Electrolyte substrate for solid oxide fuel cell, single cell for solid oxide fuel cell, solid oxide fuel cell stack, and method for producing electrolyte substrate for solid oxide fuel cell

By forming a gap of 24% to 72% between the electrolyte layer and the barrier layer of the solid oxide fuel cell, the crack problem caused by thermal expansion difference or calcination shrinkage difference during sintering is solved, and the strength and reliability of the cell are improved. , improves the power generation characteristics.

CN118901154APending Publication Date: 2024-11-05MURATA MFG CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380028683.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-04
Filing Date
2023-03-27
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

In the existing solid oxide fuel cells, the electrolyte layer and the barrier layer crack due to thermal expansion difference or calcination shrinkage difference during the sintering process, which reduces the long-term reliability and power generation characteristics of the battery.

Method used

A gap of 24% to 72% is formed between the electrolyte layer and the barrier layer to alleviate the thermal expansion difference or the calcination shrinkage difference, and to reduce the generation of cracks by burning materials such as resin beads in the barrier layer.

Benefits of technology

The cracks between the electrolyte layer and the barrier layer are effectively suppressed, the strength of the electrolyte substrate and the long-term reliability of the battery are improved, the isolation function of the oxidant gas and fuel gas is maintained, and the power generation characteristics are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118901154A_ABST
    Figure CN118901154A_ABST
Patent Text Reader

Abstract

An electrolyte substrate (10) for a solid oxide fuel cell is provided with an electrolyte layer (20) comprising a sintered body of scandium oxide-stabilized zirconium oxide or yttrium oxide-stabilized zirconium oxide, and a barrier layer (30) provided on at least one main surface of the electrolyte layer (20) and comprising a sintered body of Ce (X) O2 (where X is any one of Sm, Gd, and Y). When the cross-section of the barrier layer (30) in the thickness direction is observed, voids (40) are present in the barrier layer (30) at an area ratio of 24-72%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an electrolyte substrate for a solid oxide fuel cell, a single cell for a solid oxide fuel cell, a solid oxide fuel cell stack, and a method for manufacturing an electrolyte substrate for a solid oxide fuel cell. Background Art

[0002] Solid oxide fuel cell (SOFC) is a fuel electrode: H2+O 2- →H2O+2e - 、Air electrode: (1 / 2)O2+2e - →O 2- A device that extracts electrical energy by reacting. A solid oxide fuel cell is a device that uses a stacked structure in which a plurality of single cells for a solid oxide fuel cell are stacked, each of which has a fuel electrode and an air electrode disposed on an electrolyte substrate for the solid oxide fuel cell.

[0003] Patent document 1 discloses a solid oxide fuel cell, characterized in that, in a solid oxide fuel cell having a fuel electrode and an air electrode arranged with an electrolyte membrane therebetween, an intermediate layer of Ce(X)O2 (wherein X is any one of Sm, Gd, and Y) is arranged between the above-mentioned electrolyte membrane of scandium oxide-stabilized zirconia and the above-mentioned air electrode of La(Ni)FeO3.

[0004] Furthermore, Patent Document 1 discloses a method for manufacturing a solid oxide fuel cell, which is characterized in that a fuel electrode is formed on one surface of an electrolyte membrane of scandium oxide-stabilized zirconia, a slurry of Ce(X)O2 (wherein X is any one of Sm, Gd, and Y) is coated on the other surface, an intermediate layer is formed by sintering, and then an air electrode of La(Ni)FeO3 is set. Patent Document 1 also discloses a method for manufacturing a solid oxide fuel cell, which is characterized in that a scandium oxide-stabilized zirconia electrolyte membrane is formed on a fuel electrode, sintered, and then a slurry of Ce(X)O2 (wherein X is any one of Sm, Gd, and Y) is coated on the above-mentioned electrolyte membrane, an intermediate layer is formed by sintering, and then an air electrode of La(Ni)FeO3 is set.

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent No. 3789380 Summary of the invention

[0008] According to Patent Document 1, by forming an intermediate layer such as Ce(Sm)O2 between the La(Ni)FeO3 air electrode and the zirconium oxide-based electrolyte, the reaction between La(Ni)FeO3 as the air electrode and the zirconium oxide in the electrolyte can be suppressed during electrode sintering, thereby improving battery performance.

[0009] However, in order to form an intermediate layer (hereinafter referred to as a barrier layer) as described in Patent Document 1, when the electrolyte layer and the barrier layer are co-sintered, or when the barrier layer is subsequently baked onto the sintered electrolyte layer, cracks may occur in the electrolyte layer or the barrier layer or both due to the difference in thermal expansion or calcination shrinkage between the materials. Moreover, when such cracks occur, problems such as reduced strength of the electrolyte layer, reduced long-term reliability (durability) of the battery cell after the electrode is formed, and reduced power generation characteristics due to reduced isolation function of the oxidant gas and the fuel gas occur.

[0010] The present invention is made to solve the above-mentioned problems, and its purpose is to provide an electrolyte substrate for a solid oxide fuel cell in which the difference in thermal expansion or calcination shrinkage between an electrolyte layer and a barrier layer is mitigated and crack generation is suppressed. In addition, the present invention aims to provide a single cell for a solid oxide fuel cell having the above-mentioned electrolyte substrate, a solid oxide fuel cell stack having a plurality of the above-mentioned single cells stacked therein, and a method for manufacturing the above-mentioned electrolyte substrate.

