Hydrogel-coated oxygenation membrane and preparation method thereof

By coating the hydrogel layer on the surface of the oxygenated film, the problems of high threshold and poor coating effect in the existing oxygenated film modification process are solved, and efficient blood gas exchange and excellent anti-plasma leakage and blood Compatibility.

CN118904089AActive Publication Date: 2024-11-08TIANJIN UNIV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411022884.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-08
Estimated Expiration
2044-07-29

AI Technical Summary

Technical Problem

During the modification process, the existing oxygenated film has high thresholds and insufficient coating effect, which leads to poor anti-plasma leakage performance and blood compatibility, and is prone to problems such as coating blocking holes and hindering gas exchange.

Method used

By using the hydrogel coating method, by adding a modified substance and a diluent to the polyolefin, a 0.5-3 μm thick hydrogel layer is coated on the surface of the film by spin coating or dip coating, and the film body and hydrocoagulation are strengthened. The interaction of the glue layer forms a double-layer structure of loose microporous layer and dense non-porous layer, promoting gas exchange.

Benefits of technology

It significantly improves the anti-plasma leakage performance and hemocompatibility of the oxygenated membrane, enhances gas permeability, prolongs the anti-plasma leakage time, reduces protein adhesion and hemolysis rate, and improves the overall performance of the membrane.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118904089A_ABST
    Figure CN118904089A_ABST
Patent Text Reader

Abstract

The invention relates to a hydrogel coated oxygenation membrane and a preparation method thereof. Adding polyolefin resin and a modified substance into the diluent, and heating and stirring to obtain a membrane casting solution; taking the membrane casting solution as a raw material, and performing membrane scraping or spinning by using a thermally induced phase separation method to obtain a flat membrane or a hollow fiber membrane; irradiating the hydrogel solution under ultraviolet light to enable the hydrogel solution to reach a semi-cured state, so as to obtain a pre-polymerized hydrogel solution; coating a flat sheet membrane or a hollow fiber membrane with the obtained pre-polymerized hydrogel solution; then irradiating the membrane coated with the pre-polymerized hydrogel solution under ultraviolet light to enable the hydrogel solution to be completely cured; and drying at room temperature to obtain the oxygenation membrane coated with the hydrogel, wherein the thickness of the hydrogel layer is 0.5-3 microns. The hydrogel-coated oxygenation membrane is used as a blood-gas exchange medium in an extracorporeal membrane lung oxygenation process; the anti-plasma leakage time is 180-560h, the protein adhesion amount is 0.3-1.1 [mu] g cm < 2 >, and the hemolysis rate is 0.79-1.01%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the field of membrane technology, and specifically relates to a hydrogel-coated oxygenation membrane and a preparation method thereof. Background Art

[0002] Extracorporeal membrane oxygenation (ECMO) is an important means of treating patients with severe cardiopulmonary dysfunction. It can simultaneously improve blood oxygen saturation and remove carbon dioxide from the blood while assisting blood circulation. The oxygenation membrane acts as a barrier between blood and gas. Its gas permeability, blood compatibility, and resistance to plasma leakage are key factors affecting the long-term performance of the oxygenator.

[0003] Commercially available oxygenation membranes are mainly made of polypropylene (PP) and poly-4-methyl-1-pentene (PMP), which are representative materials of hollow fiber oxygenation membranes. Because medical-grade PP raw materials are cheap and easy to obtain, PP membranes have good gas permeability, with permeation rates of CO2 and O2 of 7.12 and 8.33 ml / (min·cm 2 ·bar)[1]. Although the presence of surface micropores increases the risk of gas embolism and plasma leakage during oxygenation, and plasma leakage occurs in PP membranes after about 8 hours, it is suitable for short-term cardiac surgery and can provide temporary respiratory support, making the market capacity of PP oxygenators large. The gas permeability of PMP membranes is low, with the permeation rates of CO2 and O2 being 1.69 and 0.59 ml / (min·cm 2 ·bar)[2], its structure is asymmetric structure with dense surface and porous inner layer, which makes its anti-plasma leakage time greater than 168h, suitable for long-term respiratory support for patients with cardiopulmonary failure. The surface of the commercial membrane is coated with anticoagulant heparin coating, heparin-like coating or zwitterion coating after plasma treatment, which can improve the blood compatibility of the membrane surface. However, a large amount of heparin anticoagulant needs to be injected in the application, and if the coating is blocked, it is easy to cause the gas exchange rate of the membrane to decrease, which is not conducive to clinical application.

[0004] PMP and PP only have methyl and methylene groups, but no active groups; plasma technology membrane surface modification is usually used to create oxygen-containing active groups on the membrane surface, but its process is complex and the precision is high, and there is still a certain threshold for large-scale application; other researchers mostly use strong acids, strong bases, and toxic chemical reagents to activate and modify them. According to the current market demand, providing an oxygenation membrane with a simple and efficient modification process, good anti-leakage performance, good blood compatibility, and high blood gas exchange performance is an urgent problem to be solved by personnel in this technical field.

[0005] [1]J.Li,T.He,H.Chen,Y.Cheng,E.Drioli,Z.Wang,Z.Cui,Preparation ofHyflon AD / Polypropylene Blend Membrane for Artificial Lung,Membranes 13(2023).https: / / doi.org / 10.3390 / membranes13070665.

[0006] [2]T.He, application,J.Membr.Sci.704(2024)122891.https: / / doi.org / https: / / doi.org / 10.1016 / j.memsci.2024.122891. Summary of the invention

[0007] In view of the above-mentioned prior art, the present invention provides a hydrogel-coated oxygenation membrane and a preparation method thereof. The present invention designs and prepares a series of hydrogel-coated oxygenation membranes. The high water content, good biocompatibility and network polymer structure of the hydrogel are utilized to solve the problems in the prior art that the modification threshold of the oxygenation membrane is high and the coating effect is not obvious, resulting in poor anti-plasma leakage performance and blood compatibility of the oxygenation membrane, and the occurrence of coating pore clogging and hindering gas exchange.

[0008] In order to solve the above technical problems, the present invention provides a hydrogel-coated oxygenation membrane, which comprises a step of modifying a flat membrane or a hollow fiber membrane with a microporous structure by using 20-40wt% polyolefin, 60-80wt% diluent and a modifying substance accounting for 5-15wt% of the mass fraction of polyolefin in the process of preparing the oxygenation membrane, promoting the migration of oxygen-containing functional groups to the membrane surface, so as to solve the modification problem of polyolefin and strengthen the interaction between the membrane body and the hydrogel layer. A 0.5-3μm hydrogel layer is coated on the surface of the flat membrane by a spin coating method with a rotation speed of 500-3000rpm or on the surface of the hollow fiber membrane by a dip coating method with a rotation speed of 500-1500mm / min. Break through the technical bottleneck of hydrogel membrane making and realize an efficient blood gas exchange process.

