Ultraviolet curable silicone composition
By optimizing the coordination of polyorganosiloxane, hydrosiloxane and platinum-based catalyst, the problem of insufficient curability of the ultraviolet curable silicone composition in the light-unirradiated part and in the thickness direction is solved, and a stable curing effect is achieved. Suitable for sealing materials for electrical and electronic components.
Patent Information
- Application Number
- CN202380028741.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-31
- Filing Date
- 2023-03-22
- Publication Date
- 2024-11-05
AI Technical Summary
The existing ultraviolet curable silicone compositions have insufficient curability in the part that is not irradiated with light and in the thickness direction, and the existing solutions require additional equipment or complex operation, resulting in unstable quality.
By using a prescribed content of polyorganosiloxane, polyorganohydrogensiloxane and platinum-based catalyst, combined with ultraviolet irradiation and specific process treatment, the curability of the composition is optimized to ensure sufficient part of the light that is not irradiated and in the thickness direction. Curing.
Excellent curability in the part that is not irradiated with light and in the thickness direction is achieved, and a stable quality ultraviolet curable silicone composition is provided, which is suitable for sealing materials for electrical and electronic components.
Smart Images

Figure BDA0005050130490000081 
Figure BDA0005050130490000191 
Figure BDA0005050130490000211
Abstract
Description
Technical Field
[0001] The present invention relates to an ultraviolet curable silicone composition, and more particularly to an ultraviolet curable silicone composition whose cured product can be suitably used as a sealing material for electric parts, electronic parts, and the like. Background Art
[0002] Silicone compositions can be used as elastic adhesives, sealing materials, coating materials, electrical insulating sealing materials, etc. in semiconductor elements such as ICs and LSIs, electrical / electronic components such as capacitors and resistors, and optical components such as lenses, mirrors, filters, and prisms, etc., from the perspective of excellent heat resistance and good adhesion and bonding to these components. In particular, ultraviolet curable addition reaction type silicone compositions utilizing hydrosilylation reactions are widely used because they are cured by ultraviolet irradiation for a short time, and thus have excellent productivity and can bond components well to each other.
[0003] As such an ultraviolet-curable silicone composition, Patent Document 1 discloses an ultraviolet-curable organopolysiloxane gel composition for a vibration-damping material for an objective lens driving device, which contains (A) an organopolysiloxane having an average of more than 0.1 alkenyl groups bonded to silicon atoms in one molecule, (B) an organohydrogenpolysiloxane having more than 2 hydrogen atoms bonded to silicon atoms in one molecule, and (C) a photoactive platinum complex curing catalyst in a specified ratio, and indicates that a composition having both the advantages of a specified polymer design and rapid curing properties based on ultraviolet irradiation can be prepared.
[0004] In addition, Patent Document 2 discloses an ultraviolet-curable liquid silicone composition for an image display device having a predetermined viscosity, which contains (A) an organopolysiloxane having a viscosity of 50 to 100,000 mPa·s at 25° C. and containing at least two alkenyl groups in one molecule, (B) an organohydrogenpolysiloxane such as a linear organohydrogenpolysiloxane having hydrogen atoms (Si—H groups) directly bonded to silicon atoms only at the ends of both sides of the molecular chain, and (C) one or more photoactive hydrosilylation reaction catalysts selected from a specific compound group, and is shown to be capable of being cured for several minutes to several tens of minutes under mild temperature conditions of 100° C. or less, and to provide a cured product having excellent mechanical and optical properties.
[0005] Since this type of UV-curable silicone composition is cured by irradiation with ultraviolet rays, there is a problem that the composition flows during the period until it is completely cured or the portion not irradiated with ultraviolet rays is not fully cured. In order to solve this problem, various methods for curing UV-curable silicone compositions have been proposed. For example, Patent Document 3 discloses a curing method, which includes the following steps: for the purpose of curing the composition while maintaining the shape at the initial stage of heating, the composition is irradiated with light having a specific emission spectrum and then heated. In addition, Patent Document 4 discloses a method for curing a composition, which includes: a first step, for the purpose of uniformly curing even portions not irradiated with light or thick molded objects, the composition is irradiated with ultraviolet rays to increase the catalytic activity of a photoactive platinum complex curing catalyst; and a second step, applying the composition obtained in the first step to a desired location and curing it.
[0006] Prior art literature
[0007] Patent Literature
[0008] Patent Document 1: Japanese Patent Application Publication No. 2003-213132
[0009] Patent Document 2: Japanese Patent Application Publication No. 2019-210351
[0010] Patent Document 3: Japanese Patent Application Publication No. 2012-121960
[0011] Patent Document 4: Japanese Patent Application Publication No. 2013-87199 Summary of the invention
[0012] Problems to be solved by the invention
[0013] Although the ultraviolet curable silicone compositions disclosed in Patent Documents 1 and 2 are cured by ultraviolet irradiation to show predetermined mechanical and optical properties, there are problems such as insufficient curing properties in the portion not irradiated with light and in the thickness direction, and unstable quality of the cured product. In addition, since the curing methods disclosed in Patent Documents 3 and 4 require additional equipment or complicated operations, there is a need for an ultraviolet curable silicone composition that can provide a cured product with stable quality without using these methods.
[0014] An object of the present invention is to provide an ultraviolet curable silicone composition having excellent curability in a portion not irradiated with light and in the thickness direction.
[0015] Means for solving problems
[0016] The present inventors have conducted intensive studies to solve the above problems and have found that the curability of the composition can be improved by using predetermined alkenyl group-containing polyorganosiloxane and polyorganohydrogensiloxane and controlling the amount of the platinum-based catalyst to be incorporated within a predetermined range, thereby completing the present invention.
[0017] The present invention relates to the following [1] to
[11] .
[0018] [1] A UV-curable silicone composition comprising: (A) a polyorganosiloxane having at least two alkenyl groups in one molecule and an average alkenyl content of 0.08 mmol / g or more, (B) a polyorganohydrogensiloxane having at least three hydrogen atoms bonded to silicon atoms in one molecule, and (C) a platinum-based catalyst activated by ultraviolet light, wherein the component (B) comprises (B1) a catalyst containing R c1 2HSiO 1 / 2 Unit (where R c1 are independently C1-C6 alkyl or C6-C 20 Aryl) and SiO 4 / 2 The amount of the component (C) in the composition is 8 to 400 ppm based on the mass of the platinum metal. The viscosity of the composition at 23° C. is 10 to 10,000 mPa·s. The composition is irradiated with a yellow light in a room with a diameter of 7.0 mm and an illumination of 100 mW / cm 2 , ultraviolet rays with a wavelength of 365 nm for 45 seconds, and then stored at 23° C. for 16 hours to obtain a cured product, and the cured diameter of the obtained cured product at a depth of 1.8 mm was greater than 10.8 mm.
