Al-Si alloy for casting, Al-Si alloy casting, and Al-Si alloy casting assembly
By optimizing the composition and fine structure of Al-Si alloy, the crack problem of aluminum alloy castings during self-punching rivet joint is solved, and the effect of high yield strength and low crack rate is achieved, which is suitable for various mechanical joint applications.
Patent Information
- Application Number
- CN202380023645.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-03
- Filing Date
- 2023-03-03
- Publication Date
- 2024-11-05
AI Technical Summary
In aluminum alloy castings, crack problems often occur when mechanical joints are used with self-punching rivets, and the existing Al-Mg-Si-based aluminum alloy materials are difficult to ensure high yield strength and low crack rate at the same time when bonding.
By optimizing the composition of Al-Si alloy, the content of elements such as Si, Mn, Mg, Cr, Fe is increased, and through fine tissue adjustment, the needle-like and coarseness of crystals is inhibited, and the mechanical properties are improved. The specific content range is Si : 5.0%-12.0%, Mn: 0.4%-1.5%, Mg: 0.05%-0.6%, Cr: 0.1%-0.5%, Fe: 0.1%-0.6%, to improve the yield strength of the casting and suppress crack generation.
It effectively suppresses the generation of cracks during self-punching rivets, and imparts high yield strength to the Al-Si alloy castings, with the ultimate bending angle of more than 28°, and the 0.2% yield strength is preferably 100MPa or more, and is suitable for various mechanical joint applications.
Smart Images

Figure BDA0005009890830000091 
Figure HDA0005009890840000011 
Figure HDA0005009890840000012
Abstract
Description
Technical Field
[0001] The present invention relates to an Al-Si alloy preferably used for casting, especially die casting, wherein an Al-Si alloy casting cast using the Al-Si alloy is suitable for mechanical joining using rivets (especially self-piercing rivets) and the like. Background Art
[0002] Aluminum materials are joined by brazing, bonding, welding, friction stir welding, friction pressure welding, etc. In recent years, mechanical joining using self-piercing rivets and the like has attracted attention as a simpler joining method.
[0003] The so-called self-piercing rivet joining is the following joining method: the materials to be joined are overlapped, a receiving mold is arranged on the lower surface of the lower material to be joined, and a self-piercing rivet is driven from above the upper material to be joined. The shaft of the self-piercing rivet expands when the material is driven, thereby achieving joining.
[0004] For example, in Patent Document 1 (Japanese Patent Laid-Open No. 2020-66751), an Al-Mg-Si series aluminum alloy plastic working material is disclosed, which is a plastic working material for self-piercing rivet joining, characterized in that it is the following aluminum alloy plastic working material, containing Si: 0.95 mass% to 1.25 mass%, Mg: 0.80 mass% to 1.05 mass%, Cu: 0.30 mass% to 0.50 mass%, Mn: 0.40 mass% to 0.60 mass%, Fe: 0.15 mass% to 0.30 mass%, Cr: 0.09 mass% to 0.21 mass%, B: 0.0001 mass% to 0.03 mass%, Zn content is 0.25 mass% or less, Zr content is 0.05 mass% or less, Ti content is 0.10 mass% or less, and the remainder contains Al and inevitable impurities, wherein, according to Japanese Industrial Standards (Japanese Industrial The maximum shear tensile load measured on the self-piercing rivet joints of the aluminum alloy plastic working materials is 8.5 kN or more.
[0005] The Al—Mg—Si aluminum alloy plastic working material described in Patent Document 1 can provide an Al—Mg—Si aluminum alloy plastic working material having excellent joining strength in self-piercing rivet joining by optimizing the composition.
[0006] In addition, in Patent Document 2 (Japanese Patent Laid-Open No. 2002-121635), an aluminum alloy extrusion material for automobile frames having excellent self-piercing rivet bonding properties is disclosed, characterized in that it includes an Al-Mg-Si series aluminum alloy extrusion material containing Mg: 0.30% to 0.70% (mass%, the same below), Si: 0.40% to 0.80%, Cu: 0.05% to 0.40%, Mn: 0.05% to 0.30%, Zr: 0.05% to 0.20%, and the remaining Al and inevitable impurities, and is subjected to air cooling and aging treatment after press quenching to have a strength of 200N / mm 2 The yield strength is above 3.5%, and the local elongation is above 3.5%.
