Electrode for all-solid-state battery
By using particles coated with sulfide-based solid electrolytes in the electrodes of all-solid-state batteries, the problems of moisture sensitivity and insufficient porosity are solved, thereby improving the conductivity and performance of the batteries.
Patent Information
- Application Number
- CN202380023476.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-09-01
- Filing Date
- 2023-08-29
- Publication Date
- 2024-11-05
AI Technical Summary
In existing all-solid-state batteries, sulfide-based solid electrolytes are sensitive to moisture, and the agglomeration and insufficient porosity of active materials and solid electrolytes affect battery performance.
The electrodes are made of particles coated with sulfide-based solid electrolytes. The particles contain active materials, conductive materials and binders. The conductive material is carbon black with an average particle size of 120 nm to 200 nm. The carbon black agglomerates to form secondary particles. The particle porosity is 20% to 40%. The conductivity is improved by distributing the conductive material in specific areas.
This improved the conductivity and performance of the all-solid-state battery, ensured the conductivity of the electrodes and the effective loading of active materials, and reduced the impact of moisture sensitivity.
Smart Images

Figure CN118901153A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to an electrode for an all-solid-state battery. In particular, the present invention relates to a positive electrode for an all-solid-state battery comprising particles coated with a sulfide-based solid electrolyte.
[0002] This application claims priority to Korean Patent Application No. 10-2022-0110540 filed on September 1, 2022, the entire contents of which are incorporated as a part of this specification. Background Art
[0003] Various batteries are being researched to overcome the limitations of conventional lithium secondary batteries in terms of capacity, safety, power output, large-scale and miniaturization.
[0004] For example, research is continuing in academia and industry on metal-air batteries that have a very large theoretical capacity compared to lithium secondary batteries, all-solid-state batteries that do not have an explosion risk in terms of safety, supercapacitors in terms of power output, NaS batteries or redox flow batteries (RFBs) in terms of large-scale development, and thin-film batteries in terms of miniaturization.
[0005] Among them, all-solid-state batteries are batteries that use solid electrolytes instead of liquid electrolytes commonly used in lithium secondary batteries, and since no flammable solvents are used in the battery, there is no fire or explosion usually caused by the decomposition reaction of the electrolyte, which can greatly improve safety. In addition, since Li metal or Li alloy can be used as the negative electrode material, it has the advantage of significantly improving the energy density per unit mass and per unit volume of the battery.
[0006] Among solid electrolytes used in all-solid-state batteries, inorganic solid electrolytes can be divided into sulfide-based electrolytes and oxide-based electrolytes. Currently, the most technologically advanced solid electrolytes are sulfide-based solid electrolytes, and materials whose ionic conductivity is close to that of organic electrolytes have been developed.
[0007] Among solid electrolytes, sulfide solid electrolytes have 10 -3 Up to 10 -2 S / cm, and their ductility allows them to make good contact with the interface, which is beneficial for improving resistance, but they are sensitive to moisture and produce H2S gas when in contact with moisture, so a very dry environment needs to be established during manufacturing. In addition, the agglomeration of active materials and solid electrolytes needs to be improved, and high-density electrodes are required due to the reduction of porosity.
[0008] Therefore, the inventors of the present invention continued to study electrodes for all-solid-state batteries to solve the challenges faced in the related art and completed the present invention.
[0009] [Prior Art References]
[0010] [Patent References]
[0011] (Patent Reference 1) Korean Patent Publication No. 10-2016-0146737 Summary of the Invention
[0012] [Technical Problem]
[0013] The present invention aims to provide an electrode for an all-solid-state battery including particles coated with a sulfide-based solid electrolyte, which can improve the performance of the battery when used as an electrode for an all-solid-state battery.
[0014] [Technical Solution]
[0015] According to a first aspect of the present invention, there is provided an electrode for an all-solid-state battery including particles coated with a sulfide-based solid electrolyte, wherein the particles include an active material, a conductive material, and a binder, and the conductive material is carbon black having an average particle diameter of 120 nm to 200 nm.
[0016] In an embodiment of the present invention, the BET specific surface area of the carbon black is 15 m 2 / g to 35 m 2 / g.
[0017] In an embodiment of the present invention, the DBP absorption rate of the carbon black is 70 mL / 100 g to 100 mL / 100 g.
[0018] In an embodiment of the present invention, the carbon black agglomerates to form secondary particles, and the particle diameter of the secondary particles is 600 nm to 1,100 nm.
[0019] In an embodiment of the present invention, the particles are spherical particles having a diameter of 30 μm to 150 μm.
[0020] In an embodiment of the present invention, the porosity of the particles is 20% to 40%.