[0011] The electrolyte substrate for a solid oxide fuel cell of the present invention comprises: an electrolyte layer comprising a sintered body of scandium oxide-stabilized zirconia or yttria-stabilized zirconia, and a barrier layer comprising a sintered body of Ce(X)O2 (wherein X is any one of Sm, Gd and Y) arranged on at least one main surface of the above-mentioned electrolyte layer; when observing the cross-section of the above-mentioned barrier layer along the thickness direction, there are voids with an area ratio of 24% to 72% inside the above-mentioned barrier layer.

[0012] The single cell for the solid oxide fuel cell of the present invention comprises: an air electrode, a fuel electrode, and an electrolyte substrate of the present invention arranged between the above-mentioned air electrode and the above-mentioned fuel electrode; a barrier layer of the above-mentioned electrolyte substrate is arranged between the electrolyte layer of the above-mentioned electrolyte substrate and the above-mentioned air electrode.

[0013] The solid oxide fuel cell stack of the present invention is a stack of multiple battery units, each of which includes: a single cell of the present invention, a first connector disposed on the air electrode side of the single cell, and a second connector disposed on the fuel electrode side of the single cell.

[0014] The method for manufacturing an electrolyte substrate for a solid oxide fuel cell of the present invention comprises: a step of preparing an unsintered substrate, wherein an unsintered barrier layer comprising a powder of Ce(X)O2 (wherein X is any one of Sm, Gd and Y) and a burnt material is provided on at least one main surface of an unsintered electrolyte layer comprising a powder of scandia-stabilized zirconia or yttria-stabilized zirconia, or at least one main surface of an electrolyte layer comprising a sintered body of scandia-stabilized zirconia or yttria-stabilized zirconia, and a step of calcining the unsintered substrate at a temperature above the burnt temperature of the burnt material.

[0015] According to the present invention, it is possible to provide an electrolyte substrate for a solid oxide fuel cell in which the difference in thermal expansion or calcination shrinkage between an electrolyte layer and a barrier layer is mitigated and crack generation is suppressed. In addition, according to the present invention, it is possible to provide a single cell for a solid oxide fuel cell having the above electrolyte substrate, a solid oxide fuel cell stack having a plurality of the above single cells stacked therein, and a method for manufacturing the above electrolyte substrate. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 This is a cross-sectional view schematically showing an example of the electrolyte substrate for the solid oxide fuel cell of the present invention.

[0017] Figure 2 This is a cross-sectional view schematically showing another example of the electrolyte substrate for a solid oxide fuel cell according to the present invention.

[0018] Figure 3 This is a cross-sectional view schematically showing an example of a process for producing an electrolyte layer green sheet.

[0019] Figure 4 This is a cross-sectional view schematically showing an example of a process for producing a barrier layer green sheet.

[0020] Figure 5 This is a cross-sectional view schematically showing an example of a process for producing a green substrate.

[0021] Figure 6 This is a cross-sectional view schematically showing another example of the process of producing the green substrate.

[0022] Figure 7 This is a cross-sectional view schematically showing an example of a process of firing an unsintered substrate.

[0023] Figure 8 It is a cross-sectional view schematically showing another example of the process of calcining the green substrate.

[0024] Fig. 9This is a cross-sectional view schematically showing an example of a unit cell for a solid oxide fuel cell according to the present invention.

[0025] Fig.10 This is a cross-sectional view schematically showing another example of a unit cell for a solid oxide fuel cell according to the present invention.

[0026] Fig.11 This is an exploded perspective view schematically showing an example of a solid oxide fuel cell stack according to the present invention. DETAILED DESCRIPTION

[0027] Hereinafter, the electrolyte substrate for solid oxide fuel cells, the single cell for solid oxide fuel cells, the solid oxide fuel cell stack, and the method for manufacturing the electrolyte substrate for solid oxide fuel cells of the present invention are described. It should be noted that the present invention is not limited to the following configurations, and can be appropriately changed and applied within the scope of not changing the gist of the present invention. In addition, a technical solution formed by combining two or more of the preferred configurations of the present invention described below is also the present invention.

[0028] The drawings shown below are schematic diagrams, and their dimensions, aspect ratios, and other aspects may differ from those of actual products.

[0029] [Electrolyte substrate for solid oxide fuel cells]

[0030] The electrolyte substrate for a solid oxide fuel cell of the present invention comprises: an electrolyte layer comprising a sintered body of scandium oxide-stabilized zirconia or yttria-stabilized zirconia, and a barrier layer comprising a sintered body of Ce(X)O2 (wherein X is any one of Sm, Gd and Y) arranged on at least one main surface of the above-mentioned electrolyte layer; when observing the cross-section of the above-mentioned barrier layer along the thickness direction, there are voids with an area ratio of 24% to 72% inside the above-mentioned barrier layer.

[0031] Figure 1 This is a cross-sectional view schematically showing an example of the electrolyte substrate for the solid oxide fuel cell of the present invention.

[0032] Figure 1 The electrolyte substrate 10 for a solid oxide fuel cell shown includes an electrolyte layer 20 and barrier layers 30 provided on both main surfaces of the electrolyte layer 20 .

[0033] Figure 2 This is a cross-sectional view schematically showing another example of the electrolyte substrate for a solid oxide fuel cell according to the present invention.

[0034] Figure 2The electrolyte substrate 10A for a solid oxide fuel cell shown includes an electrolyte layer 20 and a barrier layer 30 provided on one main surface of the electrolyte layer 20 .

