functionality in the epoxy resin component.
[0371] Test Method
[0372] Rheology
[0373] Viscosity was measured using a Bohlin rheometer, C / P 20, up / down 0.1-20 s-1; evaluation was performed according to the Casson model.
[0374] Lap shear strength
[0375] Lap shear strength measured according to DIN EN 1465:2009:
[0376] On DX 56Z, thickness 0.7 mm or as described substrates as indicated in the table; degreased with heptane, 10 x 25 mm bonding area, 0.2 mm adhesive layer thickness. Failure modes after lap shear testing are analyzed and classified by cohesive failure (CF) and adhesive failure (AF). Values are rounded to multiples of 10%.
[0377] Tensile test
[0378] Cured adhesive plaques with a thickness of 2 mm were prepared and cured at room temperature for 7 days. Dog-bone shaped specimens were cut from the plaques. The dimensions were according to DIN ISO EN-527-1 and the test was performed accordingly using a zwick tensile tester.
[0379] T peel strength
[0380] The T-peel strength was measured according to ISO 11339:2010. The samples were DC 04ZE (steel) from ThyssenKrupp with a thickness of 0.7 mm. Glass beads with a thickness of 0.2 mm were used as spacers between the two strips to adjust the adhesive layer to 0.2 mm. During the 7-day curing cycle at room temperature, the two strips were held together using a metal clamp. The test was performed according to ISO 11339.
[0381] Thermal conductivity
[0382] The thermal conductivity was measured according to ASTM 5470-12 on a thermal interface material tester from ZFW, Stuttgart. The test was carried out in Spaltplus mode at a thickness of 1.0 mm. The thermal interface material was considered to be type I (viscous liquid) as described in ASTM 5470-12. The upper contact was heated to about 40° C. and the lower contact was heated to about 10° C., resulting in a sample temperature of about 25° C. The A and B components were mixed with a static mixer when applied from a manual cartridge system to prepare a plaque with a thickness of 1.0 mm to measure the thermal conductivity after curing.
[0383] Volume resistivity
[0384] The volume resistivity was measured according to ASTM D257, IEC 62631-3-1 using 500 V applied for 60 seconds.
[0385] result
[0386] The results of the tests are summarized in Table 5. The comparative examples are designated "CE" and the inventive examples are designated "IE".
[0387]
[0388] Inventive Example 3 shows a significantly improved T-peel failure mode for the adhesive compared to Comparative Example 1, with 100% cohesive failure mode compared to 100% adhesive failure mode. The same is true for Inventive Example 4 compared to Comparative Example 2, with 100% cohesive failure mode compared to 80% adhesive failure mode, respectively.
[0389] Furthermore, the volume resistivity of the inventive examples is one order of magnitude higher than that of the comparative examples, which indicates significantly better electrical properties in the case of the inventive method.
Claims
1. A two-component thermally conductive adhesive comprising: (A) a resin component, the resin component comprising: (a1) at least one epoxy resin; (a2) at least one reactive toughening agent; (a3) at least one reactive silane; (a4) at least one thermally conductive filler in a concentration of [a4] (wt %) based on the total weight of Part A; and (B) a part B hardener component, the hardener component comprising: (b1) at least one polyamine; (b2) at least one catalyst capable of catalyzing the reaction of an amine with an epoxy group; (b3) at least one thermally conductive filler, in a concentration of [b3] (wt %) based on the total weight of Part B; in, When used, Part A and Part B are mixed together in a volume ratio of 0.8:1 to 1.2:1 to form an adhesive mixture, and the concentration of the thermally conductive filler in the adhesive mixture is 65-85wt% based on the total weight of the adhesive mixture, and the ratio of [a4]:[b3] is 0.7 to 0.
9.
2. The adhesive according to claim 1, wherein The reactive toughening agent is a polyurethane-based toughening agent.
3. The adhesive according to claim 1, wherein The reactive silane comprises a hydrolyzable silylalkoxy group covalently bonded to a mercapto group, a primary or secondary amine group, or an epoxy group.
4. The adhesive according to claim 1, wherein The reactive silane includes mercaptosilane.
5. The adhesive according to claim 4, wherein The mercaptosilane is selected from mercaptoalkyl(trialkoxy)silane and mercaptoalkyl(methyl-dialkoxy)silane.
6. The adhesive according to claim 4, wherein The mercaptosilane is selected from γ-mercaptopropyltrimethoxysilane and γ-mercaptopropyl(methyl-dimethoxy)silane.
7. The adhesive according to claim 1, wherein The reactive silane includes aminosilane.
8. The adhesive according to claim 7, wherein The aminosilane is selected from aminoalkyl(trialkoxy)silane and aminoalkyl(methyl-dialkoxy)silane.
9. The adhesive according to claim 8, wherein The aminosilane is selected from bis-(trimethoxysilylpropyl)amine, (3-aminopropyl)trimethoxysilane, (3-aminopropyl)triethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, trimethoxysilylpropyldiethylenetriamine, among which bis-(trimethoxysilylpropyl)amine.
10. The adhesive according to claim 9, wherein The aminosilane is (3-aminopropyl)trimethoxysilane.
11. The adhesive according to claim 1, wherein The reactive silane includes epoxy silane.
12. The adhesive according to claim 11, wherein The epoxy silane is selected from glycidyloxyalkyl(trialkoxy)silane and glycidyloxyalkyl(methyl-dialkoxy)silane.
13. The adhesive according to claim 12, wherein The epoxysilane is selected from tri(diethylene glycol methyl ether) silyl propylene glycidyl ether, (3-glycidyloxypropyl) trimethoxysilane, (3-glycidyloxypropyl) triethoxysilane, 3-glycidyloxypropyl methyl dimethoxysilane, 3-glycidyloxypropyl methyl diethoxysilane, 2-(3,4-epoxycyclohexyl)-ethyl trimethoxysilane and 2-(3,4-epoxycyclohexyl)-ethyl triethoxysilane.
14. The adhesive according to claim 13, wherein The epoxy silane is tri(diethylene glycol methyl ether) silyl propylene glycidyl ether.
15. The adhesive according to claim 1, wherein The volume ratio used for mixing was 1:1.