Diene rubber composition and method for producing same

By combining high-molecular-weight and low-molecular-weight conjugated diene rubber and modifying silicon compound, combining silica and carbon black, the existing rubber compositions in terms of resilience, wear resistance and wet grip properties are solved. Inadequately, the multi-physical properties optimization of low fuel consumption tires has been achieved.

CN118900874APending Publication Date: 2024-11-05ENTERPRISE TURNAROUND INITIATIVE CORPORATION OF JAPAN
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380028676.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-31
Filing Date
2023-03-30
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

The prior art is difficult to simultaneously improve the elasticity, wear resistance, processability and wet grip properties of diene rubber, and the physical properties of the existing rubber compositions are not ideal when mixed.

Method used

By combining high molecular weight and low molecular weight conjugated diene rubber components and performing specific silicon compound terminal modification and hydrolysis steps, a diene rubber with excellent processability, resilience and wear resistance was prepared. The composition, combining silica and carbon black as reinforcement, optimizes the physical properties of the rubber.

Benefits of technology

In low fuel consumption tire applications, rubber has improved its low fuel consumption, wear resistance and wet grip performance, while ensuring good processability and meeting the optimization of multiple physical properties indicators.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005049815550000031
    Figure BDA0005049815550000031
  • Figure BDA0005049815550000041
    Figure BDA0005049815550000041
  • Figure BDA0005049815550000061
    Figure BDA0005049815550000061
Patent Text Reader

Abstract

The present invention addresses the problem of providing: a conjugated diene rubber composition having excellent resilience and wear resistance, good processability during rubber kneading, and excellent wet grip performance; and a method for producing the conjugated diene rubber composition. A mixture of a diene rubber component (1) in which a conjugated diene polymer (1) is terminal-modified with at least one silicon compound represented by formula (1) and / or formula (2) and a diene rubber component (2) in which a conjugated diene polymer (2) is terminal-modified with at least one silicon compound represented by formula (1) and / or formula (2) is supplied to a hydrolysis step and then dried. Thus, the diene rubber composition is obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a diene rubber composition, a method for producing the same, and a tire produced using the diene rubber composition. Background Art

[0002] Conventionally, studies have been conducted on improving the rebound resilience, abrasion resistance, processability, wet grip and the like in diene rubber compositions used in fuel-efficient tires.

[0003] Patent Documents 1 and 2 disclose compositions of high molecular weight conjugated diene rubber and low molecular weight conjugated diene rubber. These rubber compositions are mainly used for molecular design of racing tires.

[0004] Patent document 3 discloses a rubber composition in which a high molecular weight component and a low molecular weight component are separately manufactured and mixed, wherein the high molecular weight component is obtained by polymerizing styrene and butadiene using alkyl lithium as a polymerization initiator and then reacting a silane compound having an R-Si-S-R'-bond.

[0005] Patent document 4 discloses a method for producing a composition consisting of a high molecular weight component and a low molecular weight component, wherein styrene and butadiene are polymerized using alkyl lithium as a polymerization initiator, and then coupled using a multifunctional silane compound to generate a high molecular weight component, and the added modifier is increased for each remaining unreacted molecule.

[0006] Patent documents 5 to 7 disclose a rubber composition, a silica compounding composition thereof, and a silica and carbon black mixed compounding composition thereof, wherein the rubber composition is prepared by polymerizing styrene and butadiene using alkyl lithium as a polymerization initiator and then modified by a siloxane compound to form a high molecular weight component having a molecular weight (Mw) of more than 350,000 g / mol and a low molecular weight component having a molecular weight (Mw) of less than 10,000.

[0007] Although the technologies described in the above documents satisfy the physical properties corresponding to the purposes of the corresponding documents, they cannot simultaneously satisfy various physical properties such as rebound resilience and wear resistance, processability during rubber kneading, and wet grip performance.

[0008] Prior art literature

[0009] Patent Literature

[0010] Patent Document 1: Japanese Patent Publication No. 5-74614

[0011] Patent Document 2: Japanese Patent Application Publication No. 3290469

[0012] Patent Document 3: Japanese Patent Application No. 2018-507303

[0013] Patent Document 4: WO2018-56025

[0014] Patent Document 5: Japanese Patent Application Publication No. 6864078

[0015] Patent Document 6: Japanese Patent Application Publication No. 6823708

[0016] Patent Document 7: Japanese Patent Publication No. 6799666 Summary of the invention

[0017] Problems to be solved by the invention

[0018] Under such circumstances, an object of the present invention is to provide a conjugated diene rubber composition having excellent rebound resilience and abrasion resistance, good processability during rubber kneading, and excellent wet grip performance, and a method for producing the same.

[0019] Means used to solve problems

[0020] The present inventors conducted intensive research to solve this problem and found that by combining a specified high molecular weight diene rubber component with a specified low molecular weight diene rubber component, a diene rubber composition with good processability, excellent rebound resilience, abrasion resistance and wet grip and a method for producing the same can be provided. Further research was conducted to complete the present invention.

[0021] That is, the present invention relates to the following aspects.

[0022] [1] A diene rubber composition, comprising: a diene rubber component 1 in which a conjugated diene polymer 1 is terminally modified with at least one silicon compound represented by formula (1) and / or formula (2) and a diene rubber component 2 in which a conjugated diene polymer 2 is terminally modified with at least one silicon compound represented by formula (1) and / or formula (2) are subjected to a hydrolysis step, followed by drying, thereby obtaining a diene rubber composition;

[0023] The conjugated diene polymer 1 is obtained by polymerizing a conjugated diene compound and an aromatic vinyl compound, and has a peak molecular weight of 400k to 2,000 kg / mol in terms of polystyrene.

[0024] The conjugated diene polymer 2 is obtained by polymerizing a conjugated diene compound and an aromatic vinyl compound, and has a peak molecular weight of 15k to 60kg / mol in terms of polystyrene.

[0025] Chemical formula 1:

[0026] (X 1 ) n (R 1 O) m -Si-(R2 ) 4-n-m Formula (1),

[0027] In the formula, R 1 and R 2 are independently an alkyl group, an aromatic group or an allyl group having 1 to 12 carbon atoms, or an alkyl group, an aromatic group or an allyl group containing an oxygen atom and / or a nitrogen atom in these groups, X 1 is iodine, bromine or chlorine, n and m are 0, 1, 2, 3 or 4 respectively,

[0028] Chemical formula 2:

[0029]

[0030] In the formula, R 3 ~R 8 Each independently represents an alkyl group, an aromatic group or an allyl group having 1 to 12 carbon atoms, or an alkyl group, an aromatic group or an allyl group containing an oxygen atom and / or a nitrogen atom in these groups. In addition, R 7 and R 8 For the ring structure, p is a number between 1.5 and 1,000 with an interval of 0.5.

[0031] [2] The diene rubber composition according to [1], wherein the 1,2-structure or 3,4-structure of the diene part in the diene rubber component 1 is 20 to 70%, and the weight ratio of the aromatic vinyl compound component in the diene rubber component 1 is 10 to 50%.

[0032] The 1,2-structure or 3,4-structure of the diene portion in the diene rubber component 2 is 40 to 80%, and the weight ratio of the aromatic vinyl compound component in the diene rubber component 2 is 5 to 35%.

[0033] [3] The diene rubber composition according to [1] or [2], wherein the ratio of the diene rubber component 1 to the diene rubber component 2 is 10 to 90 phr of the diene rubber component 2 relative to 100 phr of the diene rubber component 1.

[0034] [4] A rubber compounding composition comprising at least 20 to 150 phr of silica based on 100 phr of the total rubber component including at least 20 phr of the diene rubber composition described in [2] or [3] above.

[0035] [5] A rubber compounding composition comprising at least 20 to 150 phr of silica and 5 to 30 phr of carbon black, relative to 100 phr of the total rubber component, including at least 20 phr of the diene rubber composition described in [2] or [3] above.