[0007] Among the aluminum alloy extrusions for automobile frames described in Patent Document 2, the Al-Mg-Si aluminum alloy extrusions are subjected to aging treatment after press quenching using air cooling, which is advantageous in terms of dimensional accuracy or cost, thereby obtaining aluminum alloy extrusions having the strength (yield strength) required for automobile frames and excellent self-piercing rivet joinability.
[0008] Prior art literature
[0009] Patent Literature
[0010] Patent Document 1: Japanese Patent Application Publication No. 2020-66751
[0011] Patent Document 2: Japanese Patent Application Publication No. 2002-121635 Summary of the invention
[0012] Problems to be solved by the invention
[0013] However, the subject of Patent Document 1 is an Al—Mg—Si aluminum alloy plastic working material, and the subject of Patent Document 2 is an aluminum alloy extrusion material, and both cases relate to aluminum alloy materials in which microstructure and mechanical properties are controlled by plastic working.
[0014] In contrast, mechanical joining using self-piercing rivets or the like often requires joining aluminum alloy castings such as die castings to other structural members. When mechanical joining is applied to aluminum alloy castings, suppressing cracks generated during joining becomes a more serious issue.
[0015] In view of the above problems in the prior art, the object of the present invention is to provide an Al-Si alloy for castings, which can effectively suppress the occurrence of cracks when self-piercing rivets are pressed into aluminum alloy castings, and can also give high yield strength to Al-Si alloy castings. In addition, the object of the present invention is also to provide an Al-Si alloy casting joint body, which effectively suppresses the occurrence of cracks when self-piercing rivets are pressed into, and uses an Al-Si alloy casting with high yield strength and the Al-Si alloy casting as a joined material.
[0016] Technical means of solving problems
[0017] In order to achieve the above-mentioned purpose, the inventors have made great efforts to study the relationship between the composition, microstructure and mechanical properties of Al-Si alloy castings and cracks during the pressing of self-piercing rivets. As a result, it was found that the generation of cracks can be suppressed, especially by controlling the addition amount of Mg and Mn. The generation of cracks is strongly correlated with the limit bending angle of the bending test of the German Association of the Automotive Industry (Verband der Automobilindustrie, VDA), thus achieving the present invention.
[0018] That is, the present invention provides an Al-Si alloy for castings,
[0019] It is characterized by comprising:
[0020] Si: 5.0 mass% to 12.0 mass%,
[0021] Mn: 0.4 mass% to 1.5 mass%,
[0022] Mg: 0.05 mass% to 0.6 mass%,
[0023] Cr: 0.1 mass% to 0.5 mass%,
[0024] Fe: more than 0 mass % and 0.6 mass % or less,
[0025] The remainder includes Al and inevitable impurities.
[0026] In the Al-Si alloy for casting of the present invention, by adding 0.4 mass % or more of Mn, sintering of the mold can be prevented, and the needle-like formation of Al-Si-Fe system crystals can be suppressed, thereby suppressing the reduction in the elongation of the Al-Si alloy casting. In addition, by setting the addition amount of Mn to 1.5 mass % or less, the reduction in the elongation of the Al-Si alloy casting caused by the coarsening of the Al-Si-(Fe, Mn) system crystals can be suppressed.
[0027] Moreover, by adding 0.05 mass % or more of Mg, the mechanical properties of the Al-Si alloy casting can be improved by solid solution strengthening of Mg and precipitation strengthening of Mg-Si compounds. In addition, by setting the addition amount of Mn to 0.6 mass % or less, the excessive increase of deformation resistance can be suppressed, and the generation of cracks when the self-piercing rivet is pressed in can be suppressed very effectively.
[0028] In addition, in the Al-Si alloy for casting of the present invention,
[0029] Preferably it contains:
[0030] Cu: 0.05 mass% to 0.5 mass%,
[0031] Ca: 0.005 mass% to 0.03 mass%,
[0032] B: 0.001 mass% to 0.02 mass%,
[0033] Sr: 0.005 mass% to 0.03 mass%,
[0034] Sb: 0.01 mass% to 0.2 mass%,
[0035] Na: at least one of 0.002 mass % to 0.02 mass %.
[0036] By further adding these elements, the microstructure and mechanical properties of the Al-Si alloy casting can be adjusted, and the crack suppression effect when the self-piercing rivet is pressed in can be further improved. In addition, the desired yield strength can be given to the Al-Si alloy casting.