[0009] To achieve the above purpose, the technical solution adopted in this application is:

[0010] A method for preparing a hydrogel-coated oxygenated membrane comprises the following steps:

[0011] 1) adding 20-40 wt % of polyolefin resin and 5-15 wt % of modifying substance accounting for 60-80 wt % of polyolefin into 60-80 wt % of diluent, heating and stirring, and then standing to obtain a casting solution;

[0012] 2) using the casting solution as a raw material, scraping or spinning by thermally induced phase separation to obtain a flat membrane or a hollow fiber membrane;

[0013] 3) irradiating the hydrogel solution under ultraviolet light to make it semi-cured to obtain a pre-polymerized hydrogel solution;

[0014] 4) coating the pre-polymerized hydrogel solution obtained in step 3) on the flat membrane or hollow fiber membrane in step 2); then irradiating the membrane coated with the pre-polymerized hydrogel solution under ultraviolet light to completely solidify the hydrogel solution; and drying at room temperature to obtain a hydrogel-coated oxygenated membrane, wherein the hydrogel layer has a thickness of 0.5-3 μm.

[0015] In the step 1), the diluent includes one or more combinations of soybean oil, paraffin oil, dioctyl adipate, dibutyl phthalate, dioctyl phthalate, palm wax, triacetin, castor oil, acetyl tributyl citrate, acetyl trioctyl citrate, tributyl citrate, trioctyl citrate, and oleic acid; the polyolefin includes one of polypropylene, polyethylene, and poly(4-methyl-1-pentene); the modified substance is polyethylene-b-polyethylene glycol (PE-b-PEG), polyoxyethylene-polyoxypropylene ether (Pluronic F-127), which is a hydrophilic-hydrophobic block copolymer, one end of which is an oxygen-containing hydrophilic segment and the other end of which is a hydrophobic segment with good compatibility with polyolefins; the hydrogel includes one of poly(acrylamide-co-3-(trimethoxyphenyl)propyl methacrylate) (p(AAm-co-TMSPMA)), poly(acrylic acid-co-3-(trimethoxyphenyl)propyl methacrylate) (p(AAc-co-TMSPMA)) or poly((ethylene glycol) diacrylate-copoly(ethylene glycol) methacrylate) (p(PEGDA-co-PEGMA)).

[0016] In the step 1), the step of heating and stirring to be uniform and then standing is specifically heating to 160-180° C. and stirring to a uniform state, then heating to 170-190° C. and standing until there are no bubbles to obtain the casting solution.

[0017] In the step 2), the method of scraping the film by thermally induced phase separation is: pouring the casting liquid on a quartz glass plate with a tape having a thickness of 120-360 μm, scraping it with a scraper at a uniform speed of 1-10 cm / s, placing the glass plate with the casting liquid in a water coagulation bath at room temperature for solidification and then introducing it into the extractant, ensuring that the diluent is removed after extraction for 24-48 hours, replacing the extractant during the period, and then drying it until there is no moisture to obtain a flat membrane with micropore distribution; the extractant includes one or more of n-hexane, n-pentane, anhydrous ethanol, isopropanol, and ether.

[0018] In the step 2), the method of spinning by thermally induced phase separation is: the casting liquid is extruded through a spinneret at a spinning speed of 41 to 62 m / min and a core liquid flow rate of 8 to 20 ml / min, and then introduced into a water coagulation bath at room temperature for solidification and then introduced into an extractant, and after extraction for 24 to 48 hours, the diluent is ensured to be removed, the extractant is replaced during this period, and then dried until there is no moisture to obtain a hollow fiber membrane with a microporous distribution; the extractant includes one or more of n-hexane, n-pentane, anhydrous ethanol, isopropanol, and ether.

[0019] In the step 3), the pre-polymerized hydrogel solution is irradiated with ultraviolet light at 10-20W and 365nm to make the hydrogel solution reach a semi-cured state, wherein the semi-cured state is a sticky state between the fully fluid state of the hydrogel solution and the hard state of the cured hydrogel. The irradiation condition is preferably a time of irradiating the hydrogel solution of 50-70% of its fully cured time.

[0020] In the step 4), the method of coating the pre-polymerized hydrogel solution on the flat membrane is as follows: the flat membrane is attached to a glass plate and the pre-polymerized hydrogel solution is spin-coated with a coater at a speed of 500-3000 rpm, and then the membrane coated with the hydrogel is polymerized under ultraviolet light of 10-20W and 365nm to completely solidify the hydrogel solution, and then dried at room temperature to obtain an oxygenated membrane coated with the hydrogel.

[0021] In the step 4), the method of coating the pre-polymerized hydrogel solution on the hollow fiber membrane is as follows: the hollow fiber membrane is coated with the pre-polymerized hydrogel solution using a traction device at a speed of 500-1500 mm / min, and then the membrane coated with the hydrogel is polymerized under ultraviolet light of 10-20W and 365nm to completely cure the hydrogel solution, and then dried at room temperature to obtain a hydrogel-coated oxygenated membrane.

[0022] The hydrogel-coated oxygenation membrane prepared by the preparation method of the present invention includes a flat oxygenation membrane or a hollow fiber oxygenation membrane; the thickness of the flat oxygenation membrane is 100-300 μm, and the diameter and wall thickness of the hollow fiber oxygenation membrane are 276-632 μm and 66-153 μm; the flat oxygenation membrane and the hollow fiber oxygenation membrane have a double-layer structure as a whole, including a loose microporous layer and a dense non-porous layer, wherein the flat membrane or hollow fiber membrane composed of polyolefin and modified substance is loose microporous, and the hydrogel layer composed of hydrogel and coated on the outer surface of the flat membrane or hollow fiber membrane is dense and non-porous; the thickness of the dense non-porous hydrogel layer is 0.5-3 μm. The double-layer structure of the flat oxygenation membrane and the hollow fiber oxygenation membrane is as shown in the attached Figure 2 , Attachment Figure 4 As shown, layer 1 is a dense non-porous hydrogel layer, and layer 2 is a loose microporous flat membrane or hollow fiber membrane layer; the thickness of the dense non-porous hydrogel layer is 0.5-3 μm.