[0019] [2] The ultraviolet curable silicone composition according to [1], wherein the component (A) contains a linear polyorganosiloxane, and the alkenyl content of the component (A) is 0.09 to 1.8 mmol / g on average.
[0020] [3] The ultraviolet curable silicone composition according to [1] or [2], wherein the amount of component (C) in the composition is 40 to 350 ppm based on the mass of platinum metal.
[0021] [4] The ultraviolet curable silicone composition according to any one of [1] to [3], wherein the component (B1) comprises 3 to 6 SiO 4 / 2 Unit and 6 to 12 R c1 2HSiO 1 / 2 Polyorganohydrogensiloxane formed by unit bonding.
[0022] [5] The ultraviolet curable silicone composition according to any one of [1] to [4], wherein the component (C) is a platinum-based catalyst having a cyclic diene compound as a ligand.
[0023] [6] The ultraviolet curable silicone composition according to any one of [1] to [5], wherein the number of moles of hydrogen atoms bonded to silicon atoms in the component (B) is H B The number of moles of alkenyl groups in component (A) Vi A The ratio of H B / Vi A The ratio is 0.30~3.5.
[0024] [7] A potting material comprising the ultraviolet curable silicone composition according to any one of [1] to [6].
[0025] [8] The potting material according to [7], which is used for connector pins (Japanese: コネクタピン).
[0026] [9] A sealing material comprising a cured product of the ultraviolet curable silicone composition according to any one of [1] to [6].
[0027]
[10] The sealing material according to [9], which is used for electric parts or electronic parts.
[0028]
[11] The sealing material according to
[10] , wherein the electric component or the electronic component is a connector having connector pins.
[0029] Effects of the Invention
[0030] According to the present invention, there can be provided an ultraviolet curable silicone composition having excellent curability in a portion not irradiated with light and in the thickness direction. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 This is a photograph of the device for measuring the cured diameter taken from above in a yellow light room.
[0032] Figure 2 Observed from above Figure 1 Schematic diagram of the device.
[0033] Figure 3 yes Figure 2 A-A' line cross-sectional view.
[0034] Figure 4 Yes Figure 2 and 3 Schematic diagram illustrating the cured area and cured diameter after ultraviolet irradiation.
[0035] Figure 5This is a graph showing the relationship between the amount of platinum blended and the solidification diameters of the upper surface (depth 0 mm) and the lower surface (depth 1.8 mm) for Examples 1 to 10 and Comparative Example 5.
[0036] Figure 6 This is a graph showing the relationship between the amount of platinum blended and the cured area of the non-irradiated portion of the upper surface (depth 0 mm) and the lower surface (depth 1.8 mm) for Examples 1 to 10 and Comparative Example 5. DETAILED DESCRIPTION
[0037] The ultraviolet curable silicone composition comprises: (A) a polyorganosiloxane having at least two alkenyl groups in one molecule and an average alkenyl content of 0.08 mmol / g or more, (B) a polyorganohydrogensiloxane having at least three hydrogen atoms bonded to silicon atoms in one molecule, and (C) a platinum catalyst activated by ultraviolet light, wherein the component (B) comprises (B1) a catalyst containing R c1 2HSiO 1 / 2 Unit (where R c1 are independently C1-C6 alkyl or C6-C 20 Aryl) and SiO 4 / 2 The amount of the component (C) in the composition is 8 to 400 ppm based on the mass of the platinum metal. The viscosity of the composition at 23° C. is 10 to 10,000 mPa·s. The composition is irradiated with a yellow light in a room with a diameter of 7.0 mm and an illumination of 100 mW / cm 2 , 365nm wavelength ultraviolet light for 45 seconds, and then stored at 23°C for 16 hours to obtain a cured product, the cured diameter of the obtained cured product at a depth of 1.8mm was 10.8mm or more. The ultraviolet curable silicone composition of the present invention has excellent curability in the non-irradiated part and in the thickness direction.
[0038] In the case of application in this specification, "organic group" refers to a group containing carbon. The valence of the organic group is expressed by recording it as "n-valent" with n as an arbitrary natural number. Therefore, for example, "monovalent organic group" refers to a group containing carbon with only one bond. The bond may have elements other than carbon. Even if the valence is not specifically indicated, those skilled in the art can understand the appropriate valence according to the context.
[0039] When used in this specification, "hydrocarbon group" refers to a group containing carbon and hydrogen and at least one hydrogen atom is separated from the molecule. The hydrocarbon group is not particularly limited and may be substituted by one or more substituents. Examples of the hydrocarbon group include hydrocarbon groups having 1 to 20 carbon atoms, such as aliphatic hydrocarbon groups, aromatic hydrocarbon groups, etc. The above-mentioned "aliphatic hydrocarbon group" may be any of linear, branched or cyclic, and may be any of saturated or unsaturated. In addition, the hydrocarbon group may also contain one or more ring structures. It should be noted that the hydrocarbon group may have one or more nitrogen atoms (N), oxygen atoms (O), sulfur atoms (S), silicon atoms (Si), amide bonds, sulfonyl bonds, siloxane bonds, carbonyl groups, carbonyloxy groups and other heteroatoms or structures containing heteroatoms at its end or in the molecular chain.
[0040] In the context of the present specification, the substituent of the "hydrocarbon group" is not particularly limited, and examples thereof include: a halogen atom; a C 1-6 Alkyl, C 2-6 Alkenyl, C 2-6 Alkynyl, C 3-10 Cycloalkyl, C 3-10 unsaturated cycloalkyl, 5- to 10-membered heterocyclic group, 5- to 10-membered unsaturated heterocyclic group, C 6-10 Aryl and 5- to 10-membered heteroaryl groups.
[0041] In the present specification, unless otherwise specified, the alkyl group and the phenyl group may be unsubstituted or substituted. The substituent of the group is not particularly limited, and examples thereof include halogen atoms, C 1-6 Alkyl, C 2-6 Alkenyl and C 2-6 One or more alkynyl groups.
[0042] When describing the structure of a siloxane compound in the present specification, the structural units of the siloxane compound may be described using the following abbreviations. Hereinafter, these structural units may be referred to as "M unit", "D unit" and the like.
[0043] M: (CH3)3SiO 1 / 2
[0044] M H :H(CH3)2SiO 1 / 2
[0045] M Vi :CH2=CH(CH3)2SiO 1 / 2
[0046] D: (CH3)2SiO 2 / 2
[0047] D H :H(CH3)SiO 2 / 2
[0048] D Vi :CH2=CH(CH3)SiO 2 / 2
[0049] T: CH3SiO 3 / 2
[0050] Q:SiO 4 / 2 (Tetrafunctional)
[0051] The siloxane compound is a compound constructed by combining the above structural units, and may at least partially contain a portion in which the methyl group of the above structural unit is substituted by a halogen such as fluorine, a hydrocarbon group such as phenyl, or other substituents. H 20 D 20 In the case of D H The T unit is followed by 20 D units, but the units can be arranged arbitrarily. The siloxane compound can take various structures three-dimensionally through the T unit or the Q unit.