[0037] The strength and yield strength of Al-Si alloy castings can be increased by adding Cu, and the local elongation of Al-Si alloy castings can be improved by adding B. In addition, Ca, Sr, Sb and Na have the effect of refining and granulating eutectic Si, which can improve the elongation of Al-Si alloy castings.
[0038] The present invention also provides an Al-Si alloy casting, characterized by comprising the Al-Si alloy for casting of the present invention. The Al-Si alloy casting of the present invention effectively suppresses cracking when a self-piercing rivet is pressed in, and has a high yield strength.
[0039] In the Al-Si alloy casting of the present invention, the limiting bending angle of the VDA bending test specified in VDA238-100 is preferably 28° or more, more preferably 30° or more, and most preferably 33° or more.
[0040] Here, VDA is the German Association of the Automotive Industry standard (Verband der Automobilindustrie), and defines VDA238-100 as a plate bending test for the purpose of evaluating the fracture behavior when a member is crushed.
[0041] In the Al-Si alloy casting of the present invention, the 0.2% yield strength is preferably 100 MPa or more, more preferably 105 MPa or more, and most preferably 110 MPa or more.
[0042] Furthermore, the present invention also provides a self-piercing rivet joint, characterized in that it is a joint made by using a self-piercing rivet, and at least one of the joined members is the Al-Si alloy casting of the present invention.
[0043] In the self-piercing rivet joint of the present invention, the Al-Si alloy casting having excellent mechanical properties given various shapes is firmly mechanically fastened to other metal members, and the occurrence of cracks in the joint is suppressed, so it can be preferably used in various applications.
[0044] Effects of the Invention
[0045] According to the present invention, an Al-Si alloy for castings can be provided, which can effectively suppress cracks when self-piercing rivets are pressed into aluminum alloy castings, and can also give high yield strength to Al-Si alloy castings. In addition, an Al-Si alloy casting joint body can also be provided, which effectively suppresses cracks when self-piercing rivets are pressed into, and uses Al-Si alloy castings with high yield strength and the Al-Si alloy castings as joined materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0046] [ Figure 1 ] is a photograph of the appearance of the self-piercing rivet joint (Example 2).
[0047] [ Figure 2 ] is a photograph of the appearance of the Al-Si alloy sheet after the VDA bending test (Example 2).
[0048] [ Figure 3 ] is a photograph of the appearance of a self-piercing rivet joint (Comparative Example 1). DETAILED DESCRIPTION
[0049] Hereinafter, the Al-Si alloy for casting, the Al-Si alloy casting, and the Al-Si alloy casting joint of the present invention will be described in detail, but the present invention is not limited thereto.
[0050] 1. Al-Si alloy for castings
[0051] The Al-Si alloy for casting of the present invention is characterized in that Mn, Mg, Cr and Fe are added in combination to the hypoeutectic Al-Si alloy.
[0052] (1) Necessary additional elements
[0053] Si: 5.0 mass% to 12.0 mass%
[0054] Si has the effect of improving the castability of aluminum alloy and the effect of improving mechanical properties such as tensile strength. The above effects become significant when the content is 5.0 mass % or more. If the content exceeds 12.0 mass %, the eutectic Si or primary Si tends to coarsen, the elongation decreases, and cracks are easily generated when the self-piercing rivet is pressed. The amount of Si added is preferably 6.0 mass % to 9.0 mass %.
[0055] Mn: 0.4 mass% to 1.5 mass%
[0056] Mn has the effect of preventing sintering of the mold and inhibiting the needle-like formation of Al-Si-Fe series crystals and the effect of inhibiting the reduction of elongation. The above effect becomes significant when it is above 0.4 mass%. On the contrary, if it exceeds 1.5 mass%, Al-Si-(Fe, Mn) series crystals tend to coarsen, which becomes the main reason for the reduction of elongation. The content of Mn is preferably set to 0.5 mass% to 0.7 mass%.
[0057] Mg: 0.05 mass% to 0.6 mass%
[0058] Mg has the effect of being dissolved in Al to improve mechanical properties, and has the effect of precipitating as a Mg-Si compound together with Si during aging treatment to improve mechanical properties. The above effect becomes significant when it is above 0.05 mass%, on the contrary, if it exceeds 0.6 mass%, the deformation resistance increases, and cracks are easily generated when self-piercing rivets are driven. The addition amount of Mg is preferably set to 0.05 mass% to 0.3 mass%, and more preferably set to 0.05 mass% to 0.14 mass%.