[0021] In an embodiment of the present invention, the electrode for an all-solid-state battery is a positive electrode, and the active material is selected from LiCoO2, LiNiO2, LiMnO2, Li2MnO3, LiMn2O4, Li(Ni a Co b Mn c )O2 (where 0 < a < 1, 0 < b < 1, 0 < c < 1, and a + b + c = 1), LiNi 1-y Co y O2 (where 0 < y < 1), LiCo 1-y Mny O2, LiNi 1-y Mn y O2 (where 0 < y < 1), Li(Ni a Co b Mn c )O4 (where 0 < a < 2, 0 < b < 2, 0 < c < 2, and a + b + c = 2), LiMn 2-z Ni z O4 (where 0 < z < 2), LiMn 2-z Co z O4 (where 0 < z < 2) and combinations thereof.
[0022] In one embodiment of the present invention, the binder is an organic binder, and the organic binder is selected from the group consisting of: polyvinylidene fluoride (PVDF), vinylidene fluoride - hexafluoropropylene copolymer (PVDF - co - HFP), polyvinyl alcohol, starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, polyimide, polyamideimide, polyethylene, polypropylene, ethylene - propylene - diene monomer (EPDM), sulfonated EPDM, styrene - butadiene rubber, and fluororubber.
[0023] In one embodiment of the present invention, the particles comprise 85 wt% to 99.8 wt% of the active material, 0.1 wt% to 10 wt% of the binder, and 0.1 wt% to 10 wt% of the conductive material.
[0024] In one embodiment of the present invention, in the electrode for an all - solid - state battery, the thickness of the electrode active material layer comprising particles coated with a sulfide - based solid electrolyte is 100 μm to 300 μm.
[0025] In one embodiment of the present invention, in the electrode for an all - solid - state battery, the electrode active material layer comprising particles coated with a sulfide - based solid electrolyte comprises 10 wt% to 30 wt% of the sulfide - based solid electrolyte based on the content of the particles.
[0026] In one embodiment of the present invention, when the inner diameter of the particles is divided into equal intervals and divided into a first region, a second region, and a third region from the center of the particles to the outside, the content of the conductive material in the particles increases in the order of the first region, the second region, and the third region.
[0027] In one embodiment of the present invention, the R value of the particles is 5 or less, and the R value is defined by the following formula 1.
[0028] According to the second aspect of the present invention, the present invention provides an all - solid - state battery comprising the electrode for an all - solid - state battery as a positive electrode or a negative electrode.
[0029] [Beneficial Effects]
[0030] In an electrode for an all-solid-state battery comprising particles coated with a sulfide-based solid electrolyte, the particles contain an active material, a conductive material and a binder, and the physical properties of the primary or secondary particles of carbon black as the conductive material contained in the particles are specifically specified, thereby improving the conductivity of the particles and improving the performance of a battery using the particles. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1a is a SEM image of particles of Preparation Example 1 according to Experimental Example 1 (×1,000 magnification).
[0032] Figure 1b is a SEM image of particles of Preparation Example 1 according to Experimental Example 1 (×5,000 magnification).
[0033] Figure 2a is a SEM image of particles of Comparative Preparation Example 1 according to Experimental Example 1 (×1,000 magnification).
[0034] Figure 2b is a SEM image of particles of Comparative Preparation Example 1 according to Experimental Example 1 (×5,000 magnification).
[0035] Figure 3 Schematic diagram of the positions of the first region (A), the second region (B), and the third region (C) in a particle. DETAILED DESCRIPTION
[0036] The embodiments provided by the present invention can be realized through the following description. It should be understood that the following describes the preferred embodiments of the present invention, but the present invention is not necessarily limited thereto.
[0037] For the properties described herein, if the measurement conditions and methods are not specifically described, the properties are measured according to the measurement conditions and methods commonly used by those skilled in the art.
[0038] In one aspect of the present invention, an electrode for an all-solid-state battery comprising particles coated with a sulfide-based solid electrolyte is provided. The particles are spherical particles comprising an active material, a conductive material, and a binder. Here, spherical particles do not necessarily mean perfectly spherical particles, but generally include the concept of round particles. The powdered granular active material is combined with a conductive material as a primary particle or a secondary particle through a binder solution to grow into particles with a certain specification range. The conductive material can be applied as a primary particle, a secondary particle, or a mixture of a primary particle and a secondary particle.
[0039] According to one embodiment of the present invention, the particles are spherical particles having a diameter of 30 μm to 150 μm. Here, since the spherical particles do not represent perfectly spherical particles, the diameter represents the maximum value of the distance from any point on the particle surface to a point on another surface. Specifically, the diameter of the particles may be 30 μm or more, 35 μm or more, 40 μm or more, 45 μm or more, 50 μm or more, 150 μm or less, 145 μm or less, 140 μm or less, 135 μm or less, 130 μm or less, 125 μm or less, or 120 μm or less, and may be 30 μm to 150 μm, 40 μm to 140 μm, or 50 μm to 120 μm. If the diameter of the particles is less than the above range, since there are fewer pores in the particle layer, the amount of sulfide-based solid electrolyte infiltrated and coated on the particles may decrease, and the improvement in battery performance may not be obvious. If the diameter of the particles is greater than the above range, the distance between the surface in contact with the sulfide-based solid electrolyte and the center of the particles may increase, and the improvement in battery performance may not be obvious.