[0052] <(A) Polyorganosiloxane having at least two alkenyl groups in one molecule and an average alkenyl group content of 0.08 mmol / g or more>
[0053] The (A) component is a polysiloxane having at least two alkenyl groups in one molecule and an average alkenyl content of 0.08 mmol / g or more. The (A) component functions as a base polymer of a UV-curable silicone composition. The alkenyl group may be bonded to the molecular chain end of the main chain of the molecule, to a side chain in the middle of the molecular chain, or to both. In this specification, the main chain of the molecule refers to the relatively longest bond chain in the molecule. The molecular structure of the (A) component is not particularly limited as long as it is a structure with siloxane bonds as the main skeleton, and may be any of a linear, branched, cyclic or three-dimensional mesh structure, and the siloxane skeleton may also be interrupted by a divalent organic group. The (A) component may be used alone or in combination of two or more.
[0054] (A) component has at least 2 alkenyl groups in one molecule. (A) component can be a mixture of multiple polyorganosiloxanes having at least 2 alkenyl groups in one molecule. Among them, from the viewpoint of forming a stable three-dimensional structure by cross-linking reaction during curing and imparting appropriate hardness to the cured product, (A) component preferably includes a straight-chain polyorganosiloxane, and more preferably includes a straight-chain polyorganosiloxane having 1 alkenyl group at each end of the main chain of the molecule. In this case, (A) component preferably includes a straight-chain polyorganosiloxane of 30% by mass or more relative to 100% by mass of (A) component, more preferably includes 50% by mass or more, and further preferably includes 80% by mass or more. The upper limit of the content of the straight-chain polyorganosiloxane relative to 100% by mass of (A) component is 100% by mass.
[0055] As long as the alkenyl group has a carbon-carbon double bond and is capable of an addition reaction, there is no particular limitation. The number of carbon atoms of the alkenyl group is preferably 2 to 20, more preferably 2 to 8, and further preferably 2 to 6. The alkenyl group may have a branched structure or a ring structure. The position of the carbon-carbon double bond in the hydrocarbon constituting the alkenyl group may be at any position. From the aspect of reactivity, the carbon-carbon double bond is preferably at the end of the group. As a preferred example of the alkenyl group, vinyl can be cited from the aspect of easy synthesis of polyorganosiloxane.
[0056] The alkenyl content of component (A) is an average of 0.08 mmol / g or more, preferably 0.08 to 11.0 mmol / g, more preferably 0.09 to 5.0 mmol / g, further preferably 0.09 to 1.8 mmol / g, and particularly preferably 0.1 to 0.5 mmol / g. By making the alkenyl content within the above range, an ultraviolet curable silicone composition having excellent curability and storage stability in the non-irradiated part and in the thickness direction can be prepared. Here, when component (A) is a mixture of multiple polyorganosiloxanes, the alkenyl content of component (A) is the average value of the mixture.
[0057] The alkenyl content of the component (A) can be determined from the absorbance (near 2,150 nm) of the CH2=CH- group using a spectrophotometer.
[0058] In one embodiment of the present invention, component (A) has at least two alkenyl groups bonded to silicon atoms in one molecule. Component (A) forms a network structure by an addition reaction with a hydrosilyl group (Si—H group) of component (B) described later. Component (A) typically has at least two alkenyl-containing siloxane units represented by general formula (1) in the molecule.
[0059] R 1 m R 2 n SiO(4-m-n) / 2 (1)
[0060] (Where,
[0061] R 1 It is an unsubstituted or substituted monovalent hydrocarbon group having no aliphatic unsaturated bond;
[0062] R 2 is alkenyl;
[0063] m is an integer from 0 to 2;
[0064] n is an integer of 1 to 3, wherein m+n is 1 to 3. )
[0065] R 1 is an unsubstituted or substituted monovalent hydrocarbon group having no aliphatic unsaturated bond. 1 Examples include: alkyl groups, such as C1-C6 alkyl groups (such as methyl, ethyl, propyl, etc.); cycloalkyl groups, such as C3-C 10 Cycloalkyl (e.g. cyclohexyl, etc.); aryl, such as C6~C 20 Aryl (e.g., phenyl, tolyl, xylyl, naphthyl, anthracenyl, etc.); aralkyl, e.g., C7-C 13 Aralkyl (e.g., 2-phenylethyl, 2-phenylpropyl, etc.); substituted hydrocarbon group, such as halogen-substituted hydrocarbon group (e.g., chloromethyl, chlorophenyl, 3,3,3-trifluoropropyl, etc.). From the perspective of ease of synthesis, alkyl groups are preferred, among which methyl, ethyl and propyl groups are preferred, and methyl groups are more preferred. In order to adjust the refractive index, aryl groups may be used in combination, among which phenyl groups are preferred from the perspective of ease of synthesis.
[0066] From the viewpoint of obtaining an ultraviolet curable silicone composition having excellent curability and storage stability, the component (A) preferably contains a linear polyorganosiloxane having one alkenyl group at each end of the molecular main chain. In one embodiment of the present invention, the linear polyorganosiloxane can be represented by formula (I), for example.
[0067] [Chemistry 1]
[0068]
[0069] (Where,
[0070] R a1 are independently C2-C6 alkenyl,
[0071] R b1 are independently C1-C6 alkyl or C6-C 20 Aryl,
[0072] n1 is a number that makes the average alkenyl content of the linear polyorganosiloxane 0.08 mmol / g or more)
[0073] Examples of C2-C6 alkenyl groups include vinyl, allyl, 3-butenyl, and 5-hexenyl. Examples of C1-C6 alkyl groups include methyl, ethyl, propyl, butyl, pentyl, and hexyl. 20 Examples of the aryl group include phenyl, naphthyl, and anthracenyl.
[0074] From the perspective of easy synthesis and not impairing the fluidity of the composition before curing and the heat resistance of the cured product, R a1 Preferably, R is a vinyl group. b1 It is preferably a C1-C6 alkyl group, and particularly preferably a methyl group. Therefore, the component (A) is preferably a polymethylvinylsiloxane having both ends blocked by dimethylvinylsiloxane units and an intermediate unit containing a dimethylsiloxane unit.
[0075] In 100% by mass of the component (A), the content of polymethylvinylsiloxane having both ends blocked by dimethylvinylsiloxane units and containing dimethylsiloxane units in the middle unit is preferably 30% by mass or more, more preferably 50% by mass or more, and even more preferably 80% by mass or more. The upper limit of the above content is 100% by mass.