[0023] The hydrogel-coated oxygenation membrane of the present invention is used as a medium for blood gas exchange during extracorporeal membrane oxygenation.

[0024] Different from the prior art, the beneficial effects of the present invention are:

[0025] 1. The hydrogel-coated oxygenation membrane of the present invention utilizes the high water content, good biocompatibility and network polymer structure of the hydrogel to solve the problems in the prior art that the modification threshold of the oxygenation membrane is high and the coating effect is not obvious, resulting in poor plasma leakage resistance and blood compatibility of the oxygenation membrane, and the occurrence of coating pore clogging that hinders gas exchange. The oxygen-containing groups on the surface of the difficult-to-modify oxygenation membrane are functionalized through hydrophobic interactions to strengthen the interaction between the membrane body and the hydrogel, thereby avoiding the generation of defects and coating shedding. The functional groups in the hydrogel can enhance the transmission performance of carbon dioxide and oxygen; furthermore, the highly cross-linked hydrogel surface is dense, which can ensure excellent plasma leakage resistance and blood compatibility. The carbon dioxide and oxygen permeabilities of the flat oxygenation membrane coated with hydrogel in the present application can reach 163.58-208.94 and 110.77-208.89 ml·min -1 cm -2 bar -1 The O2 and CO2 permeabilities of the hydrogel-coated hollow fiber oxygenation membrane were 67.54-100.31 and 56.66-86.02 ml·min -1 cm -2 bar -1 The anti-plasma leakage time of the hydrogel-coated oxygenated membrane was 180-560 h, and the protein adhesion was 0.3-1.1 μg cm 2 The hemolysis rate was 0.79%-1.01%, which was significantly lower than that of PMP and PP commercial membranes. The finally prepared hydrogel-coated oxygenated membrane had good blood compatibility.

[0026] 2. The preparation method of the present application uniformly disperses the modifier in the casting solution, and scrapes and spins the film by thermally induced phase separation, and coats the hydrogel by spin coating and dip coating. The film-making process is simple and efficient, which greatly reduces the difficulty of film making and coating. The prepared hydrogel-coated oxygenation membrane is highly competitive as a blood-gas exchange medium in extracorporeal membrane oxygenation (ECMO). BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 This is a surface scanning electron micrograph of the hydrogel-coated flat oxygenated membrane of Example 2 of the present application.

[0028] Figure 2 This is a cross-sectional scanning electron microscope image of the hydrogel-coated flat oxygenation membrane of Example 2 of the present application, wherein layer 1 is a dense non-porous hydrogel layer, and layer 2 is a loose microporous membrane layer.

[0029] Figure 3 This is a surface scanning electron micrograph of the hydrogel-coated hollow fiber oxygenation membrane of Example 5 of the present application.

[0030] Figure 4 This is a cross-sectional scanning electron microscope image of the hydrogel-coated hollow fiber oxygenation membrane of Example 5 of the present application, including an overall cross-sectional image (a) and a cross-sectional scanning electron microscope image (b) within the black dashed area in Figure (a). In Figure (b), layer 1 is a dense, non-porous hydrogel layer, and layer 2 is a loose microporous membrane layer. DETAILED DESCRIPTION

[0031] The present application will be described in detail below in conjunction with the various embodiments shown in the accompanying drawings. However, these embodiments do not limit the present application, and any structural, methodological, or functional changes made by a person of ordinary skill in the art based on these embodiments are all within the scope of protection of the present application.

[0032] The present invention utilizes hydrophobic interaction to modify in one step to obtain a membrane body with a microporous structure, promotes the migration of oxygen-containing functional groups to the membrane surface, and strengthens the interaction between the membrane body and the hydrogel layer to solve the modification problem of polyolefins. The hydrogel is coated on the surface of the modified flat membrane by spin coating, or on the surface of the modified hollow fiber membrane by dip coating, breaking through the technical bottleneck of hydrogel membrane making and realizing an efficient blood-gas exchange process. The functional groups in the hydrogel reduce the transmission resistance of carbon dioxide and oxygen in the membrane, significantly improve the gas permeability of the oxygenation membrane, and at the same time ensure excellent plasma leakage resistance and blood compatibility; avoiding the complex manufacturing process of regulating the membrane structure in the current production of oxygenation membranes to improve the blood compatibility, plasma leakage resistance and gas transmission of the membrane.

[0033] The technical solution of the present application is further explained in detail below with reference to specific embodiments.

[0034] The hydrogels involved in the following embodiments include:

[0035] The hydrogel includes poly(acrylamide-co-3-(trimethoxyphenyl)propyl methacrylate) (p(AAm-co-TMSPMA)), poly(acrylic acid-co-3-(trimethoxyphenyl)propyl methacrylate) (p(AAc-co-TMSPMA)), poly((ethylene glycol) diacrylate-co poly(ethylene glycol) methacrylate) (p(PEGDA-co-PEGMA)), and the hydrogel is prepared by any method.

[0036] The technical solution of the present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments. The specific examples described are only used to explain the present invention and are not intended to limit the present invention.

[0037] Embodiment 1:

[0038] A hydrogel-coated flat oxygenation membrane was prepared using the following steps:

[0039] Step 1): Add 4 g of poly(4-methyl-1-pentene) resin and 0.20 g of PE-PEG to 3.6 g of acetyl trioctyl citrate and 2.4 g of tributyl citrate, and stir in a three-necked flask at 160° C. until uniform. Then, heat to 170° C. and let stand until there are no bubbles to obtain a casting solution.

[0040] Step 2): The casting liquid is used as a raw material and a film is scraped by a thermally induced phase separation method. The casting liquid is poured onto a quartz glass plate with a tape having a thickness of 120 μm, and scraped with a scraper at a uniform speed of 1 cm / s. The glass plate with the casting liquid is placed in a water coagulation bath at room temperature for solidification and then introduced into anhydrous ethanol as an extractant. The extraction is performed for 24 hours to ensure that trioctyl acetyl citrate and tributyl citrate are removed, during which ethanol is replaced twice, and then dried at room temperature until there is no moisture to obtain a flat film.

[0041] Step 3): Irradiate the p(AAm-co-TMSPMA) hydrogel solution under ultraviolet light of 10W and 365nm to make it semi-cured to obtain a pre-polymerized hydrogel solution, wherein the irradiation condition is that the irradiation time of the hydrogel solution is 50% of its complete curing time.