[0040] The electrode for an all-solid-state battery according to one embodiment of the present invention may be a negative electrode or a positive electrode, and more specifically, a positive electrode.
[0041] When the electrode is a negative electrode, the electrode active material contained in the particles may be any material that can be used as a negative electrode active material in a lithium-ion secondary battery. For example, the negative electrode active material may be one or more selected from the following: carbon, such as anthracite or graphitized carbon; metal composite oxides, such as Li x Fe2O3 (where 0 ≤ x ≤ 1), Li x WO2 (where 0 ≤ x ≤ 1), or Sn x Me 1-x Me’ y O z (where Me is Mn, Fe, Pb, or Ge; Me’ is Al, B, P, Si, an element of Group 1, 2, or 3 of the periodic table, or a halogen; 0 < x ≤ 1; 1 ≤ y ≤ 3; and 1 ≤ z ≤ 8); lithium metal; lithium alloy; silicon-based alloy; tin-based alloy; metal oxides, such as SnO, SnO2, PbO, PbO2, Pb2O3, Pb3O4, Sb2O3, Sb2O4, Sb2O5, GeO, GeO2, Bi2O3, Bi2O4, or Bi2O5; conductive polymers, such as polyacetylene; Li-Co-Ni-based materials; titanium oxide; and lithium titanium oxide. According to one embodiment of the present invention, the negative electrode active material may contain a carbon-based material and / or Si.
[0042] When the electrode is a positive electrode, the electrode active material contained in the particles can be any electrode active material that can be used as a positive electrode active material in a lithium ion secondary battery. For example, the positive electrode active material can be a lithium transition metal oxide containing one or more transition metals. In one embodiment of the present invention, the positive electrode active material can be selected from the group consisting of: LiCoO2, LiNiO2, LiMnO2, Li2MnO3, LiMn2O4, Li(Ni a Co b Mn c )O2 (where 0 < a < 1, 0 < b < 1, 0 < c < 1, and a + b + c = 1), LiNi 1-y Co y O2 (where 0 < y < 1), LiCo 1-y Mn y O2, LiNi 1-y Mn y O2 (where 0 < y < 1), Li(Ni a Co b Mn c )O4 (where 0 < a < 2, 0 < b < 2, 0 < c < 2, and a + b + c = 2), LiMn 2-z Ni z O4 (where 0 < z < 2), LiMn 2-z Co z O4 (where 0 < z < 2) and combinations thereof.
[0043] The conductive material contained in the particles of one embodiment of the present invention is carbon black having an average particle diameter of 120 nm to 200 nm. The average particle diameter is the arithmetic average of the particle diameters. Specifically, the average particle diameter of the carbon black can be 120 nm or more, 125 nm or more, 130 nm or more, 135 nm or more, 200 nm or less, 190 nm or less, 180 nm or less, 170 nm or less, and can be 120 nm to 200 nm, 130 nm to 190 nm, or 135 nm to 170 nm. When the diameter of the carbon black is less than the above range, the external area of the carbon black is too small, making it difficult for the conductive material to form a structure that can effectively function between multiple active material particles. If the diameter of the carbon black exceeds the above range, it is difficult for the conductive material to be dispersed and positioned at an appropriate position. In addition, the conductive material having a particle diameter within the above range helps to form secondary particles having desired properties.
[0044] According to one embodiment of the present invention, the BET specific surface area of the carbon black is 15 m 2 / g to 35 m 2 / g. The BET specific surface area is the specific surface area measured by the BET method. Specifically, the BET specific surface area of the carbon black is greater than or equal to 15 m 2 / g, greater than or equal to 16m 2 / g, greater than or equal to 17m 2 / g, greater than or equal to 18m 2 / g, greater than or equal to 19m 2 / g, greater than or equal to 20m 2 / g, 35m 2 / g or less, 34m 2 / g or less, 33m 2 / g or less, 32m 2 / g or less, 31m 2 / g or less, 30m 2 / g or less, or can be 15m 2 / g to 35m 2 / g, 17m 2 / g to 33m 2 / g or 20m 2 / g to 30m 2 / g. If the BET specific surface area of carbon black is less than the above range, the area in contact with the active material may be reduced relative to the weight of the carbon black, and it may be difficult to ensure functionality. If the BET specific surface area of carbon black is greater than the above range, it may be difficult to ensure functionality because the excessively large specific surface area is not easy to contact with the active material or the solid electrolyte. In addition, the conductive material having a BET specific surface area within the above range helps to form secondary particles having desired properties.