[0076] From the viewpoint of ensuring stable liquid properties of the composition and curability in the portion not irradiated with light and in the thickness direction, n1 is a number that makes the average alkenyl content of the straight-chain polysiloxane greater than 0.08 mmol / g, preferably a number that makes it 0.08 to 11.0 mmol / g, more preferably a number that makes it 0.09 to 5.0 mmol / g, further preferably a number that makes it 0.09 to 1.8 mmol / g, and particularly preferably a number that makes it 0.1 to 0.5 mmol / g.
[0077] The viscosity of the component (A) is a value measured using a rotational viscometer at No. 1, 2, 3 or 4 rotor, 60 rpm, and 23° C. in accordance with JIS K 6249.
[0078] The component (A) may be a mixture of a polymethylvinylsiloxane having both ends blocked with dimethylvinylsiloxane units and containing dimethylsiloxane units as intermediate units, and other linear, branched or cyclic alkenyl-containing polyorganosiloxanes.
[0079] (A) component can utilize commercially available products. In addition, polyorganosiloxanes into which alkenyl groups are introduced by known reactions can be used. As (A) component, it is distinguished according to the position or type of the substituent, the degree of polymerization, etc., and only one compound can be used, or two or more compounds can be mixed and used. (A) component is polyorganosiloxane, and therefore can be a mixture of polyorganosiloxanes having various degrees of polymerization.
[0080] From the viewpoint of the balance among handling properties, curability and storage stability, the amount of component (A) is preferably 70.0 to 99.8% by mass, more preferably 80.0 to 99.7% by mass, and even more preferably 90.0 to 99.7% by mass based on 100% by mass of the ultraviolet curable silicone composition.
[0081] <(B) Polyorganohydrogensiloxane having at least three hydrogen atoms bonded to silicon atoms in one molecule>
[0082] The component (B) is a polyorganohydrogensiloxane having at least three hydrogen atoms bonded to silicon atoms in one molecule. The component (B) functions as a crosslinking agent and forms a network structure by an addition reaction with the alkenyl group of the component (A).
[0083] The hydrogen atom of the (B) component may be bonded to the silicon atom at the end of the molecular chain, may be bonded to the silicon atom in the middle of the molecular chain, or may be bonded to both. The molecular structure of the (B) component is not particularly limited as long as it is a structure with siloxane bonds as the main skeleton, and may be any of linear, branched, cyclic or three-dimensional mesh structures, and the siloxane skeleton may be interrupted by a divalent organic group. In addition, the (B) component may have a hydroxyl group or an alkoxy group such as a methoxy group or an ethoxy group bonded to the silicon atom. The (B) component may be used alone or in combination of two or more.
[0084] Typically, the component (B) has at least three siloxane units represented by the general formula (2) containing hydrogen atoms bonded to silicon atoms in the molecule.
[0085] R 3 p H q SiO (4-p-q) / 2 (2)
[0086] (Where,
[0087] R 3 It is an unsubstituted or substituted monovalent hydrocarbon group having no aliphatic unsaturated bond;
[0088] p is an integer from 0 to 2;
[0089] q is an integer from 1 to 3, wherein p+q is 1 to 3. )
[0090] As R 3 , which is the same as R in the general formula (1) 1 The same preferred embodiments apply to the same groups. In the component (B), the number of hydrogen atoms bonded to silicon atoms is preferably 3 to 100, more preferably 5 to 50, per molecule.
[0091] (B) component contains (B1) containing R c1 2HSiO 1 / 2 Unit (where R c1 are independently C1-C6 alkyl or C6-C 20 Aryl) and SiO 4 / 2 The present inventors have found that, by making the component (B) include the component (B1), when the composition is irradiated with ultraviolet rays, the composition can be cured not only in the irradiated range, but also in a range that is three-dimensionally expanded to cure the composition, thereby forming a composition having excellent curability even in the portion around the irradiated portion that is not irradiated by light and in the thickness direction.
[0092] The component (B1) may be branched, cyclic or three-dimensional network structure (SiO 4 / 2 From the perspective of ease of synthesis, R c1 It is preferably a C1-C6 alkyl group, and particularly preferably a methyl group.
[0093] Among them, component (B1) preferably has 3 to 6 SiO 4 / 2 Unit and 6 to 12 R c1 2HSiO 1 / 2 Unit bonded polyorganohydrogensiloxane; particularly preferably such as [R c1 2HSiO 1 / 2 ]6[SiO 4 / 2 ]3. [R c1 2HSiO 1 / 2 ]8[SiO 4 / 2 ]4. [R c1 2HSiO 1 / 2 ] 10 [SiO 4 / 2 ]5. [R c1 2HSiO 1 / 2 ] 12 [SiO 4 / 2 ]6 3 to 6 SiO 4 / 2 The units form a cyclic siloxane skeleton and 4 / 2 There are 2 R bonds on the unit c1 2HSiO 1 / 2 Cyclic polyorganohydrogensiloxane containing 2,4-dimethyl-1,2-dioxane units.
[0094] The viscosity of the component (B) at 23° C. is preferably 1 to 100 mPa·s, more preferably 1 to 50 mPa·s. The viscosity is a value measured in accordance with JIS K 6249 using a rotational viscometer at No. 1 or 2 rotor, 60 rps, and 23° C.
[0095] The component (B) can utilize a commercially available product. In addition, the component (B) can also be synthesized by a known reaction. The component (B) can be distinguished according to the position or type of the substituent, the degree of polymerization, etc., and can use only one compound or a mixture of two or more compounds. Since the component (B) is a polyorganohydrogensiloxane, it can be a mixture of polyorganohydrogensiloxanes having various degrees of polymerization.
[0096] From the viewpoint of handling properties, curing properties, and expansibility of the curing range, the number of moles of hydrogen atoms bonded to silicon atoms in the component (B) H B The number of moles of alkenyl groups in component (A) Vi A The ratio of H B / Vi A The ratio is preferably 0.30 to 3.5, more preferably 0.30 to 3.0, further preferably 0.40 to 2.0, further preferably 0.45 to 1.1, and particularly preferably 0.50 to 1.0.
[0097] <(C) Platinum-based catalyst activated by ultraviolet light>
[0098] The component (C) is a catalyst activated by ultraviolet light and used to promote the addition reaction between the alkenyl group of the component (A) and the hydrosilyl group (Si-H group) of the component (B). From the viewpoint of improving the catalytic activity, the component (C) is preferably a platinum-based catalyst having a cyclic diene compound as a ligand. The component (C) may be used alone or in combination of two or more.