[0036] [6] A method for producing a diene rubber composition,

[0037] i) in the presence of an organic lithium compound, initiating polymerization of a conjugated diene compound and an aromatic vinyl compound in a hydrocarbon;

[0038] ii) the conjugated diene polymer 1 having a peak molecular weight of 400 k to 2,000 kg / mol in terms of polystyrene after polymerization in i) is polymerized with at least one silicon compound represented by formula (1) and / or formula (2), and then immediately subjected to terminal modification to produce a diene rubber component 1;

[0039] iii) the conjugated diene polymer 2 having a peak molecular weight of 15k to 60 kg / mol in terms of polystyrene after polymerization in i) is polymerized via at least one silicon compound represented by formula (1) and / or formula (2), and then immediately subjected to terminal modification to produce a diene rubber component 2;

[0040] iv) subjecting the obtained diene rubber component 1 and diene rubber component 2 to a hydrolysis step, preferably to steam coagulation, and then drying;

[0041] Chemical formula 3:

[0042] (X 1 ) n (R 1 O) m -Si-(R 2 ) 4-n-m Formula (1),

[0043] In the formula, R 1 and R 2 are alkyl groups, aromatic groups or allyl groups having 1 to 12 carbon atoms, or alkyl groups, aromatic groups or allyl groups containing oxygen atoms and / or nitrogen atoms in these groups, X 1 is a halogen atom of iodine, bromine or chlorine, n and m are 0, 1, 2, 3 or 4,

[0044] Chemical formula 4:

[0045]

[0046] In the formula, R 3 ~R 8 Each of them is independently an alkyl group, an aromatic group or an allyl group having 1 to 12 carbon atoms, or an alkyl group, an aromatic group or an allyl group containing an oxygen atom and / or a nitrogen atom in these groups, and R 7 and R 8 For the ring structure, p is a number between 1.5 and 1,000 with an interval of 0.5.

[0047] [7] The method according to [6], wherein polymerization of the diene rubber component 1 alone or both the diene rubber component 1 and the diene rubber component 2 is initiated in the presence of an organic lithium compound and a secondary amine compound.

[0048] [8] The method according to [6] or [7], wherein, when the diene rubber component 1 is polymerized, isoprene is prepolymerized with an organic lithium compound, and then a conjugated diene compound other than isoprene is polymerized with the aromatic vinyl compound.

[0049] [9] A method according to any one of [6] to [8], wherein after the diene rubber component 1 is polymerized, a conjugated diene compound, an aromatic vinyl compound, and an optional 1,2-structure or 3,4-structure regulator of the diene portion are added, and the polymerization is reinitiated in the presence of an organic lithium compound.

[0050]

[10] The method according to any one of [6] to [9], wherein after step iii) and before step iv), a silicon halide compound represented by formula (3) or an alkali metal compound represented by formula (4) in an amount satisfying the condition of formula (5) is added, and then steam coagulation / drying in step iv) is performed.

[0051] Chemical formula 5:

[0052] (R 9 ) q -M 1 -(X 2 ) 4-q Formula (3),

[0053] Where M 1 is a silicon atom, R 9 is an alkyl group, an aromatic group or an allyl group having 1 to 12 carbon atoms, X 2 is a halogen atom of iodine, bromine or chlorine, q is 0 or 1,

[0054] Chemical formula 6:

[0055] R 10 -OM 2 Formula (4),

[0056] Where M 2 is an alkali metal atom, preferably a lithium atom, a sodium atom or a potassium atom, R 10 is an alkyl group, an aromatic group, an allyl group or an acyl group having 1 to 12 carbon atoms,

[0057] Chemical formula 7:

[0058] 1.5≥[nX1 +(4q)X 2 ](L+M 2 )≥0.9 Formula (5),

[0059] Wherein, L is the molar number of the organic lithium compound added to the polymerization initiator, M 2 is the number of moles of the alkali metal compound represented by formula (4), X 1 is the number of moles of the silicon compound represented by formula (1), X 2 is the number of moles of the silicon halide compound represented by formula (3), n is the same as n in the silicon compound represented by formula (1), and q is also the same as q in the silicon halide compound represented by formula (3).

[0060]

[11] The method according to any one of [6] to

[10] , wherein the ratio of the diene rubber component 1 to the diene rubber component 2 is 10 to 90 phr of the diene rubber component relative to 1100 phr of the diene rubber component.

[0061] Effects of the Invention

[0062] The present invention relates to a silica-modified diene rubber composition which, when used as a tire rubber, has excellent fuel efficiency and wear resistance, good processability when compounded with rubber, and also good wet grip performance, and a method for producing the same. DETAILED DESCRIPTION

[0063] Examples of the conjugated diene compound used in the present invention include 1,3-butadiene, isoprene, 1,3-pentadiene (piperine), 2,3-dimethyl-1,3-butadiene, 1,3-hexadiene, etc. Among them, 1,3-butadiene and isoprene are preferred from the viewpoint of availability and physical properties of the obtained diene rubber. 1,3-butadiene is particularly preferred.

[0064] The conjugated diene compound used in the diene rubber component 1 as the high molecular weight component of the present invention is 50 to 90% by weight, preferably 60 to 85% by weight.

[0065] The conjugated diene compound used in the diene rubber component 2 as the low molecular weight component of the present invention is 65 to 95% by weight, preferably 70 to 95% by weight.

[0066] Examples of the aromatic vinyl compound used in the present invention include styrene, α-methylstyrene, vinyltoluene, vinylnaphthalene, divinylbenzene, trivinylbenzene, and divinylnaphthalene, etc. Among them, styrene is preferred from the viewpoint of availability and physical properties of the obtained diene rubber.

[0067] The amount of the aromatic vinyl compound used in the diene rubber component 1 as the high molecular weight component of the present invention is 10 to 50% by weight, preferably 15 to 40% by weight.

[0068] The amount of the aromatic vinyl compound used in the diene rubber component 2 as the low molecular weight component of the present invention is 5 to 35% by weight, preferably 5 to 30% by weight.

[0069] As the organic lithium compound used in the present invention, it is a lithium compound having 2 to 20 carbon atoms. For example, ethyl lithium, n-propyl lithium, isopropyl lithium, n-butyl lithium, sec-butyl lithium, tert-butyl lithium, tert-octyl lithium, n-decyl lithium, phenyl lithium, 2-naphthyl lithium, 2-butyl-phenyl lithium, 4-phenyl-butyl lithium, cyclohexyl lithium, 4-cyclopentyl lithium, 1,4-dilithium-butene-2, etc. Preferably, n-butyl lithium, sec-butyl lithium, tert-butyl lithium are preferred from the perspective of industrial availability and stability, and n-butyl lithium and sec-butyl lithium are particularly preferred.

[0070] The secondary amine compound used in the present invention is a compound represented by formula (6) or formula (7).

[0071] Chemical formula 8

[0072] R 11 R 12 NH Formula (6)

[0073] Chemical formula 9

[0074]

[0075] In the formula, R 11 , R 12 is an alkyl, cycloalkyl or aralkyl group having 1 to 20 carbon atoms, R 11 and R 12 can be the same or different, and R 13 It is a divalent alkylene group, a bicycloalkane group, an oxy- or amino-alkylene group having 3 to 12 methylene groups.

[0076] R in formula (6) 11 , R 12 Examples include methyl, ethyl, butyl, hexyl, octyl, cyclohexyl, 3-phenyl-1-propyl, isobutyl, etc. Specifically, methylethylamine, diethylamine, dibutylamine, ethylbutylamine, dihexylamine, dioctylamine, butyloctylamine, octylcyclohexylamine, diisobutylamine, butyl(3-phenyl-1-propyl)amine, etc. Preferably, dioctylamine and dihexylamine are industrially available and have good solubility in hydrocarbon solvents.

[0077] R in formula (7) 13The alkyl group includes, for example, trimethylene, tetramethylene, hexamethylene, oxydiethylene, N-alkyl azadiethylene, etc. As specific examples, pyrrolidine, piperidine, hexamethyleneimine or heptamethyleneimine, etc., can be cited. In addition, it can be a dicyclic body such as decahydroisoquinoline, octahydroindole, etc. In particular, pyrrolidine, piperidine, hexamethyleneimine or heptamethyleneimine is suitable.

[0078] Examples of the compound to be prepolymerized with the organolithium compound in the presence of the secondary amine compound include compounds having a faster vulcanization rate than butadiene, specifically isoprene, 1,3-pentadiene (piperine), and 2,3-dimethyl-1,3-butadiene. Isoprene is preferred in terms of industrial availability and vulcanization rate.