[0045] According to one embodiment of the present invention, carbon black as a conductive material is agglomerated to form secondary particles, wherein the particle size of the secondary particles is 600nm to 1,100nm. In this specification, carbon black before agglomeration into secondary particles may be represented as primary particles. Secondary particles may be agglomerates of various shapes, wherein the particle size represents the maximum value of the distance from any point on the surface of the particle to a point on another surface. When carbon black is agglomerated and used in the form of secondary particles, a highly functional structure can be formed because the electrolyte or active material can become accessible through the pores between the carbon blacks while maintaining a conductive network between the carbon blacks constituting the secondary particles. Specifically, the particle size of the secondary particles may be greater than 600nm, greater than 650nm, greater than 700nm, less than 1,100nm, less than 1,000nm, less than 900nm, 600nm to 1,100nm, 650nm to 1,000nm, or 700nm to 900nm. If the particle size of the secondary particles is smaller than the above range, the functionality that can be achieved by forming the secondary particles may be minimal. If the particle size of the secondary particles is larger than the above range, the conductive material may be over-concentrated, making it difficult to efficiently disperse the conductive material throughout the particles.
[0046] According to one embodiment of the present invention, the DBP absorption rate of carbon black as a conductive material is 70mL / 100g to 100mL / 100g. The DBP absorption rate indicates the torque change that occurs when impregnated with a plasticizer dibutyl phthalate (DBP), and the DBP absorption rate of the conductive material may affect the formation of secondary particles by the conductive material. Specifically, the DBP absorption rate of carbon black can be 70mL / 100g or more, 71mL / 100g or more, 72mL / 100g or more, 73mL / 100g or more, 74mL / 100g or more, 75mL / 100g or more, 100mL / 100g or less, 98mL / 100g or less, 96mL / 100g or less, 94mL / 100g or less, 92mL / 100g or less, 90mL / 100g or less, 70mL / 100g to 100mL / 100g, 73mL / 100g to 94mL / 100g, or 75mL / 100g to 90mL / 100g. Carbon black with DBP absorption rate in the above range helps to form secondary particles with desired properties.
[0047] The binder contained in the particles of one embodiment of the present invention is mixed with a powdered granular active material and a conductive material as a primary particle or a secondary particle, so as to bond these components and help the particles grow. Since sulfide solid electrolytes have moisture sensitivity, such as producing H2S gas when in contact with moisture, it is advantageous to exclude as much moisture as possible in the formation of particles. According to one embodiment of the present invention, the binder is an organic binder. An organic binder refers to an adhesive that is soluble or dispersible in an organic solvent, particularly N-methylpyrrolidone (NMP), which is different from an aqueous binder that is soluble or dispersible in water. Specifically, the organic binder can be selected from, but not limited to, the group consisting of: polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone, polyimide, polyamide-imide, polyethylene, polypropylene, ethylene-propylene-diene monomer (EPDM), sulfonated EPDM, styrene-butadiene rubber and fluororubber.
[0048] According to one embodiment of the present invention, in the particles, the content of the active material is 85 wt % to 99.8 wt %, particularly 88 wt % to 99.5 wt %, more particularly 90 wt % to 99.3 wt %, the content of the binder is 0.1 wt % to 10 wt %, particularly 0.2 wt % to 8 wt %, more particularly 0.3 wt % to 7 wt %, and the content of the conductive material is 0.1 wt % to 10 wt %, particularly 0.15 wt % to 8 wt %, more particularly 0.2 wt % to 5 wt %. When the contents of the active material, the binder and the conductive material are adjusted within the above range, it is beneficial to improve the performance of the battery.
[0049] According to one embodiment of the present invention, the porosity of the particles is 20% to 40%. The porosity of the particles represents the ratio of the pore volume in the particles. Specifically, the porosity of the particles can be more than 20%, more than 21%, more than 22%, more than 23%, more than 24%, more than 25%, less than 40%, less than 39%, less than 38%, less than 37%, less than 36% or less than 35%. If the porosity of the particles is lower than the above range, the performance improvement of the battery may not be obvious because the sulfide solid electrolyte is difficult to be in close contact with the particles. If the porosity of the particles is higher than the above range, the amount of active material is reduced relative to the volume of the particles, resulting in difficulty in providing an electrode with a high active material loading, so the performance improvement of the battery may not be obvious.
[0050] Typically, in the preparation of particles, a binder solution is introduced together with a powdered particulate active material and a conductive material to grow the particle size of the particles to a certain level, wherein the interior of the device can be rotated to sphericalize the particles and separate them from each other. This rotation can produce centrifugal forces on the particles and may cause the components of the particles to be concentrated on the outside of the particles rather than in the center of the particles. However, when particles are prepared according to one embodiment of the present invention, the migration of conductive materials to the surface of the particles can be minimized during the high temperature solvent drying process, so that the conductive materials are evenly distributed within the particles. This can be seen in the SEM images of Figures 1 and 2 according to the following Experimental Example 1. As shown in Figure 2, if a large amount of conductive material migrates to the surface of the particles, not only the porosity of the particles is reduced, but also the active materials in the particles are not easily exposed to the electrolyte, which can lead to a reduction in battery performance.