[0099] Examples of platinum-based catalysts using a cyclic diene compound as a ligand include (1,5-cyclooctadienyl)diphenylplatinum complex, (1,5-cyclooctadienyl)dipropylplatinum complex, (2,5-norbornadiene)dimethylplatinum complex, (2,5-norbornadienyl)diphenylplatinum complex, (cyclopentadienyl)dimethylplatinum complex, (methylcyclopentadienyl)diethylplatinum complex, (trimethylsilylcyclopentadienyl)diphenylplatinum complex, (methylcyclooctadienyl)diethyl ...2,5-norbornadienyl)dimethylplatinum complex, (2,5-norbornadienyl)diphenylplatinum complex, (2,5-norbornadienyl)dimethylplatinum complex, (2,5-norbornadienyl)diphenylplatinum complex, (2,5-norbornadienyl)dimethylplatinum complex, (2,5-norbornadienyl)diphenylplatinum complex, (2,5-norbornadienyl)dimethylplatinum complex, (2,5-norbornadienyl)diphenylplatinum complex, (2,5-norbornadienyl)dimethylplatinum complex, (2,5-norbornadienyl)diphenylplatinum complex, (2 (cyclopentadienyl) diethyl platinum complex, (cyclopentadienyl) trimethyl platinum complex, (cyclopentadienyl) ethyl dimethyl platinum complex, (cyclopentadienyl) acetyl dimethyl platinum complex, (methyl cyclopentadienyl) trimethyl platinum complex, (methyl cyclopentadienyl) trihexyl platinum complex, (trimethylsilyl cyclopentadienyl) trimethyl platinum complex, (dimethylphenyl silyl cyclopentadienyl) triphenyl platinum complex, (cyclopentadienyl) dimethyl trimethyl silyl methyl platinum complex, etc.
[0100] The amount of component (C) in the UV-curable silicone composition is 8 to 400 ppm based on the mass of platinum metal. If the amount of component (C) is less than 8 ppm based on the mass of platinum metal, the curing properties in the part not irradiated by the surrounding light of the part irradiated by ultraviolet light and in the thickness direction will deteriorate. If the amount of component (C) exceeds 400 ppm based on the mass of platinum metal, the storage stability of the UV-curable silicone composition is easily deteriorated and the cured product is yellowed, and the cost becomes high. The amount of component (C) in the UV-curable silicone composition is preferably 30 to 350 ppm based on the mass of platinum metal, more preferably 37 to 350 ppm, further preferably 40 to 350 ppm, and particularly preferably 70 to 340 ppm.
[0101] Similarly, the amount of component (C) relative to the total mass of component (A) and component (B) is preferably 8 to 400 ppm, more preferably 30 to 350 ppm, further preferably 37 to 350 ppm, further preferably 40 to 350 ppm, and particularly preferably 70 to 340 ppm, based on the mass of platinum metal.
[0102] <Other ingredients>
[0103] As for the UV-curable silicone composition, other components may be added as long as they do not impair its purpose and effect. As other components, flame retardants, adhesion-imparting agents, heat-resistance-imparting agents, diluents, thixotropy-imparting agents such as fumed silica, inorganic or organic pigments, inhibitors of addition reaction curing catalysts, resins other than polyorganosiloxanes, etc. may be appropriately added. In addition, the UV-curable silicone composition may be added with: polyorganosiloxanes other than component (A), for example, polyorganosiloxanes having one or less alkenyl groups in one molecule; polyorganohydrogensiloxanes other than component (B), for example, polyorganohydrogensiloxanes having one or two hydrogen atoms bonded to silicon atoms in one molecule, etc. The other components may be used alone or in combination of two or more.
[0104] <Method for producing ultraviolet curable silicone composition>
[0105] The UV-curable silicone composition can be obtained by mixing the components (A) to (C) and other components as needed using a planetary mixer or other mixer. During mixing, the mixing can be carried out while heating in the range of 50 to 150° C. as needed. In the case where the UV-curable silicone composition contains powder, it is preferred to perform the kneading operation under high shear force for uniform finishing. As a kneading device, there are three-roll mills, colloid mills, sand mills (Japanese: サンドグラインダー), etc. Among them, the method using a three-roll mill is preferred.
[0106] The UV-curable silicone composition may also be prepared as a two-component composition in consideration of the storage stability of the composition. In the case of preparing a two-component composition, it is preferred that: the first component contains the component (A) and the component (C) and does not contain the component (B); and the second component contains the component (B) and does not contain the component (C). In the two-component UV-curable silicone composition, the first component and the second component are prepared separately. The first component and the second component can be manufactured by the same method as the one-component composition.
[0107] The viscosity of the UV-curable silicone composition at 23°C is 10 to 10,000 mPa·s. By setting the viscosity of the composition to the above range, the handling property is excellent, and the curing property in the part not irradiated by the surrounding light of the part irradiated by the UV light and in the thickness direction can be improved. The viscosity of the UV-curable silicone composition at 23°C is preferably 20 to 5,000 mPa·s, and more preferably 100 to 2,000 mPa·s.
[0108] When the UV-curable silicone composition is a two-component composition comprising a first component and a second component, the viscosity of the first component and the second component is preferably 10 to 20,000 mPa·s, more preferably 20 to 10,000 mPa·s, and particularly preferably 100 to 5,000 mPa·s. The viscosity is a value measured using a rotational viscometer at No. 1, 2, 3 or 4 rotors, 60 rpm, and 23° C. in accordance with JIS K 6249. The UV-curable silicone composition is preferably stored under light shielding at a temperature below room temperature.
[0109] <Curing method of ultraviolet curable silicone composition>
[0110] The ultraviolet curable silicone composition can be cured by irradiation with ultraviolet rays. The irradiation dose is preferably 100 to 10,000 mJ / cm 2 , more preferably 300 to 6,000 mJ / cm 2 , more preferably 500 to 5,000 mJ / cm 2 It should be noted that the irradiation amount is a measured value of UVA. Here, UVA refers to ultraviolet rays in the range of 315 to 400 nm. The composition has good curing properties when irradiated with ultraviolet rays having a wavelength, for example, ultraviolet rays in the range of 250 to 450 nm. As light sources that emit ultraviolet rays of this wavelength, for example, there are: high-pressure mercury lamps (UV-7000) manufactured by USHIO Electric Co., Ltd., metal halide lamps (UVL-4001M3-N1), metal halide lamps (JM-MTL 2KW) manufactured by JM tech Co., Ltd. of Korea, ultraviolet irradiation lamps (OSBL360) manufactured by Mitsubishi Electric Corporation, ultraviolet irradiation machines (UD-20-2) manufactured by GS YUASA Co., Ltd., fluorescent lamps (FL-20BLB) manufactured by Toshiba Corporation), H lamps, H+ lamps, V lamps, D lamps, Q lamps and M lamps manufactured by Heraeus, LED lamps (HLDL-155UV) manufactured by CCS Co., Ltd., etc.
[0111] The curing time of the composition depends on the amount of ultraviolet irradiation, but is generally less than 30 minutes, preferably less than 10 minutes. Whether the curing of the composition is progressing can also be judged by visual inspection, and can also be quantitatively evaluated by the time until the storage modulus G' and the loss modulus G" become equal, the time until the storage modulus G' reaches a specified value, etc. For example, under the condition of 23°C after ultraviolet irradiation, when the time until the storage modulus G' and the loss modulus G" become equal is within 30 minutes, preferably within 10 minutes, it can be said that the time consumed for curing is short and the handleability is excellent, so it is preferred.