[0079] Specific examples of the silicon compound represented by the formula (1) include the following compounds.

[0080] For example, tetramethoxysilane, tetraethoxysilane, tetrapropoxysilane, tetrabutoxysilane, tetraphenoxysilane, tetratoluoyloxysilane, methyltrimethoxysilane, methyltriethoxysilane, methyltripropoxysilane, methyltributoxysilane, methyltriphenoxysilane, ethyltrimethoxysilane, ethyltriethoxysilane, ethyltripropoxysilane, ethyltributoxysilane, ethyltriphenoxysilane, dimethyldimethoxysilane, dimethyldiethoxysilane, dimethyl dipropoxysilane, dimethyldibutoxysilane, dimethyldiphenoxysilane, diethyldimethoxysilane, diethyldiethoxysilane, diethyldipropoxysilane, diethyldibutoxysilane, diethyldiphenoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, vinyltriprooxysilane, vinyltributoxysilane, vinyltriphenoxysilane, vinyltri(2-methoxyethoxy)silane, vinyltri(methylethylketoxime)silane, methyltri( methyl ethyl ketoxime) silane, methyl tris (diethyl ketoxime) silane, ethyl tris (methyl ethyl ketoxime) silane, ethyl tris (dimethyl ketoxime) silane, allyl triphenoxy silane, octenyl trimethoxy silane, phenyl trimethoxy silane, phenyl triethoxy silane, phenyl tripropropoxy silane, phenyl tributoxy silane, phenyl triphenoxy silane, 2- (3,4-epoxycyclohexyl) ethyl trimethoxy silane, vinyl tris (methoxypropoxy) silane, methyl tris [2- (dimethyl

[0043] The present invention relates to methyltris[2-(diethylamino)ethoxy]silane, methyltris[2-(dibutylamino)ethoxy]silane, ethyltris[2-(dimethylamino)ethoxy]silane, ethyltris[2-(diethylamino)ethoxy]silane, ethyltris[2-(dibutylamino)ethoxy]silane, tetrakis[2-(dimethylamino)ethoxy]silane, tetrakis[2-(diethylamino)ethoxy]silane, and tetrakis[2-(dibutylamino)ethoxy]silane. Among them, ketoxime silanes, trimethoxysilanes, triethoxysilanes, and tripropoxysilanes which are relatively easy to hydrolyze, or aminoethoxysilanes which are presumed to increase the storage stability of diene rubber and promote reactivity with silica are preferred.

[0081] Specific examples of the aminoalkoxysilane compound represented by formula (1) are shown below. Examples thereof include dimethylaminomethyltrimethoxysilane, 2-dimethylaminoethyltrimethoxysilane, 3-dimethylaminopropyltrimethoxysilane, 4-dimethylaminobutyltrimethoxysilane, dimethylaminomethyldimethoxymethylsilane, 2-dimethylaminoethyldimethoxymethylsilane, 3-dimethylaminopropyldimethoxymethylsilane, 4-dimethylaminobutyldimethoxymethylsilane, dimethylaminomethyltriethoxysilane, 2-dimethylaminoethyltriethoxysilane, 3-dimethylaminopropyltriethoxysilane, 3-diethylaminopropyltrimethoxysilane, 4-dimethylaminobutyltrimethoxymethylsilane, dimethylaminomethyltriethoxysilane, 2-dimethylaminoethyltriethoxysilane, 3-dimethylaminopropyltriethoxysilane, 3-diethylaminopropyltrimethoxysilane, 4-dimethylaminobutyltrimethoxymethylsilane, 2-dimethylaminoethyltriethoxysilane, 3-dimethylaminopropyltrimeth ... Oxysilane, 4-dimethylaminobutyltriethoxysilane, dimethylaminomethyldiethoxymethylsilane, 2-dimethylaminoethyldiethoxymethylsilane, 3-dimethylaminopropyldiethoxymethylsilane, 4-dimethylaminobutyldiethoxymethylsilane, N-(3-triethoxysilylpropyl)-4,5-dihydroimidazole, N-allyl-aza-2,2-dimethoxysilyl-cyclopentane, etc., particularly preferably 3-dimethylaminopropyltriethoxysilane, 3-diethylaminopropyltriethoxysilane, and 3-diethylaminopropyltrimethoxysilane.

[0082] Specific examples of the silicon halide compound represented by the formula (1) include the following compounds.

[0083] Examples thereof include silicon tetrachloride, methyl silicon trichloride, ethyl silicon trichloride, propyl silicon trichloride, butyl silicon trichloride, octyl silicon trichloride, cyclohexyl silicon trichloride, silicon tetrabromide, methyl silicon tribromide, ethyl silicon tribromide, propyl silicon tribromide, butyl silicon tribromide, octyl silicon tribromide, cyclohexyl silicon tribromide, silicon tetraiodide, ethyl silicon triiodide, propyl silicon triiodide, butyl silicon triiodide, octyl silicon triiodide, and cyclohexyl silicon triiodide.

[0084] Among them, silicon tetrachloride, methyl silicon trichloride, and ethyl silicon trichloride are preferred, and silicon tetrachloride and methyl silicon trichloride are particularly preferred.

[0085] The commonly used silicon compound is the compound called silicone oil. The viscosity (mm) measured at 25°C 2 The compound may be a compound with a molecular weight of 0.3 to 1000, and more preferably 0.6 to 200. Dimethyl silicone oil and methylphenyl silicone oil also belong to the compound. Modified silicone oils containing polyether groups, epoxy groups and dialkylamino groups are also suitable.

[0086] As the silicon compound represented by formula (2) among the low molecular weight compounds, specifically, the following compounds can be mentioned, but it is not limited thereto. The following compounds can be mentioned: 1,1,1,3,3,5,5-heptamethyl-5-methoxytrisiloxane, 1,1,1,3,3,5,5-heptamethyl-5-ethoxytrisiloxane, 1,1,1,3,3,5,5-heptamethyl-5-phenoxytrisiloxane, 1,1,1,3,3,5-hexamethyl-5,5-dimethoxytrisiloxane, 1,1,1,3,3,5-hexamethyl-5,5-diethoxytrisiloxane, 1,1,1,3,3,5-hexamethyl-5 ,5-diphenoxy trisiloxane, 1,1,1,3,3-pentamethyl-5,5,5-trimethoxy trisiloxane, 1,1,1,3,3-pentamethyl-5,5,5-triethoxy trisiloxane, 1,1,1,3,3-pentamethyl-5,5,5-triphenoxy trisiloxane, 1,1,3,3-tetramethyl-1,5,5,5-tetramethoxy trisiloxane, 1,1,3,3-tetramethyl-1,5,5,5-tetraethoxy trisiloxane, 1,1,3 ,3-Tetramethyl-1,5,5,5-tetraphenoxy trisiloxane, 1,3,3-trimethyl-1,1,5,5,5-pentamethoxy trisiloxane, 1,3,3-trimethyl-1,1,5,5,5-pentaethoxy trisiloxane, 1,3,3-trimethyl-1,1,5,5,5-pentaphenoxy trisiloxane, 3,3-dimethyl-1,1,1,5,5,5-hexamethoxy trisiloxane, 3,3-dimethyl-1,1,1,5,5,5-hexaethoxy trisiloxane Oxytrisiloxane, 3,3-dimethyl-1,1,1,5,5,5-hexaphenoxytrisiloxane, 1-(3-glycidyloxypropyl)-1,1,3,3-tetramethyl-5,5,5-trimethoxytrisiloxane, 1-(3-glycidyloxypropyl)-1,1,3,3-tetramethyl-5,5,5-triethoxytrisiloxane, 1-(3-glycidyloxypropyl)-1,1,3,3-tetramethyl-5,5,5-triphenoxytrisiloxane, etc.

[0087] In the siloxane compound represented by formula (2), R 7 and R 8 The cyclic siloxane compound is a cyclic siloxane compound. Specific examples of the cyclic siloxane compound include hexamethylcyclotrisiloxane (D3), octamethylcyclotetrasiloxane (D4), decamethylcyclopentasiloxane (D5), dodecamethylcyclohexasiloxane (D6), tetradecamethylcycloheptasiloxane (D7), hexadecylcyclooctasiloxane (D8), octadecylcyclononasiloxane (D9), and eicosylcyclodecasiloxane (D10). D3, D4, and D5 are preferred.