[0051] Figure 3 is a schematic diagram of the particle shape of one embodiment of the present invention, such as Figure 3As shown, the interior of the particle can be divided into a first region (region A), a second region (region B) and a third region (region C). The first region, the second region and the third region are divided by dividing the inner diameter of the particle into equal intervals, wherein the first region is located at the centralmost part of the particle, the third region is located at the outermost part of the particle, and the second region is located between the first region and the third region. According to one embodiment of the present invention, the content of the conductive material in the particle increases in the order of the first region, the second region and the third region.
[0052] According to one embodiment of the present invention, the R value of the particle is less than 5, less than 4.5, or less than 4. The R value quantifies the variation in the content of the conductive material between adjacent regions and is defined by the following formula 1:
[0053] [Formula 1]
[0054]
[0055] Among them, r A is the content (%) of the conductive material in the first region, r B is the content (%) of the conductive material in the second region, r C is the content (%) of the conductive material in the third region. Since the content of the conductive material in each region is based on the total content of the conductive material in the particle, r A 、r B and r C The sum is 100%. Basically, since the content of the conductive material of one embodiment of the present invention increases in the order of the first region, the second region, and the third region, the value of R is greater than or equal to 1. If the content of the conductive material in these regions varies greatly, the R value can be higher, and if the content of the conductive material in these regions varies little, the R value can be lower. Although a low R value may help to improve the conductivity of the entire particle due to the uniform distribution of the conductive material, the conductivity of the particle is affected not only by the R value but also by the size, shape, content, etc. of the conductive material.
[0056] In an electrode for an all-solid-state battery, a solid electrolyte is coated on at least a portion of the surface or the entire surface of the particles. The solid electrolyte may be a polymer solid electrolyte formed by adding a polymer resin to a solvated lithium salt, or a polymer gel electrolyte formed by embedding an organic electrolyte, an ionic liquid, a monomer or an oligomer containing an organic solvent and a lithium salt in a polymer resin. The solid electrolyte may use one or more selected from a polymer solid electrolyte, a sulfide solid electrolyte and an oxide solid electrolyte, and according to one embodiment of the present invention, the solid electrolyte is a sulfide solid electrolyte. In an electrode for an all-solid-state battery, a sulfide solid electrolyte is applied by impregnating a sulfide electrolyte with a particle layer composed of particles and then drying it.
[0057] According to one embodiment of the present invention, the lithium salt can be Li + X - The anion of the lithium salt is not particularly limited, but may include, for example, F - , Cl - Br - ,I - 、NO3 - 、N(CN)2 - 、BF4 - 、ClO4 - PF6 - 、(CF3)2PF4 - 、(CF3)3PF3 - 、(CF3)4PF2 - 、(CF3)5PF - 、(CF3)6P - CF3SO3 - CF3CF2SO3 - 、(CF3SO2)2N - 、(FSO2)2N - 、 CF3CF2(CF3)2CO-, (CF3SO2)2CH-, (SF5)3C - 、(CF3SO2)3C - CF3(CF2)7SO3 - CF3CO2 - 、CH3CO2 - 、SCN - and (CF3CF2SO2)2N - . In one embodiment of the present invention, the sulfide-based solid electrolyte contains sulfur (S) and has the ionic conductivity of a metal of Group 1 or 2 of the periodic table, and may include Li-PS-based glass or Li-PS-based glass ceramics. Non-limiting examples of sulfide-based solid electrolytes may be the following or include one or more thereof: Li2S-P2S5, Li2S-LiI-P2S5, Li2S-LiI-Li2O-P2S5, Li2S-LiBr-P2S5, Li2S-LiCl-P2S5, Li2S-Li2O-P2S5, Li2S-Li3PO4-P2S5, Li2S-P2S5-P2O5, Li2S-P2S5-SiS2, Li2S-P2S5-SnS, Li2S-P2S5-Al2S3, Li2S-GeS2, and Li2S-GeS2-ZnS.
[0058] The all-solid-state battery electrode of one embodiment of the present invention can be prepared by loading particles onto a current collector to produce a flaky particle layer, then impregnating the particle layer with a sulfide electrolyte and drying it. The current collector is a conductive material such as a metal plate, and an electrode known in the art can be appropriately used according to the polarity of the battery.