[0112] <Curing properties of UV-curable silicone composition>
[0113] The UV curable silicone composition has excellent curing properties in the non-irradiated part and in the thickness direction. Specifically, the UV curable silicone composition was irradiated in a yellow light room with a diameter of 7.0 mm and an illumination of 100 mW / cm 2 , 365nm wavelength ultraviolet light for 45 seconds, and then stored at 23°C for 16 hours to obtain a cured product, the cured diameter of which at a depth of 1.8mm is 10.8mm or more. The cured diameter is preferably 11.0mm or more, more preferably 12.0mm or more, and even more preferably 13.0mm or more.
[0114] use Figures 1 to 4 , the method for measuring the above-mentioned solidification diameter is explained. Figure 1 This is a photograph of the device used to measure the cured diameter taken from above in a yellow light room. Figure 2 This is a schematic diagram of the device as viewed from above. Figure 3 yes Figure 2 A-A' line cross-sectional view.
[0115] Figure 4 Yes Figure 2 and 3 Schematic diagram illustrating the cured area and cured diameter after ultraviolet irradiation.
[0116] A yellow light room refers to an environment in which light with a wavelength of 500 nm or less, including ultraviolet rays, is shielded. Specifically, it refers to an environment in which wavelengths of 500 nm or less from light of a fluorescent lamp are cut off by more than 98%. For example, a yellow light room is usually set up when photosensitive materials are processed in a clean room of a semiconductor factory. For example, a yellow light room can be formed by using a room without windows and using a commercially available yellow fluorescent lamp as lighting. Examples of commercially available yellow fluorescent lamps include yellow straight tube LED lamps manufactured by Toshiba Corporation.
[0117] like Figure 2 and 3 As shown, a rectangular depression 1 ( Figure 2 and Figure 3 A metal mold 6 (within the dotted line) was provided. In order to prevent the reflection of ultraviolet rays, a bottom black tape 4 (thickness 0.2 mm) was attached to the entire bottom surface of the depression 1. After that, the samples 7 (compositions of the examples and comparative examples) were filled into the depressions 1 in a yellow light room, and an upper black tape 5 (thickness 0.2 mm) having a hole 2 with a diameter of 7.0 mm was attached to cover the upper part of the composition. Furthermore, a transparent glass 3 with a thickness of 1 mm, which was one size larger than the size of the depression 1, was placed on the upper black tape 5.
[0118] The sample 7 thus arranged was irradiated with an illuminance of 100 mW / cm2 through the hole 2 using a UV-LED irradiator manufactured by CCS Corporation. 2 , UV light with a wavelength of 365nm for 45 seconds (irradiation dose 4,500mJ / cm 2 ) and stored at 23°C for 16 hours. Figure 4 As shown, the sample 7 is cured within the range of the curing area 8. The upper black tape 5 is removed, and the sample is placed against a metal mold 6 to remove the uncured portion. The maximum diameter of each of the cured upper and lower surfaces is measured with a vernier ruler as the cured diameter.
[0119] <Applications of UV-curable silicone compositions>
[0120] The cured product of the ultraviolet curable silicone composition has excellent adhesiveness and transparency and can be suitably used in potting materials. Specifically, the ultraviolet curable silicone composition can be suitably used in materials having a portion that is not easily irradiated with light, especially potting materials for connector pins.
[0121] In another embodiment of the present invention, the cured product of the UV-curable silicone composition can be suitably used as a sealing material. Articles using the cured product of the UV-curable silicone composition as a sealant have excellent water resistance and durability on the bonding surface and the sealing part, so the cured product can be suitably used as a sealing material for electrical components or electronic components. In addition, the UV-curable silicone composition has excellent curing properties in the part not irradiated by the surrounding light and in the thickness direction, so the quality of the cured product is stable. Therefore, it can be used, for example, as: an adhesive for bonding image display devices such as liquid crystal, plasma, and organic EL; or a sealant for sealing LED elements or OLED elements. In particular, the sealing material containing the cured product of the UV-curable silicone composition can be suitable for use in electrical components or electronic components, and in particular, it is suitable for connectors with connector pins.
[0122] Example
[0123] Next, the present invention will be described in more detail by way of examples and comparative examples. However, the present invention is not limited to these examples. Unless otherwise specified, all values are expressed as parts by mass or mass %.
[0124] <Ingredients used>
[0125] The components used are shown below. Here, the meanings of the symbols are as follows.
[0126] M: (CH3)3SiO 1 / 2
[0127] M H :H(CH3)2SiO1 / 2
[0128] M Vi :CH2=CH(CH3)2SiO 1 / 2
[0129] D: (CH3)2SiO 2 / 2
[0130] D H :H(CH3)SiO 2 / 2
[0131] D Vi :CH2=CH(CH3)SiO 2 / 2
[0132] Q:SiO 4 / 2 (Tetrafunctional)
[0133] Component (A): a polyorganosiloxane having at least two alkenyl groups in one molecule and an average alkenyl content of 0.08 mmol / g or more
[0134] Use the following Vi The unit is blocked and the middle unit contains a polymethylvinylsiloxane D unit.
[0135] M Vi D m1 M Vi (1): Average vinyl content: 0.346 mmol / g, viscosity at 23°C: 140 mPa·s
[0136] M Vi D m2 M Vi (2): Average vinyl content: 0.106 mmol / g, viscosity at 23°C: 1,400 mPa·s
[0137] M Vi D m5 M Vi (5): Average vinyl content: 0.145 mmol / g, viscosity at 23°C: 1,200 mPa·s
[0138] Component (A'): a polyorganosiloxane having at least two alkenyl groups in one molecule and an average alkenyl content of less than 0.08 mmol / g
[0139] M Vi D m3 M Vi (3): Average vinyl content: 0.047 mmol / g, viscosity at 23°C: 13,000 mPa·s
[0140] MVi D m4 M Vi (4): Average vinyl content: 0.029 mmol / g, viscosity at 23°C: 78,000 mPa·s
[0141] The alkenyl content of the components (A) and (A') was determined by using a spectrophotometer from the absorbance (near 2,150 nm) of the CH2=CH- group.