[0088] When the compound of formula (2) is used, it may be used alone, but it is preferred to use it in combination with the compound of formula (1) because a branched structure is generated.

[0089] Examples of the alkoxysilane compound having a protective group that converts to a primary amino group after hydrolysis include N,N-bis(trimethylsilyl)-3-aminopropyltrimethoxysilane, N,N-bis(trimethylsilyl)-3-aminopropyltriethoxysilane, N,N-bis(trimethylsilyl)-3-aminopropyltripropoxysilane, N,N-bis(trimethylsilyl)-2-aminoethyltrimethoxysilane, N,N-bis(trimethylsilyl)-3-aminopropyltriethoxysilane, Examples of the ketimines include 3-triethoxysilyl-N-(1,3-dimethyl-butylene)propylamine, 3-trimethoxysilyl-N-(1,3-dimethyl-butylene)propylamine, and 3-tripropoxysilyl-N-(1,3-dimethyl-butylene)propylamine, which are easily hydrolyzed.

[0090] The diene rubber component of the present invention is produced by solution polymerization. The amounts of raw materials used, reaction temperature, reaction time and other conditions for producing the solution polymerization diene rubber are as follows.

[0091] The solution polymerization of diene rubber is carried out by a commonly used method, wherein a conjugated diene compound or an aromatic vinyl compound is polymerized in the presence of an organic lithium compound and a polar compound such as an ether compound or an amine compound at a temperature of 10 to 120° C. for tens of minutes to several hours.

[0092] The amount of the organolithium compound used is usually in the range of 0.01 to 10 millimoles per 100 g of diene rubber. When it is less than 0.01 millimole, the molecular weight becomes too high, the solution viscosity increases or the MV viscosity becomes high, and problems arise in the rubber production process and tire manufacturing process. In addition, when it exceeds 10 millimoles, the molecular weight of the diene rubber becomes too low.

[0093] During polymerization, as ether compounds for adjusting the microstructure of the diene monomer portion of the diene rubber, in particular, adjusting the vinyl content (1,2-structure or 3,4-structure of the diene portion), diethyl ether, di-n-butyl ether, ethylene glycol diethyl ether, ethylene glycol dibutyl ether, diethylene glycol dimethyl ether, propylene glycol dimethyl ether, propylene glycol diethyl ether, propylene glycol dibutyl ether, tetrahydrofuran (THF), 2,2-bis(2-tetrahydrofuranyl)propane (DTHFP), bis-tetrahydrofurfuryl formal, methyl ether of tetrahydrofurfuryl alcohol, ethyl ether of tetrahydrofurfuryl alcohol, butyl ether of tetrahydrofurfuryl alcohol, α-methoxytetrahydrofuran, dimethoxybenzene, dimethoxyethane, and the like are used.

[0094] As the amine compound, a tertiary amine compound such as triethylamine, pyridine, N,N,N',N'-tetramethylethylenediamine, dipyridineethane, methyl ether of N,N-diethylethanolamine, ethyl ether of N,N-diethylethanolamine, butyl ether of N,N-diethylethanolamine, etc. is used.

[0095] Preferred compounds include tetrahydrofuran (THF) and 2,2-di(2-tetrahydrofuryl)propane (DTHFP) in consideration of polymerization rate and modification efficiency.

[0096] The amount of these compounds added is usually 0.01 to 10 mol, preferably 0.2 to 5 mol, per mol of the organolithium compound when containing a plurality of nitrogen atoms or oxygen atoms. Compounds having one oxygen atom in the molecule such as tetrahydrofuran are preferably added in an amount of 0.05 to 10% based on the solvent.

[0097] The polymerization reaction is carried out in a hydrocarbon solvent. Suitable hydrocarbon solvents are selected from aliphatic hydrocarbons, aromatic hydrocarbons, alicyclic hydrocarbons, and particularly propane, n-butane, isobutane, n-pentane, isopentane, cyclopentane, n-hexane, cyclohexane, methylcyclohexane, n-heptane, cycloheptane, propylene, 1-butene, isobutylene, trans-2-butene, cis-2-butene, 1-pentene, 2-pentene, 1-hexene, 2-hexene, benzene, toluene, xylene, ethylbenzene, etc. having 3 to 12 carbon atoms. Preferably, n-pentane, isopentane, cyclopentane, n-hexane, cyclohexane, and n-heptane are used. In addition, these solvents can be mixed with two or more.

[0098] In the present invention, the conjugated diene compound or the conjugated diene compound and the aromatic vinyl compound are mainly anion polymerized to react the active diene rubber with the silicon compound. In the case of intermittent polymerization and adiabatic method, these modification reactions are 0 to 120°C, preferably 20 to 100°C, and the reaction time is 1 to 60 minutes, preferably 5 to 40 minutes. In the case of isothermal method, these modification reactions are 30 to 100°C, preferably 50 to 80°C, and the reaction time is 1 to 250 minutes, preferably 30 to 200 minutes.

[0099] In the case of continuous polymerization, these modification reactions are carried out at 30 to 100°C, preferably 50 to 80°C.

[0100] The polymerization method used in the present invention may be a batch polymerization method or a continuous polymerization method. In particular, the batch polymerization method is suitable for diene rubbers in order to have the characteristics of resilience, and in particular, the continuous polymerization method is suitable for diene rubbers in order to have the characteristics of wear resistance and processability.

[0101] The diene rubber component 1 as the high molecular weight component of the present invention may be polymerized batchwise or continuously, but continuous polymerization is preferred.

[0102] The diene rubber component 2 as the low molecular weight component of the present invention may be polymerized batchwise or continuously, but batch polymerization is more suitable.

[0103] It is relatively simple to polymerize the diene rubber component 1 and the diene rubber component 2 of the present invention in different receptacles, but it is also possible to add a predetermined polar compound or conjugated diene compound, an aromatic vinyl compound, and an initiator after producing the diene rubber component 1, and produce both components in one polymerizer.

[0104] In the steps ii) and iii), a silicon compound represented by formula (1) is added to produce the diene rubber in a manner such that the bi-branched structure of the diene rubber is 40% or less. As the amount of silane compound added, in the steps ii) and iii), it is preferred to add an amount equivalent to 0.7 to 2 times the number of molecules per molecule of active diene rubber, and more preferably 0.9 to 1.5 times. In the case where the amount is less than 0.7, the number of alkoxysilyl groups introduced into the active diene rubber decreases, and the reactivity with silica decreases. If it is more than 2 times, the storage stability deteriorates.

[0105] In the step iii), when the siloxane compound represented by formula (2) is used, it is preferably added in an amount equal to or greater than 1 to 100 times, more preferably 1 to 5 times, of Si—O bonds per molecule of the remaining active diene rubber.

[0106] In this case, it is also preferred to use a trifunctional or higher-functional silicon compound represented by formula (1) in combination.

[0107] According to the present invention, the branched structure after steam coagulation / drying is the following 2-branched structure-A or 2-branched structure-A', which is presumed to be a structure that is stable when storing rubber and highly reactive with silica when combined with silica. The reaction mechanism is presumed to be as follows: the 2-branched structure-A is generated by the condensation of (Rubber)-Si-OH formed by hydrolysis of (Rubber)-Si-OR modified by the silicon compound represented by formula (1). It is also presumed that the (Rubber)-Si-(O-Si) modified by the silicon compound represented by formula (2) n When -OLi is also neutralized, (Rubber)-Si-(O-Si) is formed n Thus, a 2-branched structure -A' is formed similar to the 2-branched structure -A.

[0108] In the conventional two-branched structure-B, the reactivity with silica is reduced.

[0109] 2-branched structure-A (structure of the present invention): (Rubber)-Si-O-Si-(Rubber)

[0110] 2-branched structure-A' (structure of the present invention): (Rubber)-Si-O-(Si-O) n -Si-(Rubber)

[0111] 2-branched structure-B (existing structure): (Rubber)-Si-(Rubber)

[0112] The ratio of these branched structures and the like can be determined by GPC in the production process.