[0059] According to one embodiment of the present invention, in an electrode for an all-solid-state battery, the thickness of the electrode active material layer containing particles coated with a sulfide solid electrolyte is 100 μm to 300 μm. If a current collector is used in the manufacture of the electrode, the electrode active material layer refers to a sheet-like layer coated on the current collector that does not include the current collector. Specifically, the thickness of the electrode active material layer may be 100 μm or more, 110 μm or more, 120 μm or more, 130 μm or more, 140 μm or more, 150 μm or more, 300 μm or less, 290 μm or less, 280 μm or less, 270 μm or less, 260 μm or less, or 250 μm or less. If the thickness of the electrode active material layer is less than the above range, the load of the active material may be reduced and the performance improvement of the battery may not be obvious. If the thickness of the electrode active material layer exceeds the above range, the durability of the electrode may be reduced and the performance improvement of the battery may not be obvious.
[0060] According to one embodiment of the present invention, in an electrode for an all-solid-state battery, an electrode active material layer comprising particles coated with a sulfide solid electrolyte comprises a sulfide solid electrolyte accounting for 10% to 30% by weight of the particle content. Specifically, the content of the sulfide solid electrolyte may be 10% by weight or more, 11% by weight or more, 12% by weight or more, 13% by weight or more, 14% by weight or more, 15% by weight or more, 30% by weight or less, 29% by weight or less, 28% by weight or less, 27% by weight or less, 26% by weight or less, or 25% by weight or less. If the content of the sulfide solid electrolyte is lower than the above range, as an all-solid-state battery, since it is difficult for electrons to be transmitted between the electrolyte and the active material, the performance improvement of the battery may not be significant, and if the content of the sulfide solid electrolyte exceeds the above range, the performance improvement of the battery may not be significant due to the relative reduction in the load of the active material.
[0061] In one aspect of the present invention, an all-solid-state battery comprising the all-solid-state battery electrode as a positive electrode and / or a negative electrode is provided. When preparing an all-solid-state battery, in addition to the solid electrolyte contained in the electrode, a separate solid electrolyte layer can be introduced between the positive electrode and the negative electrode, and the solid electrolyte layer can act as a separator in a conventional lithium secondary battery. In some cases, the electrode can be used in a semi-solid-state battery with a liquid electrolyte, which may further require a separate polymer separator.
[0062] The polymer separator is placed between the negative electrode and the positive electrode, and is used to electrically isolate the negative electrode from the positive electrode while allowing lithium ions to pass through. The polymer separator can be any polymer separator conventionally used in the field of all-solid-state batteries, but is not particularly limited thereto.
[0063] In one aspect of the present invention, a battery module including the all-solid-state battery as a unit cell, a battery pack including the battery module, and a device including the battery pack as a power source are provided.
[0064] Specific examples of the device include, but are not limited to: power tools powered by electric motors; electric vehicles, including electric vehicles (EVs), hybrid electric vehicles (HEVs), and plug-in hybrid electric vehicles (PHEVs); electric two-wheeled vehicles, including electric bicycles (E-bikes) and electric scooters; electric golf carts; and electrical energy storage systems.
[0065] Hereinafter, examples are provided to facilitate understanding of the present invention. The following examples are provided to illustrate the present invention, but the present invention is not limited thereto.
[0066] Preparation Example: Preparation of Particles Containing Active Materials
[0067] Preparation Example 1
[0068] LiNi as active material 0.6 Co 0.2 Mn 0.2 O2 (NCM 622), agglomerated carbon black (average particle size (D 50 ) is about 150nm, and the BET specific surface area is about 25m 2 / g, DBP absorption is about 81mL / 100g) secondary particles (particle size is about 800nm) and polyvinylidene fluoride (PVDF) as a binder are mixed in an N-methylpyrrolidone solvent in a weight ratio of 94:3:3 (active material: conductive material: binder) to prepare a slurry, and then particles with a diameter of about 60μm (porosity of 31%) are prepared by spray drying.
[0069] Comparative Preparation Example 1
[0070] LiNi as active material 0.6 Co 0.2 Mn 0.2 O2 (NCM 622), agglomerated carbon black (average particle size (D 50 ) is about 30nm, and the BET specific surface area is about 120m 2 / g, DBP absorption is about 190mL / 100g) secondary particles (particle size is about 150nm) and polyvinylidene fluoride (PVDF) as a binder are mixed in an N-methylpyrrolidone solvent in a weight ratio of 94:3:3 (active material: conductive material: binder) to prepare a slurry, and then particles with a diameter of about 60μm (porosity of 15%) are prepared by a spray drying method.
[0071] Comparative Preparation Example 2
[0072] LiNi as active material 0.6 Co 0.2 Mn 0.2 O2 (NCM 622), agglomerated carbon black (average particle size (D 50 ) is about 40nm, and the BET specific surface area is about 90m 2 / g, DBP absorption is about 230mL / 100g) secondary particles (particle size is about 750nm) and polyvinylidene fluoride (PVDF) as a binder are mixed in an N-methylpyrrolidone solvent in a weight ratio of 94:3:3 (active material: conductive material: binder) to prepare a slurry, and then particles with a diameter of about 60μm (porosity of 19%) are prepared by a spray drying method.