[0035] The electrolyte layer 20 includes a sintered body of scandia-stabilized zirconia or yttria-stabilized zirconia.

[0036] Examples of scandia-stabilized zirconia include Zr(Sc)O 2 and Zr(Sc,M)O 2 (wherein M is any one of Al 2 O 3 , CeO 2 and Y 2 O 3 ).

[0037] Examples of yttria-stabilized zirconia include Zr(Y)O 2 and the like.

[0038] The barrier layer 30 includes a sintered body of Ce(X)O2 (where X is any one of Sm, Gd and Y). The barrier layer 30 provided on each main surface of the electrolyte layer 20 may be two or more layers, and preferably one layer.

[0039] The barrier layer 30 has the same function as the intermediate layer described in Patent Document 1 as that of inhibiting the electrolyte layer 20 and the air electrode 50 (see the following description). Fig. 9 and Fig.10 )'s reaction function.

[0040] like Figure 1 and Figure 2 As shown, there are voids 40 within the barrier layer 30 .

[0041] By forming the voids 40 inside the barrier layer 30 , the difference in thermal expansion or the difference in shrinkage during firing between the electrolyte layer 20 and the barrier layer 30 is alleviated, and the occurrence of cracks can be suppressed.

[0042] On the other hand, when voids are formed inside the electrolyte layer 20 , if the voids are connected to each other and penetrate the electrolyte layer 20 , the isolation function of the oxidant gas and the fuel gas is lost, thereby causing a decrease in power generation characteristics. Therefore, it is preferable to form voids 40 inside the barrier layer 30 .

[0043] Regarding the relaxation of the firing shrinkage difference, when the shrinkage of the electrolyte layer 20 is greater than the shrinkage of the barrier layer 30 , it is effective to form the voids 40 inside the barrier layer 30 .

[0044] Regarding the relaxation of the thermal expansion difference, when the thermal expansion coefficient of the electrolyte layer 20 is smaller than the thermal expansion coefficient of the barrier layer 30 , it is effective to form the voids 40 inside the barrier layer 30 .

[0045] Furthermore, as shown in the examples described later, it was found that the more voids 40 there were in the barrier layer 30, the higher the substrate strength was. This is presumably due to the effect of reducing residual stress (i.e., tensile stress applied to the surface of the barrier layer 30) due to the relaxation of thermal expansion differences during calcination, and the effect of preventing cracks from developing even when cracks were generated by the voids 40.

[0046] On the other hand, if there are too many voids 40 inside the barrier layer 30, the barrier layer 30 is easily separated from the electrolyte layer 20. This is considered to be because the bonding area between the electrolyte layer 20 and the barrier layer 30 is reduced and the strength of the barrier layer 30 itself is also reduced.

[0047] For the above reasons, when observing the cross section of the barrier layer 30 along the thickness direction, preferably 24% to 72% of the voids 40 are present in the barrier layer 30. In other words, the void area ratio in the barrier layer 30 is preferably 24% to 72%.

[0048] The thickness of the barrier layer 30 is not particularly limited, and may be the same as the thickness of the electrolyte layer 20, may be greater than the thickness of the electrolyte layer 20, or may be less than the thickness of the electrolyte layer 20. Since the higher the ratio of the thickness of the barrier layer 30 to the thickness of the electrolyte layer 20, the easier it is to generate cracks, the effect of the voids 40 can be exerted. On the other hand, the higher the ratio of the thickness of the barrier layer 30 to the thickness of the electrolyte layer 20, the easier it is to reduce the power generation characteristics. Therefore, from the viewpoint of ensuring the power generation characteristics, it is preferred that the ratio of the thickness of the barrier layer 30 to the thickness of the electrolyte layer 20 is 20% or less. On the other hand, from the viewpoint of exerting the strength of the barrier layer 30 itself, the adhesion between the barrier layer 30 and the electrolyte layer 20, and the function of the barrier layer 30, the ratio of the thickness of the barrier layer 30 to the thickness of the electrolyte layer 20 may be, for example, 1% or more, preferably 5% or more, and more preferably 10% or more.

[0049] For example, the thickness of the barrier layer 30 is preferably 20 μm or less. On the other hand, the thickness of the barrier layer 30 may be 1 μm or more, preferably 5 μm or more, and more preferably 10 μm or more. When the thickness of the barrier layer 30 is within the above range, the thickness of the electrolyte layer 20 is preferably 80 μm to 120 μm. In addition, when the thickness of the barrier layer 30 is within the above range, the ratio of the thickness of the barrier layer 30 to the thickness of the electrolyte layer 20 is preferably within the above range.

[0050] It should be explained, such as Figure 1 As shown, in the case where the two main surfaces of the electrolyte layer 20 are provided with the barrier layer 30, and as shown in Figure 2As shown, when the barrier layer 30 is provided on one main surface of the electrolyte layer 20, in any case, the thickness of the barrier layer 30 refers to the thickness of the barrier layer 30 provided on each main surface of the electrolyte layer 20 (the thickness of one layer).

[0051] In addition, the shape, size, etc. of the gaps 40 are not particularly limited. The shapes of the gaps 40 may be the same or different. Similarly, the sizes of the gaps 40 may be the same or different.