[0113] In the present invention, in order to improve the drying process and storage stability, in the steps ii) and iii), when at least one silicon compound represented by formula (1) and / or formula (2) reacts with the active diene rubber, the reaction is carried out under conditions that minimize the generation of the di-branched structure -B. In addition, before the steam coagulation / drying in the step v), a halogenated silicon compound represented by formula (3) or an alkali metal compound represented by formula (4) may be added. The halogenated silicon compound or alkali metal compound is added under the condition that satisfies formula (5), is inactivated by impurities contained in the solvent or monomer, and is used to neutralize the lithium compound and the like produced as by-products in the reaction between the active diene rubber and the silicon compound, as well as the unreacted Si-Cl bonds and the by-product HCl.

[0114] Although (Rubber)-Si-OLi is not easy to condense, it forms (Rubber)-Si-OH after neutralization. It is easy to condense into (Rubber)-Si-O-Si-(Rubber), which improves storage stability.

[0115] The compounds represented by formula (1) and formula (2) may produce acidic compounds or alkaline compounds as by-products depending on the compounds used for the modification reaction, and it is necessary to change the neutralization method. In this case, it is preferred that 1.5≥[nX 1 +(4-q)X 2 ] / (L+M 2 )≥0.9. When it is below 0.9, the alkalinity increases and the condensation reaction is difficult to proceed. It is preferably above 0.95.

[0116] When the value is 1.5 or more, the acidity increases, which may lead to the problem of technical corrosion of manufacturing equipment. It is preferably 1.2 or less

[0117] The Mooney viscosity (MV for short, ML for short) of the diene rubber obtained in the present invention is 1+4 / 100℃ . ) is preferably in the range of 20 to 150. When it is less than 20, the breaking strength, wear resistance and rebound resilience deteriorate. On the other hand, when it exceeds 150, the processability and the like are reduced.

[0118] The content of 1,2-structure or 3,4-structure of the diene part of the diene rubber in the present invention is usually in the range of 20 to 80%. When abrasion resistance is important, the vinyl content is reduced, and when braking performance on wet roads is important, the vinyl content is increased.

[0119] The 1,2-structure or 3,4-structure of the diene part in the conjugated diene polymer of the diene rubber component 1 as the high molecular weight component is 20 to 70%, preferably 25 to 60%, and the 1,2-structure or 3,4-structure of the diene part in the conjugated diene polymer of the diene rubber component 2 as the low molecular weight component is 40 to 80%, preferably 45 to 75%.

[0120] As the ratio of diene rubber component 1 to diene rubber component 2, diene rubber component 2 is 10 to 90 phr, preferably 15 to 80 phr, relative to 1100 phr of diene rubber component. When it is less than 10 phr, the blending MV increases and the processability deteriorates. In addition, when it is more than 90 phr, the adhesiveness of the rubber composition increases and becomes difficult to handle.

[0121] An extender oil may be added to the polymerization reaction solution containing the diene rubber of the present invention. As the extender oil, those commonly used in the rubber industry may be used, and examples thereof include paraffin extender oils, aromatic extender oils, and cycloparaffin extender oils.

[0122] The pouring point of the extension oil is preferably -20 to 50°C, more preferably -10 to 30°C. If it is within this range, it is easy to extend and a rubber composition with an excellent balance between tensile properties and low heat build-up properties is obtained. The appropriate aromatic carbon content (CA%, Kurtz analysis method) of the extension oil is preferably 20% or more, more preferably 25% or more. In addition, the appropriate paraffin carbon content (CP%) of the extension oil is preferably 55% or less, more preferably 45%. When CA% is too small or CP% is too large, the tensile properties are insufficient. The content of polycyclic aromatic compounds in the extension oil is preferably less than 3%. This content is measured by the IP346 method (the inspection method of The Institute Petroleum in the UK).

[0123] The content of the extension oil is preferably 0 to 40 parts by weight, more preferably 5 to 30 parts by weight, relative to 100 parts by weight of the rubber composition. When the content of the extension oil is within this range, the viscosity of the rubber composition containing silica becomes moderate, and the balance between tensile properties and low heat build-up properties is excellent.

[0124] When the diene rubber of the present invention is used as a rubber composition for tires, it can be blended with natural rubber, isoprene rubber, butadiene rubber, emulsion polymerized styrene butadiene rubber, etc. within a range that hardly impairs the effects of the present invention, and after reinforcing agents such as silica and / or carbon black and various compounding ingredients are kneaded by a roll mill or a Banbury mixer, sulfur, a vulcanization accelerator, etc. are added to prepare tire rubber for treads, sidewalls, carcasses, etc. In addition, these compositions can also be used for industrial products such as belts and vibration damping rubbers.

[0125] When the diene rubber of the present invention is used in a tire, especially in a tire tread, a filler having a hydroxyl group on the surface, such as silica, is the best reinforcing material to be filled. In addition, carbon black may be used in combination. The filling amount of the filler is preferably 20 to 150 phr, more preferably 30 to 100 phr, relative to 100 phr of the total rubber component.

[0126] Examples of silica include dry-process silica, wet-process silica, colloidal silica, and precipitated silica. Among them, wet-process silica containing hydrated silicic acid as a main component is particularly preferred. These silicas may be used alone or in combination of two or more.

[0127] The particle size of the primary particles of silica is not particularly limited, and is 1 to 200 nm, more preferably 3 to 100 nm, and particularly preferably 5 to 60 nm. When the particle size of the primary particles of silica is within this range, the balance between tensile properties and low heat generation is excellent. It should be noted that the particle size of the primary particles can be measured by electron microscopy or specific surface area.

[0128] When rubber is added to the rubber composition of the present invention in order to further improve tensile properties and low heat build-up properties, it is preferred to add a silane coupling agent. Examples of the silane coupling agent include β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane, bis(3-triethoxysilylpropyl)tetrasulfide, bis(3-tri-isopropoxysilylpropyl)tetrasulfide, bis(3-tributoxysilylpropyl)tetrasulfide, γ-trimethoxysilylpropyldimethylthiocarbamoyl Tetrasulfides such as tetrasulfide, γ-trimethoxysilylpropylbenzothiazolyl tetrasulfide, bis(3-triethoxysilylpropyl)disulfide, bis(3-tri-isopropoxysilylpropyl)disulfide, bis(3-tributoxysilylpropyl)disulfide, γ-trimethoxysilylpropyldimethylthiocarbamoyl disulfide, and γ-trimethoxysilylpropylbenzothiazolyl disulfide.

[0129] In order to avoid scorching during kneading, the silane coupling agent preferably contains 4 or less sulfur atoms in one molecule. More preferably, it contains 2 or less sulfur atoms. These silane coupling agents can be used alone or in combination of two or more.

[0130] The amount of the silane coupling agent blended is preferably 0.1 to 30 parts by weight, more preferably 1 to 20 parts by weight, and particularly preferably 2 to 10 parts by weight, based on 100 parts by weight of silica.

[0131] Examples of carbon black include carbons of grades N110, N220, N330, N440, and N550. These carbon blacks may be used alone or in combination of two or more.

[0132] The specific surface area of ​​carbon black is not particularly limited, and is expressed as the nitrogen adsorption specific surface area (N 2 SA), preferably 5 to 200 m 2 / g, more preferably 50 to 150 m 2 / g, particularly preferably 80 to 130 m 2 / g. When the nitrogen adsorption specific surface area is within this range, the tensile properties are more excellent. In addition, the DBP adsorption amount of carbon black is not particularly limited, and is preferably 5 to 300 ml / 100 g, more preferably 50 to 200 ml / 100 g, and particularly preferably 80 to 160 ml / 100 g. When the DBP adsorption amount is within this range, a rubber compound composition with more excellent tensile properties is obtained. In addition, by using the adsorption specific surface area of ​​hexadecyltrimethylammonium bromide (CTAB) disclosed in Japanese Patent Publication No. 5-230290, the specific surface area is 110 to 170 m 2 / g, and the DBP (24M4DBP) oil absorption of 110-130ml / 100g after repeated compression 4 times under a pressure of 24,000psi is high-structure carbon black, which can improve wear resistance.

[0133] The amount of carbon black blended is 1 to 50 parts by weight, preferably 2 to 30 parts by weight, and particularly preferably 3 to 20 parts by weight, based on 100 parts by weight of the rubber component.