[0042] Step 4): Spin coating at 500 rpm on 10 cm 2 2 ml of pre-polymerized hydrogel solution was coated on the surface of the flat membrane, and the membrane coated with the pre-polymerized hydrogel solution was irradiated with ultraviolet light at 10W and 365nm for the remaining 50% of the time required for the hydrogel solution to be completely cured. After drying at room temperature, a hydrogel-coated oxygenated membrane was obtained, wherein the thickness of the hydrogel layer was 0.5 μm.

[0043] The thickness of the hydrogel-coated oxygenated membrane was 100 μm, and the membrane’s O2 and CO2 permeabilities were 110.77 and 163.58 ml·min -1 cm -2 bar -1 The anti-plasma leakage time was 180 h and the protein adhesion amount was 0.3 μg cm 2 , the hemolysis rate was 0.79%.

[0044] Embodiment 2:

[0045] A hydrogel-coated flat oxygenation membrane was prepared using the following steps:

[0046] Step 1): Add 3 g of polypropylene resin and 0.30 g of Pluronic F-127 to 4.2 g of paraffin oil and 2.8 g of acetyl tributyl citrate, and stir in a three-necked flask at 170° C. until uniform. Then heat to 180° C. and let stand until there are no bubbles to obtain a casting solution.

[0047] Step 2): The casting liquid is used as a raw material and a film is scraped by a thermally induced phase separation method. The casting liquid is poured onto a quartz glass plate with a tape having a thickness of 240 μm, and scraped at a uniform speed of 6 cm / s with a scraper. The glass plate with the casting liquid is placed in a water coagulation bath at room temperature for solidification and then introduced into a mixed solution of extractants n-pentane and isopropanol. Extraction is performed for 36 hours to ensure that paraffin oil and acetyl tributyl citrate are removed. During this period, n-pentane and isopropanol are replaced twice, and then dried at room temperature until there is no moisture to obtain a flat film.

[0048] Step 3): Irradiate the p(AAc-co-TMSPMA) hydrogel solution under ultraviolet light of 15W and 365nm to make it semi-cured to obtain a pre-polymerized hydrogel solution, wherein the irradiation condition is that the irradiation time of the hydrogel solution is 60% of its complete curing time.

[0049] Step 4): Spin coating at 1500 rpm on 10 cm 2 4 ml of pre-polymerized hydrogel solution was coated on the surface of the flat membrane, and the membrane coated with the pre-polymerized hydrogel solution was irradiated under ultraviolet light of 15W and 365nm for the remaining 40% of the time required for the hydrogel solution to be completely cured. After drying at room temperature, a hydrogel-coated oxygenated membrane was obtained, wherein the thickness of the hydrogel layer was 2.25 μm.

[0050] like Figure 1 , Figure 2 As shown, the prepared hydrogel-coated flat oxygenation membrane includes a flat membrane with micropore distribution and a dense non-porous hydrogel layer wrapped on the surface of the flat membrane; Figure 2In the embodiment, one layer is a dense non-porous hydrogel layer, and the other two layers are loose microporous membrane layers of the flat membrane. The thickness of the hydrogel-coated flat oxygenation membrane is about 150 μm, and the thickness of the hydrogel layer is about 2.3 μm.

[0051] The O2 and CO2 permeabilities of the hydrogel-coated oxygenation membrane were 165.53 and 176.55 ml·min -1 cm -2 bar -1 The anti-plasma leakage time was 240 h and the protein adhesion amount was 0.7 μg cm 2 , the hemolysis rate was 0.91%.

[0052] Embodiment 3:

[0053] A hydrogel-coated flat oxygenation membrane was prepared using the following steps:

[0054] Step 1): Add 2 g of polyethylene resin and 0.30 g of PE-PEG to 4.8 g of dioctyl adipate and 3.2 g of castor oil, and stir in a three-necked flask at 180° C. until uniform. Then heat to 190° C. and let stand until there are no bubbles to obtain a casting solution.

[0055] Step 2): The casting liquid is used as a raw material and a film is scraped by a thermally induced phase separation method. The casting liquid is poured onto a quartz glass plate with a tape having a thickness of 360 μm, and scraped at a uniform speed of 10 cm / s with a scraper. The glass plate with the casting liquid is placed in a water coagulation bath at room temperature for solidification and then introduced into an extractant, anhydrous ethanol, and extracted for 48 hours to ensure that diisooctyl adipate and castor oil are removed. During this period, n-hexane and anhydrous ethanol are replaced twice, and then dried at room temperature until there is no moisture to obtain a flat film.

[0056] Step 3): Irradiate the p(PEGDA-co-PEGMA) hydrogel solution under ultraviolet light of 20W and 365nm to make it semi-cured to obtain a pre-polymerized hydrogel solution, wherein the irradiation condition is that the irradiation time of the hydrogel solution is 70% of its complete curing time.

[0057] Step 4): Spin coating at 3000 rpm on 10 cm 2 3 ml of pre-polymerized hydrogel solution was coated on the surface of the flat membrane, and the membrane coated with the pre-polymerized hydrogel solution was irradiated with ultraviolet light at 20 W and 365 nm for the remaining 30% of the time required for the hydrogel solution to be completely cured. After drying at room temperature, a hydrogel-coated oxygenated membrane was obtained, wherein the thickness of the hydrogel layer was 3.0 μm.

[0058] The thickness of the hydrogel-coated oxygenated membrane was 300 μm, and the membrane’s O2 and CO2 permeabilities were 208.89 and 208.94 ml·min -1cm -2 bar -1 The anti-plasma leakage time was 560 h and the protein adhesion amount was 1.1 μg cm 2 , the hemolysis rate was 1.01%.

[0059] Embodiment 4:

[0060] A hydrogel-coated hollow fiber oxygenation membrane is prepared by the following steps:

[0061] Step 1): Add 240g of poly(4-methyl-1-pentene) resin and 12g of Pluronic F-127 to 360g of dioctyl phthalate, stir in a reactor of a twin-screw spinning machine at 160°C until uniform, then heat to 170°C and let stand until there are no bubbles to obtain a casting solution.

[0062] Step 2): The casting solution is used as a raw material, and spinning is performed by a twin-screw spinning machine using a thermally induced phase separation method. The casting solution is extruded through a spinneret, the spinning speed is 41m / min, the core liquid flow rate is 8ml / min, and then introduced into a water coagulation bath at room temperature for solidification and then introduced into anhydrous ethanol as an extractant, and extracted for 24h to ensure the removal of dioctyl phthalate, during which the anhydrous ethanol is replaced twice, and then dried at room temperature until there is no water to obtain a hollow fiber membrane.