[0052] For example, some of the gaps 40 may be connected to each other. If the gaps 40 are connected to each other and penetrate the barrier layer 30, it is possible that the electrolyte layer 20 and the air electrode 50 (see below) are connected. Fig. 9 and Fig.10 ) reacts, and in addition, when cracks are generated, it is difficult to fully obtain the effect of preventing crack growth by the voids 40. Therefore, it is preferred that the voids 40 are not connected from one main surface opposite to the other main surface in the thickness direction of the barrier layer 30.

[0053] The voids 40 are preferably uniformly dispersed in the barrier layer 30. That is, the voids 40 are preferably not concentrated in the barrier layer 30.

[0054] like Figure 1 As shown in FIG. 1 , when the barrier layer 30 is provided on both main surfaces of the electrolyte layer 20, it is preferred that the thickness, void area ratio, etc. of the barrier layer 30 are the same. The so-called "same" here may not be strictly the same, as long as it falls within a range of about 3%. By providing the barrier layer 30 symmetrically with respect to the electrolyte layer 20, warping during sintering can be suppressed.

[0055] In addition, the shape, size, thickness, etc. of the electrolyte substrates 10 and 10A are not particularly limited.

[0056] [Method for producing electrolyte substrate for solid oxide fuel cell]

[0057] The method for manufacturing an electrolyte substrate for a solid oxide fuel cell of the present invention comprises: a step of preparing an unsintered substrate, wherein an unsintered barrier layer comprising a powder of Ce(X)O2 (wherein X is any one of Sm, Gd and Y) and a burnt material is provided on at least one main surface of an unsintered electrolyte layer comprising a powder of scandia-stabilized zirconia or yttria-stabilized zirconia, or at least one main surface of an electrolyte layer comprising a sintered body of scandia-stabilized zirconia or yttria-stabilized zirconia, and a step of calcining the unsintered substrate at a temperature above the burnt temperature of the burnt material.

[0058] In the step of preparing the unsintered substrate, an unsintered substrate may be prepared in which an unsintered barrier layer including a powder of Ce(X)O2 (where X is any one of Sm, Gd and Y) and a burnt material is provided on at least one main surface of an unsintered electrolyte layer including a powder of scandia-stabilized zirconia or yttria-stabilized zirconia. In this case, the barrier layer is formed by co-sintering with the electrolyte layer.

[0059] Examples of methods for forming an unsintered electrolyte layer include a method of preparing a green sheet for an electrolyte layer and a method of applying a paste for an electrolyte layer. Examples of methods for forming an unsintered barrier layer include a method of preparing a green sheet for a barrier layer and a method of applying a paste for a barrier layer.

[0060] For example, the process of preparing an unsintered substrate includes: a process of preparing an unfired electrolyte layer raw sheet comprising a powder of scandium oxide-stabilized zirconia or yttria-stabilized zirconia, a process of preparing an unfired barrier layer raw sheet comprising a powder of Ce(X)O2 (wherein X is any one of Sm, Gd and Y) and a burnt material, and a process of stacking the above-mentioned electrolyte layer raw sheets and the above-mentioned barrier layer raw sheets.

[0061] Alternatively, in the step of preparing the unsintered substrate, an unsintered substrate may be prepared in which an unsintered barrier layer including a powder of Ce(X)O2 (where X is any one of Sm, Gd and Y) and a burnt material is provided on at least one main surface of an electrolyte layer including a sintered body of scandia-stabilized zirconia or yttria-stabilized zirconia. In this case, the barrier layer is formed by baking onto the sintered electrolyte layer.

[0062] In the method for producing the electrolyte substrate of the present invention, voids are intentionally formed inside the barrier layer. Specifically, the voids are formed by pre-incorporating a burnt material (a material that burns during firing) into the barrier layer green sheet or the barrier layer paste.

[0063] As the burnout material, for example, resin beads, carbon, binders, and other organic substances can be cited. The burnout material can be only one kind or two or more kinds. Among them, the preferred burnout material is resin beads. By using resin beads as the burnout material, the shape of the gap can be easily adjusted.

[0064] Hereinafter, referring to the accompanying drawings Figure 1 The electrolyte substrate 10 or Figure 2 An example of a method for manufacturing the electrolyte substrate 10A shown will be described according to each step.

[0065] Figure 3 This is a cross-sectional view schematically showing an example of a process for producing an electrolyte layer green sheet.

[0066] For example, the unfired electrolyte layer green sheet 2s is produced by molding the electrolyte layer ceramic slurry. The electrolyte layer green sheet 2s contains a powder 5 of scandia-stabilized zirconia or yttria-stabilized zirconia.

[0067] The ceramic slurry for the electrolyte layer can be prepared, for example, by mixing powder of scandia-stabilized zirconia or yttria-stabilized zirconia, a binder, a dispersant, an organic solvent, and the like.

[0068] Figure 4 This is a cross-sectional view schematically showing an example of a process for producing a barrier layer green sheet.

[0069] For example, the unfired barrier layer green sheet 3 s is produced by molding a barrier layer ceramic slurry. The barrier layer green sheet 3 s contains a powder 6 of Ce(X)O 2 (where X is any one of Sm, Gd, and Y) and a burnt material 4 .

[0070] The ceramic slurry for the barrier layer can be prepared, for example, by mixing powder of Ce(X)O2 (wherein X is any one of Sm, Gd and Y), a burnt material, a binder, a dispersant, an organic solvent and the like.

[0071] Figure 5 This is a cross-sectional view schematically showing an example of a process for producing a green substrate.