[0134] In the rubber compounding composition of the present invention, the vulcanizing agent can be used in an amount preferably within a range of 0.5 to 10 phr, more preferably 1 to 6 phr, based on 100 phr of the total rubber component.

[0135] Typical examples of the vulcanizing agent include sulfur, other sulfur-containing compounds, and peroxides.

[0136] In addition, a required amount of a vulcanization accelerator such as sulfenamide, guanidine, thiuram, etc. may be used together with the vulcanizing agent. Also, a required amount of zinc oxide, a vulcanizing aid, an antioxidant, a processing aid, etc. may be used.

[0137] Furthermore, the various compounding ingredients of the rubber compounding composition obtained using the diene rubber of the present invention are not particularly limited, but in order to further improve the processability during kneading or the balance of anti-wet skid properties, rebound resilience and wear resistance, in addition to various compounding ingredients such as vulcanizers, vulcanization accelerators, zinc oxide, vulcanization aids, scorch retardants, tackifiers, other fillers, etc. formulated in other extender oils or ordinary rubber compositions, a compatibilizer can also be added during kneading. The compatibilizer is an organic compound selected from, for example, epoxy-containing compounds, carboxylic acid compounds, carboxylic acid ester compounds, ketone compounds, ether compounds, aldehyde compounds, hydroxyl-containing compounds and amino-containing compounds, or a silicon compound selected from alkoxysilane compounds, siloxane compounds and aminosilane compounds.

[0138] Next, the present invention will be described in more detail by way of examples, but the present invention is not limited to these examples at all. It should be noted that the physical properties of the polymer were measured by the following methods.

[0139] The peak molecular weight (Mp) and peak area are calculated as follows. The molecular weight of the highest point of the peak of the GPC analysis of the conjugated diene polymer 1 immediately after polymerization is taken as the peak molecular weight, recorded as Mp1. After adding the silicon compound, peaks corresponding to the 2-branched structure, 3-branched structure, and 4-branched structure appear. The peak area corresponding to Mp1 after modification is taken as C Mp1 , the peak area with more than 2 branches is taken as C Mp1,2 to perform the calculation.

[0140] When the calculation is performed similarly based on the GPC chart after steam coagulation / drying, the rubber molecules to which the silicon compound is added to the terminal and the rubber molecules to which the silicon compound is added via the two-branched structure are condensed, C Mp1,D Less than C Mp1 , C Mp1,2<,D Greater than C Mp1,2< . C Mp1,2<,D Larger than C Mp1,2< , the storage stability and reactivity with silica increase.

[0141] In the present invention, Mp1 is 400 kg / mol or more.

[0142] The molecular weight at the highest point of the peak in the GPC analysis of the conjugated diene polymer 2 immediately after polymerization was taken as the peak molecular weight, which was recorded as Mp2. After the addition of the silicon compound, peaks corresponding to a 2-branched structure, a 3-branched structure, and a 4-branched structure appeared. The peak area corresponding to Mp2 after modification was taken as C Mp2 , the peak area with more than 2 branches is taken as C Mp2,2< to calculate.

[0143] When the calculation is performed similarly based on the GPC chart after steam coagulation / drying, the rubber molecules to which the silicon compound is added to the terminal and the rubber molecules to which the silicon compound is added via the two-branched structure are condensed, C Mp1,D The area of ​​C Mp2,2<,D The area of ​​C Mp1,2<,D The more C Mp1,2< The larger the particle size, the greater the storage stability and the reactivity with silica.

[0144] In the present invention, Mp2 is lower than 60 kg / mol.

[0145] The styrene unit content in the polymer is based on 1 The glass transition point (T g ) was measured using a differential scanning calorimeter (DSC) Model 7 manufactured by Perkin Elmer, under conditions of cooling to -100°C and then heating to 10°C / min.

[0146] The kneading characteristics and physical properties of the vulcanized rubber were measured by the following methods, and the Mooney viscosity of the rubber compounding composition was measured as follows.

[0147] The kneading of the vulcanized product for preparing the rubber compounding composition was carried out in accordance with JIS K 6299:2001 "Rubber - Method for preparing test specimens".

[0148] The kneading conditions (A kneading) of the rubber composition not containing a vulcanizing agent were as follows: a filling rate of about 65% (volume ratio), a rotor speed of 50 rpm, and a kneading start temperature of 90° C. using a Laboplast Mill Banbury mixer manufactured by Toyo Seiki Seisaku-sho, Ltd.

[0149] The kneading conditions for blending the vulcanizing agent into the rubber compound composition after A kneading (B kneading) were as follows: the vulcanizing agent was blended at room temperature using an 8-inch roll manufactured by Daihan Co., Ltd.

[0150] Regarding the temperature dispersion of the viscoelasticity test, "TA INSTRUMENTS viscoelasticity measuring device RSA3" was used in accordance with JIS K 7244-7:2007 "Plastics - Test methods for dynamic mechanical properties - Part 7: Torsional vibration - Non-resonance method" at a measuring frequency of 10 Hz, a measuring temperature of -50 to 80°C, a dynamic strain of 0.1%, and a heating rate of 4°C / min. The test was performed using a sample with a specimen shape of "5 mm wide × 40 mm long × 1 mm thick".

[0151] The smaller the tanδ(60°C), the greater the rebound resilience and the lower the heat build-up. The larger the tanδ(0°C), the better the wet grip performance.

[0152] (2) Regarding tensile properties, the breaking strength (T) when cut was measured according to JIS K6251:2004. B ), modulus, elongation at break, etc.

[0153] Regarding wear resistance, the wear amount of the vulcanized rubber compound composition was measured by Akron wear test B method according to JIS K6264-2: 2005 "Rubber vulcanized and thermoplastic rubber - Method for determining wear resistance - Part 2: Test method". The wear resistance of the control sample was set to 100, and the index was displayed as the wear resistance index. The larger the index, the better.

[0154] The Mooney viscosity was measured at 100°C in accordance with JIS K6300-2001. 1+4 / 100 ℃].

[0155] Example

[0156] Diene rubber component 1-1

[0157] The autoclave with an internal volume of 10L was fully substituted with dry nitrogen, 5500g of cyclohexane was added, and 215mg (1.17mmol) of 2,2-di(2-tetrahydrofuranyl)propane (DTHFP), 210g (2.02mol) of styrene, and 460g (8.50mol) of 1,3-butadiene were added to the autoclave. After adjusting the temperature in the autoclave to 25°C, 74.7mg (1.17mmol) of n-butyl lithium effective for polymerization was added to the autoclave to initiate polymerization. During polymerization, the temperature was adiabatically increased, and the maximum temperature reached 78°C. At this time, 30g of 1,3-butadiene was added, and polymerization was carried out for another 5 minutes. Here, 20mL of the polymerization solution was extracted from the autoclave into a container fully substituted with nitrogen for analysis, and then diluted and subjected to GPC analysis. Next, 0.324 g (1.17 mmol) of 3-diethylaminopropyltriethoxysilane was added to the autoclave and reacted for 15 minutes. The rubber was referred to as (diene rubber component 1-1). The styrene content of the diene rubber was 30% and the vinyl content was 44%. The Mp obtained by GPC analysis was 560 kg / mol.

[0158] Then, after the solution was mixed with the diene rubber component 2, the solvent was removed by steam coagulation and the mixture was dried using a roll at 110°C.

[0159] Diene rubber component 2-1

[0160] The autoclave with an internal volume of 10L was fully substituted with dry nitrogen, 5500g of cyclohexane was added, and 5.27g (114mmol) of 2,2-di(2-tetrahydrofuranyl)propane (DTHFP), 200g (1.92mol) of styrene, and 770g (14.24mol) of 1,3-butadiene were added to the autoclave. After adjusting the temperature in the autoclave to 25°C, 1.83g (29mmol) of n-butyllithium was added to the autoclave to initiate polymerization. During polymerization, the temperature was adiabatically increased, and the maximum temperature reached 88°C. At this time, 30g of 1,3-butadiene was added, and polymerization was carried out for another 5 minutes. Here, 20mL of the polymerization solution was extracted from the autoclave into a container fully substituted with nitrogen for analysis, and then diluted and subjected to GPC analysis. Next, 7.93 g (28.6 mmol) of 3-diethylaminopropyltriethoxysilane was added to the autoclave and reacted for 15 minutes. The remaining solution was desolventized by steam coagulation and dried with a roller at 110°C. The rubber was used as [Diene Rubber Component 2-1]. The styrene content in the diene rubber was 21%. The vinyl content was 59%. The Mp obtained by GPC analysis was 34 kg / mol.