[0063] Step 3): Irradiate the p(AAm-co-TMSPMA) hydrogel solution under ultraviolet light of 10W and 365nm to make it semi-cured to obtain a pre-polymerized hydrogel solution, wherein the irradiation condition is that the irradiation time of the hydrogel solution is 50% of its complete curing time.

[0064] Step 4): 8 ml of the pre-polymerized hydrogel solution was coated on the surface of a hollow fiber membrane having a length of 1.5 m and a diameter of 275.5 μm by a dip coating method at a rotation speed of 500 mm / min, and the membrane coated with the pre-polymerized hydrogel solution was irradiated with ultraviolet light at 10 W and 365 nm for the remaining 50% of the time required for the hydrogel solution to be completely cured. After drying at room temperature, a hydrogel-coated oxygenated membrane was obtained, wherein the thickness of the hydrogel layer was 0.5 μm.

[0065] The diameter and wall thickness of the hydrogel-coated oxygenation membrane were 276 μm and 66 μm, and the membrane permeabilities of O2 and CO2 were 67.54 and 56.66 ml·min -1 cm -2 bar -1 The anti-plasma leakage time was 180 h and the protein adhesion amount was 0.3 μg cm 2 , the hemolysis rate was 0.79%.

[0066] Embodiment 5:

[0067] A hydrogel-coated hollow fiber oxygenation membrane is prepared by the following steps:

[0068] Step 1): Add 100 g of polypropylene resin and 15 g of PE-PEG to 250 g of soybean oil and 150 g of acetyl tributyl citrate, and stir in a reactor of a twin-screw spinning machine at 180° C. until uniform. Then heat to 190° C. and let stand until there are no bubbles to obtain a casting solution.

[0069] Step 2): The casting solution is used as a raw material, and spinning is performed by a twin-screw spinning machine using a thermally induced phase separation method. The casting solution is extruded through a spinneret, the spinning speed is 62m / min, the core liquid flow rate is 20ml / min, and then introduced into a water coagulation bath at room temperature for solidification and then introduced into extractants n-pentane and anhydrous ethanol, and extracted for 48h to ensure that soybean oil and acetyl tributyl citrate are removed, during which n-pentane and anhydrous ethanol are replaced twice, and then dried at room temperature until there is no water to obtain a hollow fiber membrane.

[0070] Step 3): Irradiate the p(AAc-co-TMSPMA) hydrogel solution under ultraviolet light of 20W and 365nm to make it semi-cured to obtain a pre-polymerized hydrogel solution, wherein the irradiation condition is that the irradiation time of the hydrogel solution is 70% of its complete curing time.

[0071] Step 4): 6 ml of the pre-polymerized hydrogel solution was coated on the surface of a hollow fiber membrane with a length of 1.0 m and a diameter of 629 μm by a dip coating method at a rotation speed of 1500 mm / min, and the membrane coated with the pre-polymerized hydrogel solution was irradiated with ultraviolet light at 20 W and 365 nm for the remaining 30% of the time required for the hydrogel solution to be completely cured. After drying at room temperature, a hydrogel-coated oxygenated membrane was obtained, wherein the thickness of the hydrogel layer was 3.00 μm.

[0072] like Figure 3 , Figure 4 As shown, the prepared hydrogel-coated hollow fiber oxygenation membrane has an internal hollow structure, including a hollow fiber membrane with micropore distribution and a dense and non-porous hydrogel layer wrapped on the surface of the hollow fiber membrane. Figure 4 In (b), layer 1 is a dense, non-porous hydrogel layer, and layer 2 is a loose microporous membrane layer of the hollow fiber. The diameter and wall thickness of the hydrogel-coated hollow fiber oxygenation membrane are about 632 μm and 153 μm, and the hydrogel layer is about 3.00 μm.

[0073] The O2 and CO2 permeabilities of the hydrogel-coated oxygenation membrane were 100.31 and 86.02 ml·min -1 cm -2 bar -1 The anti-plasma leakage time was 560 h and the protein adhesion amount was 1.1 μg cm2 , the hemolysis rate was 1.01%.

[0074] Embodiment 6:

[0075] A hydrogel-coated hollow fiber oxygenation membrane is prepared by the following steps:

[0076] Step 1): 180 g of polyethylene resin and 18 g of PE-PEG were added to 252 g of paraffin oil and 168 g of oleic acid, and stirred in a reactor of a twin-screw spinning machine at 170° C. until uniform. The mixture was then heated to 180° C. and allowed to stand until no bubbles were present to obtain a casting solution.

[0077] Step 2): The casting solution is used as a raw material, and spinning is performed by a twin-screw spinning machine using a thermally induced phase separation method. The casting solution is extruded through a spinneret, the spinning speed is 52m / min, the core liquid flow rate is 15ml / min, and then introduced into a water coagulation bath at room temperature for solidification and then introduced into extractants n-hexane and ether, and extracted for 36h to ensure that paraffin oil and oleic acid are removed, during which n-hexane and ether are replaced twice, and then dried at room temperature until there is no water, and then dried at room temperature to obtain a hollow fiber membrane.

[0078] Step 3): Irradiate the p(PEGDA-co-PEGMA) hydrogel solution under ultraviolet light of 15W and 365nm to make it semi-cured to obtain a pre-polymerized hydrogel solution, wherein the irradiation condition is that the irradiation time of the hydrogel solution is 60% of its complete curing time.

[0079] Step 4): 4 ml of the pre-polymerized hydrogel solution was coated on the surface of a hollow fiber membrane having a length of 1.3 m and a diameter of 340 μm by a dip coating method at a rotation speed of 1000 mm / min, and the membrane coated with the pre-polymerized hydrogel solution was irradiated under ultraviolet light of 15 W and 365 nm for the remaining 40% of the time required for the hydrogel solution to be completely cured. After drying at room temperature, a hydrogel-coated oxygenated membrane was obtained, wherein the thickness of the hydrogel layer was 1.0 μm.

[0080] The diameter and wall thickness of the hydrogel-coated oxygenation membrane were 340 μm and 96 μm, and the membrane permeabilities of O2 and CO2 were 79.74 and 86.66 ml·min -1 cm -2 bar -1 The anti-plasma leakage time was 300 h and the protein adhesion amount was 0.6 μg cm 2 , the hemolysis rate was 0.96%.