[0072] like Figure 5 As shown, the unsintered substrate 1 is produced by laminating the electrolyte layer green sheets 2s and the barrier layer green sheets 3s. Figure 5 In the green substrate 1 shown, green barrier layers 3 are provided on both main surfaces of the green electrolyte layer 2 .

[0073] exist Figure 5In the example shown, the unsintered substrate 1 is produced by sequentially stacking one barrier layer green sheet 3s, three electrolyte layer green sheets 2s, and one barrier layer green sheet 3s. The number of the electrolyte layer green sheets 2s contained in the unsintered electrolyte layer 2 is not particularly limited, and may be one, or may be two or more. In addition, the number of the barrier layer green sheets 3s contained in the unsintered barrier layer 3 disposed on one main surface of the unsintered electrolyte layer 2 is not particularly limited, and may be one, or may be two or more. The number of the barrier layer green sheets 3s contained in the unsintered barrier layer 3 disposed on one main surface of the unsintered electrolyte layer 2 may be the same as, more, or less than, the number of the electrolyte layer green sheets 2s contained in the unsintered electrolyte layer 2. Similarly, the number of barrier layer green sheets 3s included in the unsintered barrier layer 3 provided on the other main surface of the unsintered electrolyte layer 2 is not particularly limited, and may be 1 sheet or may be 2 or more sheets. The number of barrier layer green sheets 3s included in the unsintered barrier layer 3 provided on the other main surface of the unsintered electrolyte layer 2 may be the same as the number of electrolyte layer green sheets 2s included in the unsintered electrolyte layer 2, or may be more or less than the number. In addition, the number of barrier layer green sheets 3s included in the unsintered barrier layer 3 provided on the other main surface of the unsintered electrolyte layer 2 may be the same as the number of barrier layer green sheets 3s included in the unsintered barrier layer 3 provided on one main surface of the unsintered electrolyte layer 2, or may be more or less than the number.

[0074] Figure 6 This is a cross-sectional view schematically showing another example of the process of producing the green substrate.

[0075] like Figure 6 As shown, the unsintered substrate 1A can be produced by laminating the electrolyte layer green sheets 2s and the barrier layer green sheets 3s. Figure 6 In the green substrate 1A shown, the green barrier layer 3 is provided on one main surface of the green electrolyte layer 2 .

[0076] exist Figure 6 In the example shown, the unsintered substrate 1A is manufactured by sequentially stacking one barrier layer green sheet 3s and three electrolyte layer green sheets 2s. The number of the electrolyte layer green sheets 2s included in the unsintered electrolyte layer 2 is not particularly limited, and may be one, or may be two or more. In addition, the number of the barrier layer green sheets 3s included in the unsintered barrier layer 3 provided on one main surface of the unsintered electrolyte layer 2 is not particularly limited, and may be one, or may be two or more.

[0077] When forming the unsintered electrolyte layer 2, the thickness of the unsintered electrolyte layer 2 can be easily controlled by stacking a plurality of electrolyte layer green sheets 2s. Similarly, when forming the unsintered barrier layer 3, the thickness of the unsintered barrier layer 3 can be easily controlled by stacking a plurality of barrier layer green sheets 3s.

[0078] When the unsintered substrate 1 or 1A is produced, the electrolyte layer green sheet 2s and the barrier layer green sheet 3s may be laminated and then pressure-bonded.

[0079] Figure 7 This is a cross-sectional view schematically showing an example of a process of firing an unsintered substrate.

[0080] By Figure 5 The unsintered substrate 1 shown is calcined at a temperature above the temperature at which the burnt material 4 burns, so that the unsintered substrate 1 is sintered to form the electrolyte layer 20 and the barrier layer 30, and the burnt material 4 is burned to form the void 40 inside the barrier layer 30. As a result, the Figure 7 The electrolyte substrate 10 is shown.

[0081] Figure 8 It is a cross-sectional view schematically showing another example of the process of calcining the green substrate.

[0082] By Figure 6 The unsintered substrate 1A shown is calcined at a temperature higher than the temperature at which the burnout material 4 burns, so that the unsintered substrate 1A is sintered to form the electrolyte layer 20 and the barrier layer 30, and the burnout material 4 is burned to form the void 40 inside the barrier layer 30. As a result, the Figure 8 The electrolyte substrate 10A is shown.

[0083] [Single cell for solid oxide fuel cell]

[0084] The unit cell for a solid oxide fuel cell of the present invention comprises an air electrode, a fuel electrode, and the electrolyte substrate of the present invention disposed between the air electrode and the fuel electrode.

[0085] In the single cell for solid oxide fuel cell of the present invention, the barrier layer of the electrolyte substrate is disposed between the electrolyte layer of the electrolyte substrate and the air electrode. Therefore, the reaction between the electrolyte layer and the air electrode can be suppressed by the barrier layer.

[0086] Fig. 9 This is a cross-sectional view schematically showing an example of a unit cell for a solid oxide fuel cell according to the present invention.

[0087] Fig. 9The solid oxide fuel cell unit cell 100 shown in the figure comprises an air electrode 50, a fuel electrode 60, and an electrolyte substrate 10 (see FIG. 1 ) disposed between the air electrode 50 and the fuel electrode 60. Figure 1 ).

[0088] The electrolyte substrate 10 is Figure 1 As described in the above, the electrolyte layer 20 and the barrier layer 30 provided on both main surfaces of the electrolyte layer 20 are provided. The barrier layer 30 has voids 40 inside.