[0161] Diene rubber component 2-2

[0162] [Diene rubber component 2-2] was produced by the same process as [Diene rubber component 2-1] except that the 2,2-di(2-tetrahydrofuryl)propane (DTHFP) used in [Diene rubber component 2-1] was increased to 25.6 g (553 mmol), the n-butyl lithium was increased to 8.89 g (141 mmol), and the 3-diethylaminopropyltriethoxysilane was increased to 38.5 g (139 mmol). The styrene content in the diene rubber was 21%. The vinyl content was 58%. The Mp obtained by GPC analysis was 7 kg / mol.

[0163] Diene rubber component 2-3

[0164] [Diene rubber component 2-3] was produced by the same process as [Diene rubber component 2-1] except that the amount of 2,2-di(2-tetrahydrofuryl)propane (DTHFP) used in [Diene rubber component 2-1] was increased to 10.5 g (118 mmol). The styrene content in the diene rubber was 20%. The vinyl content was 73%. The Mp obtained by GPC analysis was 38 kg / mol.

[0165] The [diene rubber component 1-1], [diene rubber component 2-1], [diene rubber component 2-2], [diene rubber component 2-3] and emulsion polymerized ESBR (commercially available JSR#1723 was used as it is) prepared in the examples were mixed in the proportions shown in Table 2, steam coagulated, and dried by hot rolls. The vulcanization properties were evaluated according to the formulation of the vulcanization properties in Table 1. The evaluation results are also recorded in Table 2.

[0166] Table 2 shows the blended MV and tensile strength, elongation at break, M 300 / M 100 Modulus ratio, Akron wear resistance, and dynamic viscoelasticity test results. The physical property values ​​shown as indices are set at 100 for Comparative Example 2, and the larger the value is for all items, the better the physical properties are. Compared with Comparative Example 2, which is an emulsion-polymerized SBR commonly used in tire applications, the tanδ (0°C) of the dynamic viscoelasticity test corresponding to wet grip performance and the tanδ (60°C) corresponding to low fuel consumption performance in Example 1, Example 2, and Comparative Example 1 are all better than Comparative Example 2. Although the blended MV is slightly higher, the higher the reinforcement with silica, the larger the value of the modulus ratio, and the higher the correlation with Akron wear resistance.

[0167] When Mp2 is less than 10 kg / mol as compared with Comparative Example 1, the diene rubber component 2 contributes to the improvement of processability, but the effect of improving vulcanization properties is small.

[0168] The results of these physical property evaluations and the like indicate that the rubber composition is an excellently balanced rubber compounding composition in terms of fuel economy, wear resistance, wet grip performance, and processability.

[0169] Table 1

[0170] Table 1 Sulfide Compounding Prescriptions

[0171] Comply with prescription phr rubber 100 Silicon dioxide 70 Silane coupling agent Si69 6 Polyethylene glycol PEG4000 4 Carbon Black N339 4 Zinc Oxide 3 Stearic acid 2 Antioxidant 6C 1 Vulcanization accelerator D 0.5 Vulcanization accelerator CZ 2.5 sulfur 1.5 total 194.5

[0172] Cf-1) phr; parts per hundred rubber

[0173] Cf-2)Si69; bis(3-triethoxysilylpropyl)tetrasulfide

[0174] Cf-3)PEG4000; Polyethylene glycol 4000

[0175] Cf-4)6C; N-phenyl-N'-(1,3-dimethylbutyl)-p-phenyldiamine

[0176] Cf-5)D; N,N-diphenylguanidine

[0177] Cf-6)CZ; N-cyclohexyl-2-benzothiazolylsulfenamide

[0178] Table 2

[0179] Table 2 Vulcanization properties of diene rubber compositions

[0180]

[0181]

[0182]

[0183] Diene rubber component 1-2

[0184] The autoclave with a capacity of 5 L was fully replaced with dry nitrogen, 2890 g of cyclohexane was added, and 100 mg (0.544 mmol) of 2,2-di(2-tetrahydrofuranyl)propane (DTHFP), 110 g of styrene, and 243 g of 1,3-butadiene were added to the autoclave. After adjusting the temperature in the autoclave to 40°C, 87.1 mg (1.36 mmol) of n-butyl lithium effective for polymerization was added to the autoclave to initiate polymerization. During polymerization, the temperature was adiabatically increased, and the maximum temperature reached 78°C. At this time, 16 g of 1,3-butadiene was added, and polymerization was continued for another 5 minutes. Next, 377 mg (1.36 mmol) of 3-diethylaminopropyltriethoxysilane was added to the autoclave and reacted for 15 minutes. This polymerization was repeated 6 times, and the total amount was added to one tank and stirred evenly. This rubber was referred to as [Diene Rubber Component 1-2]. The diene rubber had a styrene content of 30% and a vinyl content of 47%. The Mp obtained by GPC analysis was 568 kg / mol.

[0185] Next, the solution was mixed with the diene rubber component 2, and then the solvent was removed by steam coagulation, followed by drying with a roll at 110°C.

[0186] Diene rubber component 2-4

[0187] The autoclave with an internal volume of 10 L was fully replaced with dry nitrogen, 5500 g of cyclohexane was added, and 5.27 g (114 mmol) of 2,2-di(2-tetrahydrofuranyl)propane (DTHFP), 200 g (1.92 mol) of styrene, and 770 g (14.24 mol) of 1,3-butadiene were added to the autoclave. After adjusting the temperature in the autoclave to 25°C, 1.83 g (29 mmol) of n-butyl lithium was added to the autoclave to initiate polymerization. During polymerization, the temperature was adiabatically increased, and the maximum temperature reached 83°C. At this time, 30 g of 1,3-butadiene was added, and polymerization was carried out for another 5 minutes. Next, 7.93 g (28.6 mmol) of 3-diethylaminopropyltriethoxysilane was added to the autoclave and reacted for 15 minutes. The solution was stored as a solution. The rubber was referred to as [Diene Rubber Component 2-4]. The styrene content of the diene rubber was 21%, the vinyl content was 69%, and the Mp obtained by GPC analysis was 38 kg / mol.

[0188] Diene rubber component 2-5

[0189] [Diene rubber component 2-5] was produced by the same process as [Diene rubber component 2-4] except that 3-diethylaminopropyltriethoxysilane used in [Diene rubber component 2-4] was replaced with 2.43 g (14.3 mmol) of silicon tetrachloride. The styrene content in the diene rubber was 20%. The vinyl content was 68%. The Mp obtained by GPC analysis was 40.0 kg / mol.

[0190] Diene rubber component 2-6

[0191] [Diene rubber component 2-6] was produced by the same process as [Diene rubber component 2-4] except that 3-diethylaminopropyltriethoxysilane used in [Diene rubber component 2-4] was replaced with 4.25 g (14.4 mmol) of octamethylcyclotetrasiloxane (D4). The styrene content in the diene rubber was 20%. The vinyl content was 70%. The Mp obtained by GPC analysis was 47 kg / mol.

[0192] Regarding the [diene rubber component 1-2], [diene rubber component 2-4], [diene rubber component 2-5], [diene rubber component 2-6], TDAE (aromatic oil), and emulsion polymerized ESBR (commercially available JSR#1723 was used as it is) prepared in the examples, in Examples 3 to 5, 20 phr of each of the diene rubber components 2-4 to 2-6 was mixed with 100 phr of the diene rubber component 1-2, and then the solvent was removed by steam coagulation, and the mixture was roll-dried at 110° C. In Examples 6 to 8, 40 phr of each of the diene rubber components 2-4 to 2-6 was mixed with the diene rubber component 1-2, and then the solvent was removed by steam coagulation, and the mixture was roll-dried at 110° C.

[0193] From the GPC analysis chart, the high molecular weight component and the low molecular weight component were separated by a simple method of dividing the peak by a vertical line, and the ratio of the diene rubber component 1 to the diene rubber component 2 was calculated based on the area and is shown in Table 4.