[0081] Embodiment 7:

[0082] A hydrogel-coated hollow fiber oxygenation membrane is prepared by the following steps:

[0083] Step 1): Add 180 g of poly(4-methyl-1-pentene) resin and 24 g of PE-PEG to 210 g of palm wax and 210 g of castor oil, and stir in a reactor of a twin-screw spinning machine at 160° C. until uniform. Then heat to 170° C. and let stand until there are no bubbles to obtain a casting solution.

[0084] Step 2): The casting solution is used as a raw material, and spinning is performed by a twin-screw spinning machine using a thermally induced phase separation method. The casting solution is extruded through a spinneret, the spinning speed is 41m / min, the core liquid flow rate is 8ml / min, and then introduced into a water coagulation bath at room temperature for solidification and then introduced into an extractant of anhydrous ethanol and ether, and extracted for 24h to ensure that palm wax and castor oil are removed, during which anhydrous ethanol and ether are replaced twice, and then dried at room temperature to obtain a hollow fiber membrane.

[0085] Step 3): Irradiate the p(AAm-co-TMSPMA) hydrogel solution under ultraviolet light of 17W and 365nm to make it semi-cured to obtain a pre-polymerized hydrogel solution, wherein the irradiation condition is that the irradiation time of the hydrogel solution is 50% of its complete curing time.

[0086] Step 4): 3 ml of the pre-polymerized hydrogel solution was coated on the surface of a hollow fiber membrane with a length of 1.0 m and a diameter of 385.4 μm by dip coating at a rotation speed of 500 mm / min, and the membrane coated with the pre-polymerized hydrogel solution was irradiated under ultraviolet light (17 W, 365 nm) for a time sufficient to completely cure the hydrogel solution for the remaining 50% of the time. After drying at room temperature, a hydrogel-coated oxygenated membrane was obtained, wherein the thickness of the hydrogel layer was 0.6 μm.

[0087] The diameter and wall thickness of the hydrogel-coated oxygenation membrane were 386 μm and 130 μm, and the membrane permeabilities of O2 and CO2 were 72.36 and 80.32 ml·min -1 cm -2 bar -1 The anti-plasma leakage time was 520 h and the protein adhesion amount was 0.5 μg cm 2 , the hemolysis rate was 0.83%.

[0088] Embodiment 8:

[0089] A hydrogel-coated hollow fiber oxygenation membrane is prepared by the following steps:

[0090] Step 1): Add 140g of polypropylene resin and 14g of PE-PEG to 250g of triacetin and 170g of dibutyl phthalate, and stir in a reactor of a twin-screw spinning machine at 170°C until uniform. Then heat to 180°C and let stand until there are no bubbles to obtain a casting solution.

[0091] Step 2): The casting solution is used as a raw material, and spinning is performed by a twin-screw spinning machine using a thermally induced phase separation method. The casting solution is extruded through a spinneret, the spinning speed is 51 m / min, the core liquid flow rate is 14 ml / min, and then introduced into a water coagulation bath at room temperature for solidification and then introduced into extractants n-pentane and anhydrous ethanol, and extracted for 36 hours to ensure the removal of triacetin and dibutyl phthalate, during which n-pentane and anhydrous ethanol are replaced twice, and then dried at room temperature to obtain a hollow fiber membrane.

[0092] Step 3): Irradiate the p(AAm-co-TMSPMA) hydrogel solution under ultraviolet light of 20W and 365nm to make it semi-cured to obtain a pre-polymerized hydrogel solution, wherein the irradiation condition is that the irradiation time of the hydrogel solution is 60% of its complete curing time.

[0093] Step 4): 5 ml of the pre-polymerized hydrogel solution was coated on the surface of a hollow fiber membrane with a length of 2.0 m and a diameter of 418.2 μm by a dip coating method at a rotation speed of 1000 mm / min, and the membrane coated with the pre-polymerized hydrogel solution was irradiated with ultraviolet light at 20 W and 365 nm for the remaining 40% of the time required for the hydrogel solution to be completely cured. After drying at room temperature, a hydrogel-coated oxygenated membrane was obtained, wherein the thickness of the hydrogel layer was 1.8 μm.

[0094] The diameter and wall thickness of the hydrogel-coated oxygenation membrane were 420 μm and 115 μm, respectively, and the membrane permeabilities of O2 and CO2 were 89.66 and 69.79 ml·min -1 cm -2 bar -1 The anti-plasma leakage time was 480 h and the protein adhesion amount was 0.3 μg cm 2 , the hemolysis rate was 0.94%.

[0095] Embodiment 9:

[0096] A hydrogel-coated hollow fiber oxygenation membrane is prepared by the following steps:

[0097] Step 1): Add 220g of polyethylene resin and 33g of Pluronic F-127 to 270g of tributyl citrate and 270g of trioctyl citrate, and stir in a reactor of a twin-screw spinning machine at 180°C until uniform. Then heat to 190°C and let stand until there are no bubbles to obtain a casting solution.

[0098] Step 2): The casting solution is used as a raw material, and spinning is performed by a twin-screw spinning machine using a thermally induced phase separation method. The casting solution is extruded through a spinneret, the spinning speed is 62m / min, the core liquid flow rate is 20ml / min, and then introduced into a water coagulation bath at room temperature for solidification and then introduced into an extractant, anhydrous ethanol, and extracted for 24h to ensure that tributyl citrate and trioctyl citrate are removed, during which anhydrous ethanol is replaced twice, and then dried at room temperature until there is no water to obtain a hollow fiber membrane.

[0099] Step 3): Irradiate the p(PEGDA-co-PEGMA) hydrogel solution under ultraviolet light of 10W and 365nm to make it semi-cured to obtain a pre-polymerized hydrogel solution, wherein the irradiation condition is that the irradiation time of the hydrogel solution is 70% of its complete curing time.

[0100] Step 4): 1 ml of the pre-polymerized hydrogel solution was coated on the surface of a hollow fiber membrane with a length of 0.8 m and a diameter of 537.6 μm by dip coating at a rotation speed of 500 mm / min, and the membrane coated with the pre-polymerized hydrogel solution was irradiated under ultraviolet light (15 W, 365 nm) for the remaining 30% of the time required for the hydrogel solution to completely solidify. After drying at room temperature, a hydrogel-coated oxygenated membrane was obtained, wherein the thickness of the hydrogel layer was 2.4 μm.