[0073] Comparative Preparation Example 3
[0074] LiNi as active material 0.6 Co 0.2 Mn 0.2 O2 (NCM 622), agglomerated carbon black (average particle size (D 50 ) is about 280nm, and the BET specific surface area is about 9m 2 / g, DBP absorption is about 40mL / 100g) secondary particles (particle size is about 3,000nm) and polyvinylidene fluoride (PVDF) as a binder are mixed in an N-methylpyrrolidone solvent in a weight ratio of 94:3:3 (active material: conductive material: binder) to prepare a slurry, and then particles with a diameter of about 60μm (porosity of 37%) are prepared by a spray drying method.
[0075] The properties of the particles prepared in Preparation Example 1 and Comparative Preparation Examples 1 to 3 are summarized in Table 1 below.
[0076] [Table 1]
[0077]
[0078] 1) Average particle size (nm) of primary particles of the conductive material: The particle size of each particle discernible in a scanning electron microscope (SEM) image was measured, and the arithmetic mean of the measured values was calculated.
[0079] 2) BET specific surface area of primary particles of conductive material (m 2 / g): calculated by mass gas adsorption at liquid nitrogen temperature (77K) using BELSORP-mino II manufactured by BEL Japan.
[0080] 3) DBP absorption rate of primary particles of conductive material (mL / 100 g): Plasticizer DBP (dibutyl phthalate) was mixed with the conductive material using an oil absorption measuring device (S-500, Asahi) to measure the torque change caused by the plasticizer impregnation, and the oil absorption when the viscosity represented by the torque value reached the maximum value was calculated as the DBP absorption value.
[0081] 4) Particle size (nm) of secondary particles of conductive material: measured by a wet method using a particle size analyzer (Mastersizer, Malvern).
[0082] 5) Porosity of particles (%): measured using a mercury porosimeter (Autopore, Micromeritics).
[0083] 6) Conductive material content in the first, second or third region of the particle (%): Using SEM, energy dispersive spectroscopy (EDS) measurement and image analysis program, calculate the content percentage of conductive material in a specific region in the cross section of the particle relative to the total conductive material.
[0084] 7) R value of the conductive material in the particles: calculated using the above formula 1 based on the results in 6) above.
[0085] 8) Electrical conductivity of particles (%): measured using a 4-probe powder conductivity measuring electrode (Powder Resistivity System (MCP-PD51), Mitsubishi Chemical Corporation), and calculated in % ratio based on Preparation Example 1.
[0086] Example: Preparation of electrodes and batteries comprising the prepared particles
[0087] Example 1
[0088] The particles prepared in Preparation Example 1 are applied to one surface of an aluminum current collector, rolled, impregnated with a sulfide electrolyte Li2S-P2S5, dried and rolled to provide a positive electrode having a thickness of about 130 μm (wherein the content of the sulfide electrolyte is about 20% by weight relative to the particles). Li2S-LiCl-P2S5 is mixed with a polyvinylidene fluoride (PVDF) solution (which is a solution of PVDF and toluene in a weight ratio of 8:92) to prepare a slurry, which is then applied to a lithium foil (Li foil) having a thickness of about 50 μm to prepare a solid electrolyte and a negative electrode containing it. The electrode assembly is prepared by stacking and pressing the positive and negative electrodes, which are then placed in a battery case to produce an all-solid-state battery.
[0089] Comparative Example 1
[0090] An all-solid-state battery was prepared in the same manner as in Example 1, except that, in the preparation of the positive electrode, the particles prepared in Comparative Preparation Example 1 were used instead of the particles prepared in Preparation Example 1.
[0091] Comparative Example 2
[0092] An all-solid-state battery was prepared in the same manner as in Example 1, except that the particles prepared in Comparative Preparation Example 2 were used instead of the particles prepared in Preparation Example 1 in the preparation of the positive electrode.
[0093] Comparative Example 3
[0094] An all-solid-state battery was prepared in the same manner as in Example 1, except that the particles prepared in Comparative Preparation Example 3 were used instead of the particles prepared in Preparation Example 1 in the preparation of the positive electrode.
[0095] Experimental Example: Evaluation of Preparation Examples and Examples
[0096] Experimental Example 1: SEM image of particles
[0097] The SEM images of each particle prepared in Preparation Example 1 and Comparative Preparation Example 1 were measured and shown in FIG. 1 (Preparation Example 1) and FIG. 2 (Comparative Preparation Example 1). Specifically, Figure 1a and 2a In the , the overall shape of the particles was identified by measuring at a magnification of ×1,000 and Figure 1b and 2b In the example, the distribution of the conductive material on the active material surface of the particle was identified by measuring at a magnification of ×5,000.
[0098] according to Figure 1a and 1b, the conductive material is distributed on the surface of the active material in a more defined particle form, so that each active material particle in the particle is clearly identifiable. On the other hand, according to Figure 2a and 2b , under corresponding magnification, the conductive material has very fine particles and covers the active material particles to such an extent that the surface of the active material is not visible, and the boundaries between the active material particles in the particles are not clear.