[0194] The sulfide properties were evaluated according to the sulfide property formulation in Table 3. The evaluation results are also recorded in Table 4.

[0195] Table 4 shows the blended MV and tensile strength, elongation at break, modulus ratio of M300 / M100, Akron wear resistance, and dynamic viscoelasticity test results. The physical property values ​​shown as indices are set at 100 for Comparative Example 4, and the larger the value, the better the physical property.

[0196] Compared with Comparative Example 4, which is an emulsion-polymerized SBR generally used in tire applications, Examples 3 to 8 have higher tensile strengths and are equal to or higher than the elongation at break.

[0197] Compared with Comparative Example 4, in Examples 3 to 8, the modulus ratio of the reactivity with silica is large, and both the Akron wear test and the dynamic viscoelasticity test are significantly improved.

[0198] Regarding the effect of the type of the terminal modifier of the diene rubber component 2, even when comparing Examples 3 to 5 in which 20 phr of the diene rubber component was added to 1100 phr of the diene rubber component and Examples 6 to 8 in which 40 phr of the diene rubber component was added, no significant difference was observed among the examples.

[0199] The results of these physical property evaluations and the like indicate that the rubber composition is an excellently balanced rubber compounding composition in terms of fuel economy, wear resistance, wet grip performance, and processability.

[0200] Table 3

[0201] Table 3 Sulfide Compounding Prescriptions

[0202]

[0203] Table 4

[0204] Table 4 Vulcanization properties of diene rubber compositions

[0205]

[0206]

Claims

1. A diene rubber composition, comprising: providing a diene rubber component 1 obtained by terminally modifying a conjugated diene polymer 1 with at least one silicon compound represented by formula (1) and / or formula (2) and a diene rubber component 2 obtained by terminally modifying a conjugated diene polymer 2 with at least one silicon compound represented by formula (1) and / or formula (2) to a hydrolysis step, followed by drying, to obtain a diene rubber composition; The conjugated diene polymer 1 is obtained by polymerizing a conjugated diene compound and an aromatic vinyl compound, and has a peak molecular weight of 400k to 2,000 kg / mol in terms of polystyrene. The conjugated diene polymer 2 is obtained by polymerizing a conjugated diene compound and an aromatic vinyl compound, and has a peak molecular weight of 15k to 60kg / mol in terms of polystyrene. Chemical formula 1: (X 1 ) n (R 1 O) m -Si-(R 2 ) 4-n-m Formula (1), In the formula, R 1 and R 2 are independently an alkyl group, an aromatic group or an allyl group having 1 to 12 carbon atoms, or an alkyl group, an aromatic group or an allyl group containing an oxygen atom and / or a nitrogen atom in these groups, X 1 is iodine, bromine or chlorine, n and m are 0, 1, 2, 3 or 4 respectively, Chemical formula 2: In the formula, R 3 ~R 8 Each independently represents an alkyl group, an aromatic group or an allyl group having 1 to 12 carbon atoms, or an alkyl group, an aromatic group or an allyl group containing an oxygen atom and / or a nitrogen atom in these groups. In addition, R 7 and R 8 For the ring structure, p is a number between 1.5 and 1,000 with an interval of 0.

5.

2. The diene rubber composition according to claim 1, wherein The 1,2-structure or 3,4-structure of the diene part in the diene rubber component 1 is 20 to 70%, and the weight ratio of the aromatic vinyl compound component in the diene rubber component 1 is 10 to 50%. The 1,2-structure or 3,4-structure of the diene portion in the diene rubber component 2 is 40 to 80%, and the weight ratio of the aromatic vinyl compound component in the diene rubber component 2 is 5 to 35%.

3. The diene rubber composition according to claim 1 or 2, wherein: The ratio of the diene rubber component 1 to the diene rubber component 2 is 10 to 90 phr of the diene rubber component 1 relative to 100 phr of the diene rubber component 1.

4. A rubber compounding composition comprising at least 20 to 150 phr of silica based on 100 phr of the total rubber component comprising at least 20 phr of the diene rubber composition according to claim 2 or 3.

5. A rubber compounding composition comprising at least 20 to 150 phr of silica and 5 to 30 phr of carbon black, based on 100 phr of the total rubber component comprising at least 20 phr of the diene rubber composition according to claim 2 or 3.

6. A method for producing a diene rubber composition, i) in the presence of an organic lithium compound, initiating polymerization of a conjugated diene compound and an aromatic vinyl compound in a hydrocarbon; ii) the conjugated diene polymer 1 having a peak molecular weight of 400 k to 2,000 kg / mol in terms of polystyrene after polymerization in i) is polymerized with at least one silicon compound represented by formula (1) and / or formula (2), and then immediately subjected to terminal modification to produce a diene rubber component 1; iii) the conjugated diene polymer 2 having a peak molecular weight of 15k to 60 kg / mol in terms of polystyrene after polymerization in i) is polymerized via at least one silicon compound represented by formula (1) and / or formula (2), and then immediately subjected to terminal modification to produce a diene rubber component 2; iv) subjecting the obtained diene rubber component 1 and diene rubber component 2 to a hydrolysis step, preferably to steam coagulation, and then drying; Chemical formula 3: (X 1 ) n (R 1 O) m -Si-(R 2 ) 4-n-m Formula (1), In the formula, R 1 and R 2 are alkyl groups, aromatic groups or allyl groups having 1 to 12 carbon atoms, or alkyl groups, aromatic groups or allyl groups containing oxygen atoms and / or nitrogen atoms in these groups, X 1 is a halogen atom of iodine, bromine or chlorine, n and m are 0, 1, 2, 3 or 4, Chemical formula 4: In the formula, R 3 ~R 8 Each of them is independently an alkyl group, an aromatic group or an allyl group having 1 to 12 carbon atoms, or an alkyl group, an aromatic group or an allyl group containing an oxygen atom and / or a nitrogen atom in these groups, and R 7 and R 8 For the ring structure, p is a number between 1.5 and 1,000 with an interval of 0.

5.

7. The method according to claim 6, wherein: In the presence of an organic lithium compound and a secondary amine compound, polymerization is initiated for the diene rubber component 1 alone or for both the diene rubber component 1 and the diene rubber component 2.

8. The method according to claim 6 or 7, wherein: When the diene rubber component 1 is polymerized, isoprene is prepolymerized with an organic lithium compound, and then a conjugated diene compound other than isoprene and an aromatic vinyl compound are polymerized.

9. The method according to any one of claims 6 to 8, wherein: After the diene rubber component 1 is polymerized, a conjugated diene compound, an aromatic vinyl compound, and an optional 1,2-structure or 3,4-structure modifier of the diene moiety are then added, and polymerization is reinitiated in the presence of an organic lithium compound.

10. The method according to any one of claims 6 to 9, wherein: After step iii) and before step iv), a silicon halide compound represented by formula (3) or an alkali metal compound represented by formula (4) in an amount satisfying the condition of formula (5) is added, and then steam coagulation / drying in step iv) is performed. Chemical formula 5: (R 9 ) q -M 1 -(X 2 ) 4-q Formula (3), Where M 1 is a silicon atom, R 9 is an alkyl group, an aromatic group or an allyl group having 1 to 12 carbon atoms, X 2 is a halogen atom of iodine, bromine or chlorine, q is 0 or 1, Chemical formula 6: R 10 -OM 2 Formula (4) Where M 2 is an alkali metal atom, preferably a lithium atom, a sodium atom or a potassium atom, R 10 is an alkyl group, an aromatic group, an allyl group or an acyl group having 1 to 12 carbon atoms, Chemical formula 7: 1.5≥[nX 1 +(4-q)X 2 ] / (L+M 2 )≥0.9 Formula (5), Wherein, L is the molar number of the organic lithium compound added to the polymerization initiator, M 2 is the number of moles of the alkali metal compound represented by formula (4), X 1 is the number of moles of the silicon compound represented by formula (1), X 2 is the number of moles of the silicon halide compound represented by formula (3), n is the same as n in the silicon compound represented by formula (1), and q is the same as q in the silicon halide compound represented by formula (3).

11. The method according to any one of claims 6 to 10, wherein: The ratio of the diene rubber component 1 to the diene rubber component 2 is such that the diene rubber component 2 is 10 to 90 phr relative to 100 phr of the diene rubber component 1.