[0101] The diameter and wall thickness of the hydrogel-coated oxygenation membrane were 540 μm and 136 μm, and the membrane permeabilities of O2 and CO2 were 95.47 and 73.14 ml·min -1 cm -2 bar -1 The anti-plasma leakage time was 360 h and the protein adhesion amount was 0.8 μg cm 2 , the hemolysis rate was 0.99%.

[0102] Performance Test 1:

[0103] In order to characterize the CO2 permeation rate and O2 permeation rate of the hydrogel-coated oxygenation membrane prepared in Examples 1 to 9. The hydrogel-coated oxygenation membrane prepared in Examples 1 to 9 was introduced into a homemade flat membrane assembly or a hollow fiber membrane assembly encapsulated with epoxy resin AB glue, and 1 bar of oxygen or carbon dioxide was introduced. The gas flow was measured with a soap film flowmeter. The CO2 permeation rate and O2 permeation rate of the hydrogel-coated oxygenation membrane were calculated by the following formula (1); In order to characterize the anti-plasma leakage time of the hydrogel-coated oxygenation membrane prepared in Examples 1 to 9, the anti-plasma leakage time was tested with reference to the method suggested in patent CN 112403289 A. The prepared membrane was encapsulated in a membrane assembly and the shell side or near the hydrogel layer of the assembly was filled with phosphate buffered saline (PBS) solution and kept at a constant temperature of 37°C. Nitrogen was introduced into the tube side of the membrane assembly for purging, and the outlet of the purge gas was connected to a drying tube filled with anhydrous copper sulfate. The time after the anhydrous copper sulfate in the drying tube began to change color was defined as the anti-plasma leakage time.

[0104]

[0105] P: Gas permeability of the hydrogel-coated oxygenated membrane (ml / (min·cm 2 bar)); Q i (ml / min) is the volume flow rate of gas "i", A (cm 2 ) refers to the effective membrane area of ​​the hydrogel-coated oxygenated membrane, Δp i (bar) represents the partial pressure difference between the feed end and the permeate end of gas "i", where "i" is CO2 or O2.

[0106] Performance Test 2:

[0107] In order to characterize the protein adhesion and hemolysis rate of the hydrogel-coated oxygenated membranes prepared in Examples 1 to 9. The membranes were added to a phosphate buffer solution (PBS, pH = 7.4) and immersed in bovine serum albumin (BSA, 4.5 mg / mL) for two hours after equilibration at room temperature for 2 hours, and stored in a humidified water-jacketed incubator with 5% carbon dioxide in air for 2 hours. After rinsing with PBS five times, the membranes were placed in a beaker containing 2 mL of 1% (w / v%) sodium dodecyl sulfate (SDS) aqueous solution, and ultrasonicated at room temperature for 20 minutes to separate the adsorbed proteins from the surface. A protein detection reagent called bichondroitin acid (BCA) was added and incubated at 60°C for 1 hour. After the beaker was cooled to room temperature, the absorbance with the blank sample was measured at 562 nm. Using the standard curve, the amount of protein adhesion adsorbed on the sample surface was calculated. In addition, the red blood cell compatibility of the membrane was evaluated by a hemolysis rate test. 10 ml of whole blood diluted with 60 ml of saline and 60 ml of deionized water were used as negative and positive controls, respectively. The membrane was incubated with 5 ml of whole blood diluted with saline at 37°C for 3 hours. The blood sample was centrifuged at 3000 rpm for 10 minutes, and the supernatant was taken and analyzed for hemoglobin absorbance at 545 nm. The hemolysis rate (H r ) is determined by the following formula (2):

[0108]

[0109] A s is the absorbance of the sample set, A n is the absorbance of the negative group, A p is the absorbance of the sample set.

[0110] The CO2 and O2 permeation rates, plasma leakage resistance time, membrane thickness or diameter, hydrogel layer thickness, protein adhesion amount and hemolysis rate of the hydrogel-coated oxygenation membranes prepared in Examples 1 to 9 of the present invention are summarized as shown in Table 1.

[0111] Table 1 Gas permeability, plasma leakage resistance, membrane thickness, and blood compatibility of hydrogel-coated oxygenation membranes.

[0112] Table 1

[0113]

[0114]

[0115] As shown in the above table, the CO2 permeation rate, O2 permeation rate and anti-plasma leakage time of the hydrogel-coated flat oxygenation membrane prepared in Examples 1 to 3 are significantly better than those of PMP and PP commercial membranes. The CO2 permeation rate of the hydrogel-coated flat oxygenation membrane in Example 3 is 208.94 ml / (min·cm 2·bar), O2 permeation rate is 208.89ml / (min·cm 2 ·bar); and the CO2 permeation rate, O2 permeation rate and anti-plasma leakage time of the hydrogel-coated hollow fiber oxygenation membranes prepared in Examples 4 to 9 were significantly better than those of PMP and PP commercial membranes. The CO2 permeation rate of the hydrogel-coated hollow fiber oxygenation membrane in Example 5 was 86.02 ml / (min·cm 2 ·bar), O2 permeation rate is 100.31ml / (min·cm 2 In addition, the protein adhesion amounts of Examples 1 to 9 were 0.3-1.1 μg cm 2 The hemolysis rate was 0.79%-1.01%, which was significantly lower than that of PMP and PP commercial membranes. The finally prepared hydrogel-coated oxygenated membrane had good blood compatibility.

[0116] The hydrogel-coated oxygenation membranes prepared in Examples 1 to 9 utilize the characteristics of hydrogels, and use the high water content, good biocompatibility, and network polymer structure of hydrogels to coat the hydrogels as a coating on the modified oxygenation membranes, thereby strengthening the effective coupling between the oxygenation membranes and the hydrogels. The functional groups in the hydrogels can increase the gas permeability of carbon dioxide and oxygen molecules through the oxygenation membranes while ensuring excellent plasma leakage resistance and blood compatibility, solving the problem of dense coatings shielding gas permeability; and avoiding the complex manufacturing process of regulating the membrane structure in the current production of oxygenation membranes to improve the blood compatibility, plasma leakage resistance, and gas transmission of the membranes.

[0117] The above description of the present disclosure is provided to enable any person of ordinary skill in the art to implement or use the present disclosure. Various modifications to the present disclosure will be apparent to those of ordinary skill in the art, and the general principles corresponding to the present disclosure may be applied to other variations without departing from the scope of protection of the present disclosure. Therefore, the present disclosure is not limited to the examples and designs described herein, but is consistent with the widest range of principles and novel features disclosed herein.