[0059] Cr: 0.1 mass% to 0.5 mass%
[0060] Cr has the effect of preventing sintering of the mold and improving corrosion resistance. The above effects become significant when the content is 0.1 mass % or more. On the contrary, when the content exceeds 0.5 mass %, coarse compounds are easily formed, and the elongation is easily reduced.
[0061] Fe: more than 0 mass% and 0.6 mass% or less
[0062] Fe has the effect of improving mechanical properties such as tensile strength and preventing the seizure of the mold. If it exceeds 0.6 mass%, the elongation decreases and cracks are likely to occur when driving a self-piercing rivet.
[0063] (2) Add any elements
[0064] Cu: 0.05 mass% to 0.5 mass%
[0065] Cu has the effect of improving mechanical properties, and the effect becomes significant when the content is 0.05 mass % or more. On the contrary, if it exceeds 0.5 mass %, the corrosion resistance decreases. The content of Cu is preferably set to 0.2 mass % to 0.4 mass %.
[0066] B: 0.001 mass% to 0.02 mass%
[0067] B has the effect of improving local elongation and improving the bonding properties of self-piercing rivets. The above effect becomes significant when it is 0.001 mass % or more. On the contrary, if it exceeds 0.02 mass %, it will become the main cause of increased production costs.
[0068] Ca: 0.005 mass% to 0.03 mass%
[0069] By adding 0.005 mass % to 0.03 mass % of Ca, eutectic Si can be made fine and granular. When eutectic Si is made fine and granular, elongation is improved, and cracks generated when self-piercing rivets are pressed in can be suppressed.
[0070] Sr: 0.005 mass% to 0.03 mass%
[0071] By adding 0.005 mass % to 0.03 mass % of Sr, eutectic Si can be made fine and granular. When eutectic Si is made fine and granular, elongation is improved, and cracks generated when self-piercing rivets are pressed in can be suppressed.
[0072] Sb: 0.01 mass% to 0.2 mass%
[0073] By adding 0.01 mass % to 0.2 mass % of Sb, eutectic Si can be made fine and granular. When eutectic Si is made fine and granular, elongation is improved, and cracks generated when self-piercing rivets are pressed in can be suppressed.
[0074] Na: 0.002 mass% to 0.02 mass%
[0075] By adding 0.002 mass % to 0.02 mass % of Na, eutectic Si can be made fine and granular. When eutectic Si is made fine and granular, elongation is improved, and cracks generated when self-piercing rivets are pressed in can be suppressed.
[0076] Ti: 0.005 mass% to 0.2 mass%
[0077] Ti has the effect of making the casting structure fine and improving castability and elongation. The above effect becomes significant when it is 0.005 mass% or more. On the contrary, if it exceeds 0.2 mass%, coarse crystals are easily formed and the elongation is easily reduced.
[0078] 2.Al-Si alloy castings
[0079] The Al-Si alloy casting of the present invention is characterized in that it comprises the Al-Si alloy for casting of the present invention, has high yield strength, and suppresses cracking when a self-piercing rivet is pressed in. The microstructure and mechanical properties are described in detail below.
[0080] (1) Metal structure
[0081] The reason why the Al-Si alloy casting of the present invention has excellent self-piercing rivet joinability in terms of metal structure is not necessarily clear, but it is considered that the reason is that in addition to suppressing the needle-like and coarsening of various crystals, the formation of eutectic Si aggregates is suppressed.
[0082] When fragile eutectic Si aggregates are formed, cracks propagate along the aggregates, so cracks are easily generated when the self-piercing rivet is pressed in. In the Al-Si alloy casting of the present invention, a tendency to suppress the formation of eutectic Si aggregates is confirmed, and the generation of cracks when the self-piercing rivet is pressed in can be effectively suppressed.
[0083] In addition, the method for confirming the presence or absence of eutectic Si aggregates is not particularly limited, and various microstructure observation methods known in the art can be used. For example, when a cross section of an Al-Si alloy casting after mirror polishing is observed using an optical microscope or a scanning electron microscope (SEM), and when eutectic Si is continuously formed to a thickness of 50 μm or more, it can be determined that an aggregate of eutectic Si that promotes the generation and propagation of cracks is formed.
[0084] (2) Mechanical properties
[0085] The Al-Si alloy casting of the present invention has excellent tensile properties of high strength, yield strength and ductility, and can effectively suppress the generation of cracks when a self-piercing rivet is pressed in.