[0142] Component (B): polyorganohydrogensiloxane having at least three hydrogen atoms bonded to silicon atoms in one molecule
[0143] The average unit formula is M H 8Q4-represented cross-linked polymethylhydrogensiloxane (SiH content: 10.11 mmol / g)
[0144] The average unit formula is M H D H 9D 11 M H Crosslinkable polymethylhydrogensiloxane (SiH content: 8.27 mmol / g)
[0145] The average unit formula is given by MD H 23 D 16 M represents cross-linkable polymethylhydrogensiloxane (SiH content: 8.60 mmol / g)
[0146] Component (C): Platinum catalyst activated by ultraviolet light
[0147] (Methylcyclopentadienyl)trimethylplatinum complex (manufactured by Strem Chemicals, Inc. (Germany), platinum content: 61.1 mass %)
[0148] Other Ingredients
[0149] (1) Polyorganosiloxane having at least two hydrogen atoms bonded to sulfur atoms in one molecule (SH amount: 0.96 mmol / g)
[0150] (2) Acrylic monomer: 4-hydroxybutyl acrylate (manufactured by Mitsubishi Chemical Corporation, 4HBA)
[0151] (3) Photoinitiator: 2-hydroxy-2-methyl-1-phenylpropanone (manufactured by IGM Resins BV, Irgacure (registered trademark) 1173). A 1.0 mass % diluted solution was used.
[0152] Example 1
[0153] The composition was prepared in a yellow light room. Vi D m1 M Vi (1) Dilute to 1.0 mass % Vi D m1 M Vi (1) 5.50 parts by mass of the dilution solution of the above-mentioned component (C) (component (C): 0.055 parts by mass, M Vi D m1 M Vi (1): 5.445 parts by mass) and (B) component 3.20 parts by mass were mixed to obtain the ultraviolet curable silicone composition of Example 1.
[0154] Embodiments 2 to 14
[0155] Except having changed (A) - (C) component and its blending amount as Table 1, it carried out similarly to Example 1, and obtained the ultraviolet curable silicone composition of Examples 2-14.
[0156] [Table 1]
[0157]
[0158] Comparative Examples 1 to 15
[0159] Except having changed each component and its blending amount as shown in Table 2, it carried out similarly to Example 1, and obtained the ultraviolet curable composition of Comparative Examples 1-15.
[0160] [Table 2]
[0161]
[0162] <Measurement method>
[0163] [Viscosity]
[0164] The compositions of Examples 1 to 14 and Comparative Examples 1 to 15 were measured for viscosity at 23°C using a rotational viscometer (Vismetron VDA2, manufactured by Shibaura System Co., Ltd.) at 60 rpm using a No. 2 rotor in accordance with JIS K 6249. The viscosity was measured immediately after the composition was prepared and after it was stored at 23°C outside a yellow light room for 24 hours. The results are shown in Tables 3 and 4.
[0165] [Shore 00 hardness]
[0166] The compositions of Examples 1 to 14 and Comparative Examples 1 to 15 were poured into a mold of 100 mm in length × 100 mm in width × 2 mm in depth, and irradiated with HLDL-155UV manufactured by CCS Corporation at an illumination of 100 mW / cm 2 After curing by ultraviolet irradiation for 45 seconds, the cured product was further stored at 23°C and 50 RH% for 16 hours. The obtained cured product was measured for Shore 00 hardness according to ASTM D 2240. It should be noted that the composition was recorded as "uncured" when it was not cured by ultraviolet irradiation. The results are shown in Tables 3 and 4.
[0167] [Gelation time]
[0168] For the compositions of Examples 1 to 14 and Comparative Examples 1 to 15, the storage modulus G' was measured over time from the start of ultraviolet irradiation using a viscoelasticity measuring device MCR301 (manufactured by Anton Paar). Using the above-mentioned viscoelasticity measuring device and using Φ12 mm parallel plates, the storage modulus G' of the ultraviolet curable silicone composition at 23°C was measured under the conditions of a spacing of 0.5 mm, a frequency of 1 Hz and a strain of 1%. The ultraviolet curable silicone composition was irradiated with an illuminance of 100 mW / cm 2 UV rays for 45 seconds (irradiation dose 4,500mJ / cm 2 ), the time from the start of irradiation to the time when the storage modulus G' and the loss modulus G" become equal is set as the gelation time. The shorter the gelation time, the better the rapid curing property, and it is judged to be excellent in curing property. It should be noted that the gelation time is measured until 60 minutes after the start of ultraviolet irradiation, and the case where the storage modulus G' is less than the loss modulus G" is recorded as "uncured". The results are shown in Tables 3 and 4.
[0169] [Cure diameter]
[0170] The curing diameter was measured as an index of whether the composition can be cured not only in the irradiated range but also to what extent the range can be expanded when irradiated with ultraviolet rays. Figure 1 This is a photograph of the device used for the above measurement taken from above in a yellow light room. Figure 2 This is a schematic diagram of the device as viewed from above. Figure 3 yes Figure 2 A-A' line cross-sectional view. Figure 4 Yes Figure 2 and 3 Schematic diagram illustrating the cured area and cured diameter after ultraviolet irradiation.
[0171] like Figure 2 and 3As shown, a rectangular depression 1 ( Figure 2 and Figure 3 A metal mold 6 (within the dotted line) was provided. In order to prevent the reflection of ultraviolet rays, a bottom black tape 4 (thickness 0.2 mm) was attached to the entire bottom surface of the depression 1. After that, the samples 7 (compositions of the examples and comparative examples) were filled into the depressions 1 in a yellow light room, and an upper black tape 5 (thickness 0.2 mm) having a hole 2 with a diameter of 7.0 mm was attached to cover the upper part of the composition. Furthermore, a transparent glass 3 with a thickness of 1 mm, which was one size larger than the size of the depression 1, was placed on the upper black tape 5.
[0172] The sample 7 thus arranged was irradiated with an illuminance of 100 mW / cm2 through the hole 2 using a UV-LED irradiator manufactured by CCS Corporation. 2 , UV light with a wavelength of 365nm for 45 seconds (irradiation dose 4,500mJ / cm 2 ) and stored at 23°C for 16 hours. Figure 4 As shown, the sample 7 is cured within the range of the curing area 8. Remove the upper black tape 5, stand against the metal mold 6, remove the uncured part, and measure the maximum diameter of the cured upper surface and lower surface with a vernier ruler as the cured diameter. Regarding the cured diameter, when the upper surface is more than 7.0mm and the lower surface is more than 10.8mm, it is judged that the curing property in the part not irradiated by the light around the part irradiated by ultraviolet rays and in the thickness direction is excellent. It should be noted that when the composition is not cured by ultraviolet irradiation, it is recorded as "uncured". In addition, the results are shown in Tables 3 and 4.
[0173] As an index of whether the composition can be cured beyond the range irradiated by ultraviolet rays and to what extent, the cured area of the non-irradiated portion is calculated. First, assuming that the composition of the embodiment and the comparative example is cured into a circular shape, the total cured area is calculated according to the curing diameter for the upper and lower surfaces of the sample 7. Then, the difference between the total cured area of the upper and lower surfaces and the irradiated area of ultraviolet rays (the area of hole 2) is used as the cured area of the non-irradiated portion. The results are shown in Tables 3 and 4.