Claims

1. A method for preparing a hydrogel-coated oxygenated membrane, characterized in that The following steps are involved: 1) adding 20-40 wt % of polyolefin resin and 5-15 wt % of modifying substance accounting for 60-80 wt % of polyolefin into 60-80 wt % of diluent, heating and stirring, and then standing to obtain a casting solution; 2) using the casting solution as a raw material, scraping or spinning by thermally induced phase separation to obtain a flat membrane or a hollow fiber membrane; 3) irradiating the hydrogel solution under ultraviolet light to make it semi-cured to obtain a pre-polymerized hydrogel solution; 4) coating the pre-polymerized hydrogel solution obtained in step 3) on the flat membrane or hollow fiber membrane in step 2); then irradiating the membrane coated with the pre-polymerized hydrogel solution under ultraviolet light to completely solidify the hydrogel solution; and drying at room temperature to obtain a hydrogel-coated oxygenated membrane, wherein the hydrogel layer has a thickness of 0.5-3 μm.

2. The method for preparing the hydrogel-coated oxygenated membrane according to claim 1, characterized in that In step 1), the diluent includes one or more combinations of soybean oil, paraffin oil, diisooctyl adipate, dibutyl phthalate, dioctyl phthalate, palm wax, triacetin, castor oil, acetyl tributyl citrate, acetyl trioctyl citrate, tributyl citrate, trioctyl citrate, and oleic acid; the polyolefin includes one of polypropylene, polyethylene, and poly(4-methyl-1-pentene); the modified substance is one of polyethylene-b-polyethylene glycol and polyoxyethylene-polyoxypropylene ether; the hydrogel includes one of poly(acrylamide-co-3-(trimethoxyphenyl) propyl methacrylate), poly(acrylic acid-co-3-(trimethoxyphenyl) propyl methacrylate) or poly((ethylene glycol) diacrylate-co-poly(ethylene glycol) methacrylate).

3. The method for preparing the hydrogel-coated oxygenated membrane according to claim 1, characterized in that In step 1), the step of heating and stirring to be uniform and then standing is specifically heating to 160-180° C. and stirring to a uniform state, then heating to 170-190° C. and standing until there are no bubbles to obtain a casting solution.

4. The method for preparing the hydrogel-coated oxygenated membrane according to claim 1, characterized in that In step 2), the method of scraping the film by thermally induced phase separation is: pouring the casting liquid on a quartz glass plate with a tape having a thickness of 120-360 μm, scraping it with a scraper at a uniform speed of 1-10 cm / s, placing the glass plate with the casting liquid in a water coagulation bath at room temperature for solidification and then introducing it into the extractant, ensuring that the diluent is removed after extraction for 24-48 hours, replacing the extractant during the period, and then drying it until there is no moisture to obtain a flat membrane with micropore distribution; the extractant includes one or more of n-hexane, n-pentane, anhydrous ethanol, isopropanol, and ether.

5. The method for preparing a hydrogel-coated oxygenated membrane according to claim 1, characterized in that In step 2), the method of spinning by thermally induced phase separation is: the casting liquid is extruded through a spinneret at a spinning speed of 41 to 62 m / min and a core liquid flow rate of 8 to 20 ml / min, and then introduced into a water coagulation bath at room temperature for solidification and then introduced into an extractant, and the diluent is removed after extraction for 24 to 48 hours, during which the extractant is replaced, and then dried until there is no moisture to obtain a hollow fiber membrane with a microporous distribution; the extractant includes one or more of n-hexane, n-pentane, anhydrous ethanol, isopropanol, and ether.

6. The method for preparing a hydrogel-coated oxygenated membrane according to claim 1, characterized in that In step 3), the pre-polymerized hydrogel solution is irradiated with ultraviolet light of 10-20W and 365nm to make the hydrogel solution reach a semi-cured state, and the irradiation condition is preferably such that the irradiation time of the hydrogel solution is 50-70% of its complete curing time.

7. The method for preparing a hydrogel-coated oxygenated membrane as claimed in claim 1, characterized in that In step 4), the pre-polymerized hydrogel solution is coated on the flat membrane. The flat membrane is attached to a glass plate and the pre-polymerized hydrogel solution is spin-coated with a coater at a speed of 500-3000 rpm. The membrane coated with the hydrogel is then polymerized under ultraviolet light of 10-20 W and 365 nm to completely cure the hydrogel solution. The membrane is dried at room temperature to obtain an oxygenated membrane coated with the hydrogel.

8. The method for preparing a hydrogel-coated oxygenated membrane according to claim 1, characterized in that In step 4), the pre-polymerized hydrogel solution is coated on the hollow fiber membrane. The method is as follows: the hollow fiber membrane is coated with the pre-polymerized hydrogel solution using a traction device at a speed of 500-1500 mm / min, and then the membrane coated with the hydrogel is polymerized under ultraviolet light of 10-20 W and 365 nm to completely solidify the hydrogel solution, and then it is dried at room temperature to obtain a hydrogel-coated oxygenated membrane.

9. The hydrogel-coated oxygenated membrane prepared by the preparation method of claim 1, characterized in that It comprises a flat oxygenation membrane or a hollow fiber oxygenation membrane; the thickness of the flat oxygenation membrane is 100-300 μm, and the diameter and wall thickness of the hollow fiber oxygenation membrane are 276-632 μm and 66-153 μm; the flat oxygenation membrane and the hollow fiber oxygenation membrane present a double-layer structure as a whole, including a loose microporous layer and a dense non-porous layer, wherein the flat membrane or hollow fiber membrane composed of polyolefin and modified substance is loose microporous, and the hydrogel layer composed of hydrogel and coated on the outer surface of the flat membrane or hollow fiber membrane is dense and non-porous; the thickness of the dense non-porous hydrogel layer is 0.5-3 μm.

10. The hydrogel-coated oxygenation membrane of claim 9 is used as a medium for blood gas exchange during extracorporeal membrane oxygenation.

Citation Information

Patent Citations

  • Application of natural polysaccharide hydrogel in field of hemostasis

    CN113024847A

  • Hollow fiber membrane yarn, preparation method thereof and oxygenation membrane

    CN116059835A

  • Method for preparing hollow fiber composite membrane and hollow fiber composite membrane

    CN117619160A

  • Preparation and application of agarose chemical modified polydimethylsiloxane / polyethersulfone composite membrane

    CN118161995A