[0099] Experimental Example 2: Battery Performance Evaluation
[0100] The batteries of Example 1 and Comparative Examples 1 to 3 were each discharged at 0.1C and 1.0C to measure the discharge capacity ratio (1.0C discharge capacity / 0.1C discharge capacity×100%). The results are shown in Table 2 below.
[0101] [Table 2]
[0102] performance Example 1 Comparative Example 1 Comparative Example 2 Comparative Example 3 Discharge capacity ratio (%) 91 47 62 53
[0103] According to Tables 1 and 2, the particles of Preparation Example 1 have higher conductivity than the particles of Comparative Preparation Examples 1 to 3. In addition, compared with the batteries of Comparative Examples 1 to 3 respectively including electrodes prepared using the particles of Comparative Preparation Examples 1 to 3, the battery of Example 1 including the electrode prepared using the particles of Preparation Example 1 did not significantly deteriorate the performance of the battery even under higher C rate conditions.
[0104] All simple changes or modifications of the present invention fall within the scope of the present invention, and the specific protection scope of the present invention is set forth by the accompanying claims.
Claims
1. An electrode for an all-solid-state battery, comprising particles coated with a sulfide-based solid electrolyte, in, The particles include an active material, a conductive material and a binder, and The conductive material is carbon black having an average particle size of 120 nm to 200 nm.
2. The all-solid-state battery electrode according to claim 1, in, The BET specific surface area of the carbon black is 15 m 2 / g to 35m 2 / g.
3. The all-solid-state battery electrode according to claim 1, in, The carbon black has a DBP absorption rate of 70 mL / 100 g to 100 mL / 100 g.
4. The all-solid-state battery electrode according to claim 1, in, The carbon black is agglomerated to form secondary particles, and the particle diameter of the secondary particles is 600 nm to 1100 nm.
5. The all-solid-state battery electrode according to claim 1, in, The particles are spherical particles with a diameter of 30 μm to 150 μm.
6. The all-solid-state battery electrode according to claim 1, in, The porosity of the particles is between 20% and 40%.
7. The all-solid-state battery electrode according to claim 1, in, The electrode for the all-solid-state battery is a positive electrode, and the active material is selected from the group consisting of: LiCoO 2 , LiNiO 2 , LiMnO 2 , Li 2 MnO 3 , LiMn 2 O 4 , Li(Ni a Co b Mn c )O 2 (where 0 < a < 1, 0 < b < 1, 0 < c < 1, and a + b + c = 1), LiNi 1-y Co y O 2 (where 0 < y < 1), LiCo 1- y Mn y O 2 , LiNi 1-y Mn y O 2 (where 0 < y < 1), Li(Ni a Co b Mn c )O 4 (where 0 < a < 2, 0 < b < 2, 0 < c < 2, and a + b + c = 2), LiMn 2-z Ni z O 4 (where 0 < z < 2), LiMn 2-z Co z O 4 (where 0 < z < 2) and combinations thereof.
8. The all-solid-state battery electrode according to claim 1, in, The binder is an organic binder, and the organic binder is selected from the group consisting of polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone, polyimide, polyamideimide, polyethylene, polypropylene, ethylene-propylene-diene monomer (EPDM), sulfonated EPDM, styrene-butadiene rubber and fluororubber.
9. The all-solid-state battery electrode according to claim 1, in, The particles include 85 wt % to 99.8 wt % of the active material, 0.1 wt % to 10 wt % of the binder, and 0.1 wt % to 10 wt % of the conductive material.
10. The all-solid-state battery electrode according to claim 1, in, In the all-solid-state battery electrode, the electrode active material layer including the particles coated with the sulfide-based solid electrolyte has a thickness of 100 μm to 300 μm.
11. The all-solid-state battery electrode according to claim 1, in, In the all-solid-state battery electrode, the electrode active material layer including the particles coated with the sulfide-based solid electrolyte includes the sulfide-based solid electrolyte in an amount of 10 to 30% by weight based on the content of the particles.
12. The all-solid-state battery electrode according to claim 1, in, When the inner diameter of the particle is divided into equal intervals and into a first region, a second region, and a third region from the center of the particle to the outside of the particle, the content of the conductive material in the particle increases in the order of the first region, the second region, and the third region.
13. The all-solid-state battery electrode according to claim 12, in, The R value of the particles defined by Formula 1 is 5 or less: [Formula 1] Among them, r A is the content (%) of the conductive material in the first region, r B is the content (%) of the conductive material in the second region, r C is the content (%) of the conductive material in the third region, and the content of the conductive material in each region is based on the total content of the conductive material in the particle.
14. An all-solid-state battery, comprising the electrode for an all-solid-state battery according to claim 1 as a positive electrode or a negative electrode.