[0174] [Table 3]
[0175]
[0176]
[0177] As shown in Table 3, the UV-curable silicone composition of the embodiment has a short gelation time, excellent curability, and excellent curability in the portion not irradiated by light and in the thickness direction. The UV-curable silicone composition of the embodiment comprises: (A) a polyorganosiloxane having at least two alkenyl groups in one molecule and an average alkenyl content of 0.08 mmol / g or more, (B) a polyorganohydrogensiloxane having at least three hydrogen atoms bonded to silicon atoms in one molecule, and (C) a platinum-based catalyst activated by ultraviolet light, wherein the component (B) comprises (B1) a catalyst containing R c1 2HSiO 1 / 2 Unit (where R c1 are independently C1-C6 alkyl or C6-C 20 Aryl) and SiO 4 / 2 The polyorganohydrogensiloxane has a unit, the amount of the component (C) in the composition is 8 to 400 ppm based on the mass of platinum metal, and the viscosity of the composition at 23° C. is 10 to 10,000 mPa·s.
[0178] From the comparison between Examples 1 to 10 and Comparative Example 5, it was observed that as the amount of the component (C) in the composition increased, the cured diameter and the cured area of the non-irradiated portion tended to increase. Figure 5 : is a graph showing the relationship between the amount of platinum blended and the solidified diameter at the upper surface (depth 0 mm) and the lower surface (depth 1.8 mm) of the sample 7 for Examples 1 to 10 and Comparative Example 5. Figure 6 This is a graph showing the relationship between the amount of platinum added and the cured area of the non-irradiated portion on the upper surface and the lower surface of the sample 7 for Examples 1 to 10 and Comparative Example 5. Figure 5 and 6 When the amount of component (C) is 56 and 196 ppm, an inflection point is observed near the amount of component (C). When the amount of component (C) exceeds these values, a tendency is observed to significantly increase the cured diameter and the cured area of the non-irradiated portion, especially at a depth of 1.8 mm, so it is preferred.
[0179] In Example 6 in which the alkenyl content of the component (A) was 0.346 mmol / g, the cured diameter at the lower surface (depth 1.8 m) of the sample was larger than that of Example 14 in which the alkenyl content was 0.106 mmol / g, and the curability in the thickness direction was excellent.
[0180] Comparative Examples 1 and 2, in which a polyorganosiloxane having at least two hydrogen atoms bonded to a sulfur atom in one molecule was used instead of component (B) and a photoinitiator was used, and Comparative Examples 3 and 4, in which an acrylic monomer and a photoinitiator were used, had poor curability in the portion not irradiated with light and in the thickness direction. In particular, in Comparative Examples 2 and 4, in which the content of the photoinitiator was 0.17 μmol / g, the composition could not be cured. Comparative Example 5, in which components (A) to (C) were used but the amount of component (C) in the composition was less than 8 ppm based on the mass of platinum metal, had poor curability in the portion not irradiated with light and in the thickness direction.
[0181] For Comparative Examples 6 and 7, in which the average alkenyl content of component (A) was less than 0.08 mmol / g and the viscosity of the composition at 23°C exceeded 10,000 mPa·s, the cured diameter at a depth of 1.8 mm was small and the curability in the thickness direction was poor. For Comparative Examples 8 to 15, in which component (B) was a linear polyorganohydrogensiloxane, the cured diameter at a depth of 1.8 mm was small and the curability in the thickness direction was poor. In particular, by comparing Examples 6, 8 and 10 with Comparative Examples 8 to 10 and Comparative Examples 12 to 14, it can be seen that the composition of the embodiment in which component (B) was component (B1) was significantly superior in the cured diameter at a depth of 1.8 mm and the cured area of the non-irradiated portion compared to the composition of the comparative example in which component (B) was a linear polyorganohydrogensiloxane.
[0182] Industrial Applicability
[0183] The cured product of the ultraviolet curable silicone composition is useful as a sealing material for electric parts, electronic parts, and the like.
[0184] Description of Reference Numerals
[0185] 1 Depression
[0186] 2 holes
[0187] 3. Transparent glass
[0188] 4 Use black tape on the bottom
[0189] 5 Use black tape on the upper part
[0190] 6 Metal molds
[0191] 7. Sample (UV-curable silicone composition)
[0192] 8 Curing area
[0193] 9 Curing diameter
Claims
1. A UV-curable silicone composition comprising: (A) a polyorganosiloxane having at least two alkenyl groups in one molecule and an average alkenyl content of 0.08 mmol / g or more, (B) a polyorganohydrogensiloxane having at least three hydrogen atoms bonded to silicon atoms in one molecule, and (C) a platinum catalyst activated by ultraviolet light, in, (B) component contains (B1) containing R c1 2HSiO 1 / 2 Unit and SiO 4 / 2 Unit polyorganohydrogensiloxane, formula R c1 2HSiO 1 / 2 In, R c1 are independently C1-C6 alkyl or C6-C 20 Aryl, The amount of the component (C) in the composition is 8 ppm to 400 ppm based on the mass of the platinum metal. The viscosity of the composition at 23° C. is 10 mPa·s to 10000 mPa·s, The composition was irradiated with a yellow light source with a diameter of 7.0 mm and an illumination of 100 mW / cm 2 , ultraviolet rays with a wavelength of 365 nm for 45 seconds, and then stored at 23° C. for 16 hours to obtain a cured product, and the cured diameter of the obtained cured product at a depth of 1.8 mm was greater than 10.8 mm.
2. The ultraviolet curable silicone composition according to claim 1, wherein The component (A) contains a linear polyorganosiloxane, and the alkenyl content of the component (A) is 0.09 mmol / g to 1.8 mmol / g on average.
3. The ultraviolet curable silicone composition according to claim 1 or 2, wherein The amount of the component (C) in the composition is 40 ppm to 350 ppm based on the mass of the platinum metal.
4. The ultraviolet curable silicone composition according to claim 1 or 2, wherein (B 1) The composition is 3 to 6 SiO 4 / 2 Unit and 6 to 12 R c1 2HSiO 1 / 2 Polyorganohydrogensiloxane formed by unit bonding.
5. The ultraviolet curable silicone composition according to claim 1 or 2, wherein The component (C) is a platinum-based catalyst having a cyclic diene compound as a ligand.
6. The ultraviolet curable silicone composition according to claim 1 or 2, wherein The number of moles of hydrogen atoms bonded to silicon atoms in component (B) B The number of moles of alkenyl groups in component (A) Vi A The ratio of H B / Vi A The ratio is 0.30~3.
5.
7. A potting material comprising the ultraviolet curable silicone composition according to claim 1 or 2. The potting material according to claim 7 , which is used for connector pins. 9 . A sealing material comprising a cured product of the ultraviolet curable silicone composition according to claim 1 or 2 . 10 . The sealing material according to claim 9 , which is used for an electric component or an electronic component.
11. The sealing material according to claim 10, wherein The electrical component or the electronic component is a connector having connector pins.