[0086] The mechanism of crack generation when self-piercing rivets are pressed in is complex, and it is difficult to evaluate using only measured values related to the mechanical properties of Al-Si alloy castings, such as tensile properties or hardness. In contrast, the inventors and others have conducted intensive research and have found that the limit bending angle of the VDA bending test specified in VDA238-100 is strongly correlated with the presence or absence of cracks when self-piercing rivets are pressed in.
[0087] More specifically, in order to suppress cracks when the self-piercing rivet is pressed, it is preferred to set the limit bending angle of the VDA bending test specified by VDA238-100 to 28° or more. The more preferred limit bending angle is 30° or more, and the most preferred limit bending angle is 33° or more. For example, in the case of an Al-Si alloy casting having tensile properties of 0.2% yield strength of 100MPa to 120MPa and elongation at break of about 10% to 14%, by setting the limit bending angle of the VDA bending test to 28° or more, the occurrence of cracks can be almost completely suppressed as long as the general joining conditions are met.
[0088] In the Al-Si alloy casting of the present invention, the 0.2% yield strength is preferably 100 MPa or more. The 0.2% yield strength is more preferably 105 MPa or more, and most preferably 110 MPa or more. In addition, the elongation at break is preferably 10%, more preferably 12% or more, and most preferably 14% or more.
[0089] The Al-Si alloy casting of the present invention can be manufactured by adjusting the raw materials in a manner that the composition of the Al-Si alloy casting for casting of the present invention is obtained, and casting is performed using various known casting methods (sand casting, mold casting, gravity casting, low pressure casting, and die casting, etc.). That is, the aluminum alloy casting of the present invention is not limited to a casting cast using a specific casting method.
[0090] Furthermore, the casting conditions are not particularly limited unless the effects of the present invention are impaired, and various conventionally known casting conditions can be used.
[0091] 3. Al-Si alloy casting joint (self-piercing rivet joint)
[0092] The self-piercing rivet joint of the present invention is characterized in that at least one of the members joined using the self-piercing rivet is the Al—Si alloy casting of the present invention.
[0093] In the self-piercing rivet joint, the Al-Si alloy casting having excellent mechanical properties given various shapes is firmly mechanically fastened to other metal members, and the occurrence of cracks in the joint is suppressed, so it can be preferably used in various applications.
[0094] As long as the effect of the present invention is not impaired, the material, shape and size of the self-piercing rivet are not particularly limited, and various self-piercing rivets known in the art can be used. In addition, as long as the effect of the present invention is not impaired, the pressing area of the self-piercing rivet is not particularly limited, and can be appropriately determined according to the desired joint body.
[0095] Furthermore, the other joined material to be joined to the Al-Si alloy casting of the present invention is not particularly limited unless the effects of the present invention are impaired, and various conventionally known joined materials to which self-piercing rivets can be applied can be used.
[0096] Furthermore, as long as the effects of the present invention are not impaired, the conditions for pressing the self-piercing rivet are not particularly limited and may be appropriately adjusted according to the material, shape, size, etc. of the self-piercing rivet and the materials to be joined.
[0097] As mentioned above, although the typical embodiment of this invention was demonstrated, this invention is not limited to these only, Various design changes are possible, and these design changes are all included in the technical scope of this invention.
[0098] Example
[0099] 《Implementation Examples》
[0100] The raw materials prepared in the composition (mass %) shown in Examples 1 to 8 in Table 1 were melted at 750°C, and after deslagging treatment using a flux for cleaning the molten metal and degassing treatment using Ar gas blowing, Al-Si alloy plates as Al-Si alloy castings according to the present invention were obtained by pore free (PF) die casting under the conditions of high-speed injection speed: 2.0 mm / s, casting pressure: 80±5 MPa, casting temperature: 730±10°C (Examples 1 to 8, Comparative Example 3), 700±10°C (Comparative Example 1, Comparative Example 2), and mold temperature: 100°C to 150°C. The size of the Al-Si alloy plate was 110 mm×110 mm×3 mm.