[0089] Fig.10 This is a cross-sectional view schematically showing another example of a unit cell for a solid oxide fuel cell according to the present invention.

[0090] Fig.10 The solid oxide fuel cell unit 100A shown in the figure comprises an air electrode 50, a fuel electrode 60, and an electrolyte substrate 10A disposed between the air electrode 50 and the fuel electrode 60 (see Figure 2 ).

[0091] The electrolyte substrate 10A is Figure 2 As described in , the present invention comprises an electrolyte layer 20 and a barrier layer 30 provided on one main surface of the electrolyte layer 20. The barrier layer 30 has voids 40 therein.

[0092] like Fig. 9 and Fig.10 As shown, the barrier layer 30 of the electrolyte substrate 10 is arranged between the electrolyte layer 20 of the electrolyte substrate 10 and the air electrode 50 .

[0093] As the air electrode 50, a known air electrode for solid oxide fuel cells can be used. As the material of the air electrode 50, for example, La(Ni)FeO3, (La, Sr)CoO3, (La, Sr)FeO3, (La, Sr)(Co, Fe)O3, etc. can be cited. In the case where the barrier layer 30 is not provided between the electrolyte layer 20 and the air electrode 50, if heat treatment is performed at a high temperature, the air electrode 50 reacts with the electrolyte layer 20 to generate an insulating layer such as SrZrO3, La2Zr2O7, etc.

[0094] The air electrode 50 may be provided on the entire main surface of one of the electrolyte substrates 10 or 10A, or may be provided on a portion thereof.

[0095] A known fuel electrode for solid oxide fuel cells can be used as the fuel electrode 60. Examples of the material of the fuel electrode 60 include Ni, Ni / ScSZ (scandia stabilized zirconia) cermet, Ni / YSZ (yttria stabilized zirconia) cermet, and Ni / CeO2 cermet.

[0096] The fuel electrode 60 may be provided on the entire other main surface of the electrolyte substrate 10 or 10A, or may be provided on a portion thereof.

[0097] The unit cell for the solid oxide fuel cell of the present invention can be produced by forming an air electrode on one main surface of the electrolyte substrate for the solid oxide fuel cell of the present invention and forming a fuel electrode on the other main surface.

[0098] First, a binder and a solvent are added to the powder of the material constituting the air electrode, and a dispersant is further added as needed to prepare a slurry for the air electrode. In addition, a binder and a solvent are added to the powder of the material constituting the fuel electrode, and a dispersant is further added as needed to prepare a slurry for the fuel electrode. The slurry for the air electrode is applied to one main surface of the electrolyte substrate with a specified thickness, and the slurry for the fuel electrode is applied to the other main surface of the electrolyte substrate, and the coating is dried to form green layers for the air electrode and the fuel electrode. The air electrode and the fuel electrode are formed by calcining the green layers for the air electrode and the fuel electrode. The calcination conditions such as the calcination temperature can be appropriately determined according to the types of materials of the air electrode and the fuel electrode.

[0099] When the single cell of the present invention is assembled in a solid oxide fuel cell, an oxidant gas flow path for supplying an oxidant gas such as air or oxygen to the air electrode and a fuel gas flow path for supplying a fuel gas such as hydrogen, carbon monoxide or hydrocarbon gas to the fuel electrode are required. A solid oxide fuel cell stack formed by stacking a plurality of battery cells in which an oxidant gas flow path and a fuel gas flow path are provided in the single cell of the present invention and a conductive path is further provided.

[0100] [Solid oxide fuel cell stack]

[0101] The solid oxide fuel cell stack of the present invention is formed by stacking a plurality of battery units including the single cell of the present invention, a first connector disposed on the air electrode side of the single cell, and a second connector disposed on the fuel electrode side of the single cell.

[0102] In the solid oxide fuel cell stack of the present invention, a plurality of cells are stacked with a connector (also called a separator) therebetween. That is, each of the plurality of cells has a structure sandwiched by a pair of connectors. The connector has the function of electrically connecting the plurality of cells and supplying gas to each electrode.

[0103] Fig.11 This is an exploded perspective view schematically showing an example of a solid oxide fuel cell stack according to the present invention.

[0104] Fig.11 In the solid oxide fuel cell stack 200 shown in FIG. Fig. 9 ), the first connector 210 disposed on the air electrode 50 side of the single cell 100 and the second connector 220 disposed on the fuel electrode 60 side of the single cell 100 are stacked in two layers in the Z direction. The number of stacked battery cells 110 is not particularly limited. In the solid oxide fuel cell stack 200, only Fig. 9 The single cell 100 shown may also be stacked Fig.10 The single cell 100A shown can also be stacked Fig. 9 The single cell 100 and Fig.10 Both of the single cells 100A are shown.

[0105] The solid oxide fuel cell stack 200 is provided with an oxidant gas manifold 230 and a fuel gas manifold 240 as through holes. The oxidant gas manifold 230 extends in the X direction, and the fuel gas manifold 240 extends in the Y direction.

[0106] An oxidizing gas flow path 250 is provided on the main surface of the first connecting body 210 facing the air electrode 50. The oxidizing gas flow path 250 extends in the Y direction.

[0107] A fuel gas flow path 260 is provided on the main surface of the second connecting body 220 that faces the fuel electrode 60. The fuel gas flow path 260 extends in the X direction.

[0108] The constituent materials of the first connection body 210 and the second connection body 220 may be insulating materials such as ceramic materials, or conductive materials such as metal materials.

[0109] The constituent materials of the first connecting body 210 and the second connecting body 220 may be the same or different from each other.

[0110] When the constituent material of the first connecting body 210 and the second connecting body 220 is an insulating material, examples of the first connecting body 210 and the second connecting body 220 include a sintered body of partially stabilized zirconia.

[0111] When the first connector 210 is made of an insulating material, it is preferred that at least one through conductor is provided in the first connector 210, which penetrates in the thickness direction and is connected to the air electrode 50 and is exposed on the main surface opposite to the air electrode 50. In this case, the air electrode 50 can be led out of the first connector 210 via the through conductor.

[0112] When the second connector 220 is made of an insulating material, it is preferred that at least one through conductor is provided in the second connector 220, which penetrates in the thickness direction and is connected to the fuel electrode 60 and is exposed on the main surface opposite to the fuel electrode 60. In this case, the fuel electrode 60 can be led out of the second connector 220 via the through conductor.

[0113] The constituent material of the through conductors provided in the first connecting body 210 and the second connecting body 220 is preferably an alloy of silver and palladium, or platinum.

[0114] The constituent material of the through conductor provided in the first connecting body 210 and the constituent material of the through conductor provided in the second connecting body 220 may be the same as or different from each other.

[0115] Example

[0116] Hereinafter, examples will be described which more specifically disclose the electrolyte substrate for a solid oxide fuel cell of the present invention, but it should be noted that the present invention is not limited to these examples.

[0117] [Preparation of Green Sheet for Electrolyte Layer]

[0118] After mixing powder of scandium oxide stabilized zirconium oxide, i.e., Zr(Sc)O2 (hereinafter referred to as ScSZ), a dispersant, a polyvinyl butyral binder, a plasticizer, and a toluene / ethanol solvent to prepare a slurry, the viscosity is adjusted by degassing under reduced pressure. The slurry is applied to a carrier film by a doctor blade method and dried to prepare a green sheet for an electrolyte layer.

[0119] [Production of Green Sheet for Barrier Layer]

[0120] Ce(Sm)O2 (hereinafter referred to as SDC) powder and void-forming resin beads (burning material) are mixed at a predetermined ratio, and a dispersant, a polyvinyl butyral-based binder, a plasticizer, and a toluene / ethanol-based solvent are added and mixed to prepare a slurry, and then the viscosity is adjusted by degassing under reduced pressure. The slurry is applied to a carrier film by a doctor blade method and dried to prepare a green sheet for a barrier layer.

[0121] [Fabrication of Electrolyte Substrate]

[0122] After stacking the green sheets in the order of SDC / ScSZ / SDC, isostatic pressing was performed at 100 MPa and cut into a specified size to obtain a pressed body of the green sheets (unsintered substrate). Then, a batch calcining furnace was used to burn the organic components and sintered at a furnace top temperature of 1350°C to obtain an electrolyte substrate of size 50 mm × 40 mm.

[0123] [Cross-sectional observation of electrolyte substrate]

[0124] The obtained electrolyte substrate of size 50mm×40mm was cut into single pieces of 5mm square size by a grinder, and then fixed with a thermosetting resin to make a grinding sample. The grinding sample was finally ground with 3μm diamond slurry to expose the smooth substrate cross section. Using a scanning electron microscope (SEM) with a magnification of 2000 times, 5 fields of view were randomly selected at the position where the interface between the entire surface of the thickness direction of the barrier layer (SDC layer) and the electrolyte layer (ScSZ layer) can be seen to confirm the presence or absence of cracks and take reflected electron images.

[0125] When a crack was confirmed at one location in each of the electrolyte layer (ScSZ layer) and the barrier layer (SDC layer) within the observation field, it was determined that “cracks were present”.

[0126] In addition, the thickness of the electrolyte layer (ScSZ layer) and the barrier layer (SDC layer) were measured based on the reduced scale of the image. The results are shown in Tables 1 and 2. It should be noted that the thickness of the barrier layer shown in Table 2 is the thickness of a single barrier layer provided on one main surface of the electrolyte layer.

[0127] [Measurement of void area ratio]

[0128] The reflected electron image presented above was imported into the image analysis software (WinROOF2018) for analysis. The steps are shown below.

[0129] (1) Convert a color image to a gray image.

[0130] (2) The grayscale image density detection threshold is determined so that a gap can be distinguished from other portions, and a portion below (above) the set threshold is detected.

[0131] (3) The void area ratio is calculated according to the following formula based on the total void area and the total area of ​​the barrier layer.

[0132] Void area ratio (%) = 100 × total void area / total barrier layer area

[0133] [Measurement of three-point bending strength]

[0134] The three-point bending test of the electrolyte substrate was performed using Autograph (AGS-5KNX).

[0135] The test conditions are shown below.

[0136] Distance between pivot points: 20mm

[0137] Test speed: 5mm / min

[0138] The maximum load until the electrolyte substrate breaks was measured, and the three-point bending strength was calculated according to the following calculation formula.

[0139] σ=3PL / (2bH 2 )

[0140] Here, σ: three-point bending strength, P: maximum load, L: distance between supporting points, b: sample width, h: sample thickness. The number of measurements is 10, and the average value of the three-point bending strength is calculated.

[0141] The evaluation results of the samples are shown in Tables 1 and 2. In addition, Table 2 shows the relative values ​​of the three-point bending strength when the three-point bending strength of Sample No. 2 is set to 1.00.