[0101] [Table 1]
[0102]
[0103] By cutting the Al-Si alloy plate into a size of 100mm×30mm×3mm, overlapping a steel plate (cold rolled steel plate (Steel Plate Cold Commercial, SPCC)) of 100mm×30mm×1mm, and driving rivets with an outer diameter of 5.2mm and a length of 4.4mm in the body into three locations from the steel plate side, self-piercing rivet joining is performed. The joining test was carried out 5 times for each composition, and a total of 15 self-piercing rivet joints were confirmed for the presence or absence of cracks, and the crack occurrence rate was evaluated. More specifically, the crack occurrence rate is calculated as "crack occurrence rate = (number of joints confirmed to have cracks / 15)×100". The crack occurrence rates obtained are shown in Table 1. In addition, a photograph of the appearance of the self-piercing rivet joints in the Al-Si alloy plate having the composition of Example 2 is shown. Figure 1 .exist Figure 1The self-piercing rivet joint shown has no cracks at all.
[0104] In addition, the Al-Si alloy sheet was subjected to a VDA bending test specified in VDA238-100, and the limit bending angle was evaluated. The obtained limit bending angles are shown in Table 1. The appearance photograph of the Al-Si alloy sheet having the composition of Example 2 after the VDA bending test is shown in Table 1. Figure 2 .
[0105] Furthermore, the tensile properties of the Al-Si alloy plate were evaluated. A 14B tensile test piece of JIS Z 2241 was cut out from the Al-Si alloy plate and subjected to a tensile test at a tensile speed of 5 mm / min. The obtained tensile strength, 0.2% yield strength and elongation at break are shown in Table 1.
[0106] 《Comparative Example》
[0107] Al—Si alloy plates as comparative Al—Si alloy castings of the present invention were obtained in the same manner as in the examples except that raw materials were prepared to have the compositions (mass %) shown in Comparative Examples 1 to 3 in Table 1.
[0108] In addition, the crack generation rate of the self-piercing rivet joint and the limit bending angle of the VDA bending test were evaluated in the same manner as in the examples. The obtained crack generation rate and limit bending angle are shown in Table 1. In addition, the appearance photograph of the self-piercing rivet joint of the Al-Si alloy sheet material having the composition of Comparative Example 1 is shown in Figure 3 Significant cracks were confirmed in the self-piercing rivet joints.
[0109] According to the results shown in Table 1, it can be confirmed that the Al-Si alloy sheet material as the Al-Si alloy casting according to the present invention has excellent self-piercing rivet bonding properties. In addition, it is confirmed that the crack generation rate is strongly correlated with the limit bending angle of the VDA bending test, and it is known that the generation of cracks can be effectively suppressed by setting the limit bending angle to 28° or more.
[0110] In addition, the results of the tensile test show that the Al-Si alloy sheet material, which is the Al-Si alloy casting according to the present invention, has a low crack generation rate and excellent tensile properties.
[0111] In contrast, in the case of the compositions of Comparative Examples 1 and 2 having low Mg contents, and the composition of Comparative Example 3 having high Mn and Mg contents, the limit bending angle of the VDA bending test becomes small, and the crack occurrence rate of the self-piercing rivet joint becomes a high value.
Claims
1. An Al-Si alloy for castings, It is characterized in that contain: Si: 5.0 mass% to 12.0 mass%, Mn: 0.4 mass% to 1.5 mass%, Mg: 0.05 mass% to 0.6 mass%, Cr: 0.1 mass% to 0.5 mass%, Fe: more than 0 mass % and 0.6 mass % or less, The remainder includes Al and inevitable impurities.
2. The Al-Si alloy for casting according to claim 1, It is characterized in that contain: Cu: 0.05 mass% to 0.5 mass%, Ca: 0.005 mass% to 0.03 mass%, B: 0.001 mass% to 0.02 mass%, Sr: 0.005 mass% to 0.03 mass%, Sb: 0.01 mass% to 0.2 mass%, Na: at least one of 0.002 mass % to 0.02 mass %.
3. An Al-Si alloy casting, Features , The present invention comprises the Al-Si alloy for casting according to claim 1 or 2.
4. The Al-Si alloy casting according to claim 3, It is characterized in that The limit bending angle of the VDA bending test specified by VDA 238-100 is 28° or more.
5. The Al-Si alloy casting according to claim 3, It is characterized in that The 0.2% yield strength is 100 MPa or more.
6. A self-piercing rivet joint, It is characterized in that It is a joint body joined by self-piercing rivets. At least one of the joined members is the Al—Si alloy casting according to claim 3 .
Citation Information
Cited By
High-toughness aluminum alloy bolt and preparation method thereof
CN122344672A