[0142] [Table 1]

[0143]

[0144] [Table 2]

[0145]

[0146] In Table 1 and Table 2, samples marked with * are comparative examples outside the scope of the present invention.

[0147] Table 1 shows that cracks are more likely to occur when the thickness of the barrier layer is thicker, given the same void area ratio in the barrier layer. This is believed to be because the thicker the barrier layer, the greater the effect of the thermal expansion or contraction difference between the electrolyte layer and the barrier layer during calcination.

[0148] According to Table 2, when the void area ratio in the barrier layer is 24% or more, no cracks are observed in both the electrolyte layer and the barrier layer. On the other hand, when the void area ratio in the barrier layer is less than 24%, it is considered that the thermal expansion difference or contraction difference between the electrolyte layer and the barrier layer generated during calcination is not sufficiently alleviated.

[0149] From Table 2, it was confirmed that, when the thickness of the barrier layer was the same, the three-point bending strength increased as the void area ratio in the barrier layer increased. This is believed to be due to the effect of reducing the residual stress (i.e., the tensile stress applied to the surface of the barrier layer) caused by the relaxation of the thermal expansion difference during calcination, and the effect of preventing the crack from developing even if cracks occurred due to the voids.

[0150] According to Table 2, it was confirmed that when the void area ratio in the barrier layer was 77%, the barrier layer was separated from the electrolyte layer and powdered due to the friction between the substrates generated during normal operation. It is believed that this is because in addition to the reduction in the bonding area between the barrier layer and the electrolyte layer, the strength of the barrier layer itself is also reduced. If this phenomenon occurs before the air electrode is formed, the effect of suppressing the reaction between the air electrode and the electrolyte layer is reduced. In addition, when this phenomenon occurs after the air electrode is formed, the battery characteristics are reduced due to the reduction in the reaction field.

[0151] Based on the above results, it is considered that the void area ratio in the barrier layer is appropriately in the range of 24% to 72%.

[0152] Explanation of symbols

[0153] 1. 1A unsintered substrate

[0154] 2 Unsintered electrolyte layer

[0155] 2s electrolyte layer green sheet

[0156] 3 Unsintered barrier layer

[0157] 3s barrier layer green sheet

[0158] 4 Burning materials

[0159] 5 Scandium oxide stabilized zirconia or yttria stabilized zirconia powder

[0160] 6Ce(X)O2 powder

[0161] 10.10A Electrolyte substrate for solid oxide fuel cells

[0162] 20 electrolyte layer

[0163] 30 barrier layers

[0164] 40 gaps

[0165] 50 air electrode

[0166] 60 fuel electrode

[0167] 100, 100A single cell for solid oxide fuel cells

[0168] 110 battery cells

[0169] 200 solid oxide fuel cell stack

[0170] 210 1st connector

[0171] 220 Second Connector

[0172] 230 Oxidizer Gas Manifold

[0173] 240 fuel gas manifold

[0174] 250 Oxidant gas flow path

[0175] 260 fuel gas flow path

Claims

1. An electrolyte substrate for a solid oxide fuel cell, comprising: an electrolyte layer comprising a sintered body of scandia-stabilized zirconia or yttria-stabilized zirconia, and The barrier layer is disposed on at least one main surface of the electrolyte layer and comprises Ce(X)O 2 The sintered body in, X is any one of Sm, Gd and Y; When the cross section of the barrier layer along the thickness direction is observed, voids are present in the barrier layer at an area ratio of 24% to 72%.

2. The electrolyte substrate according to claim 1, in, A ratio of the thickness of the barrier layer to the thickness of the electrolyte layer is 20% or less.

3. The electrolyte substrate according to claim 1 or 2, in, The thickness of the barrier layer is less than 20 μm.

4. A single cell for a solid oxide fuel cell, comprising: an air electrode, a fuel electrode, and the electrolyte substrate according to any one of claims 1 to 3 disposed between the air electrode and the fuel electrode, A barrier layer of the electrolyte substrate is arranged between the electrolyte layer of the electrolyte substrate and the air electrode.

5. A solid oxide fuel cell stack comprising a plurality of stacked battery units, the battery unit comprising the single cell according to claim 4, a first connector disposed on the air electrode side of the single cell, and a second connector disposed on the fuel electrode side of the single cell.

6. A method for manufacturing an electrolyte substrate for a solid oxide fuel cell, comprising: The step of preparing an unsintered substrate, wherein the unsintered substrate has a Ce(X)O layer on at least one main surface of an unsintered electrolyte layer comprising a powder of scandia-stabilized zirconia or yttria-stabilized zirconia, or on at least one main surface of an electrolyte layer comprising a sintered body of scandia-stabilized zirconia or yttria-stabilized zirconia. 2 of powder and unsintered barrier layer of burnt material, in, X is any one of Sm, Gd and Y, and The step of calcining the green substrate at a temperature higher than the temperature at which the burnt material is burnt.

7. The method for producing an electrolyte substrate according to claim 6, in, The process of making the unsintered substrate comprises: a step of preparing an unfired electrolyte layer green sheet containing a powder of scandia-stabilized zirconia or yttria-stabilized zirconia, Production of Ce(X)O 2 and a process for preparing an unfired barrier layer green sheet of the powder and the burned material, wherein X is any one of Sm, Gd and Y, and A step of laminating the electrolyte layer green sheet and the barrier layer green sheet.