PVDF hollow fiber composite membrane and preparation method thereof
PVDF hollow fiber composite film was prepared by thermal phase separation method, and the MXene nanosheets were used to closely adhere to the PVDF film surface by using high temperature and extrusion pressure, which solved the problem of easy peeling of MXene materials and improved the flux and wear resistance of the film. Achieve higher utilization and performance.
Patent Information
- Application Number
- CN202411160847.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-11-08
AI Technical Summary
The prior art is difficult to improve the firmness between the MXene material and the matrix membrane while maintaining the hydrophilicity, permeability flux and retention properties of the ultrafiltration membrane, and the operation is complicated and the utilization rate of the MXene material is low.
The PVDF hollow fiber composite film was prepared by thermally induced phase separation. By hot melting and tightly bonding the inner cast film liquid of MXene nanosheets and PVDF at high temperature and extrusion pressure, a firm inorganic MXene layer was formed, which improved MXene and Binding strength of PVDF membrane.
It significantly improves the utilization rate of MXene material and the flux and wear resistance of PVDF hollow fiber composite film, and is simple and reliable in operation, reducing the risk of falling off of the MXene layer and improving the overall performance of the film.
Smart Images

Figure CN118904102A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymer membrane materials, and in particular to a PVDF hollow fiber composite membrane and a preparation method thereof. Background Art
[0002] Ultrafiltration membrane separation technology can effectively remove macromolecular proteins, bacteria, colloidal particles, dye molecules, etc. from water, and is currently one of the key technologies in the field of water treatment. In the membrane formation process, doping with inorganic nanomaterials is a major direction for improving membrane performance. The introduction of inorganic nanoparticles can not only improve the hydrophilicity of the prepared membrane through its own hydrophilicity, but also the good mechanical strength of the inorganic material itself will give the membrane higher wear resistance.
[0003] Transition metal carbon / nitride (MXene) materials have attracted much attention as a new type of two-dimensional inorganic nanomaterial with high specific surface area, excellent conductivity and hydrophilicity. For example, patent No. CN106178979B uses suction filtration and other methods to deposit Ti3C2-MXene nanosheets on a flat porous substrate, and obtains a two-dimensional layered Ti3C2-MXene membrane after drying. The water flux of the obtained ultrafiltration membrane is more than 10 times that of the graphene oxide membrane. However, the suction filtration pressure can generally only reach 0.1MPa, and there is a problem of MXene material falling off in long-term harsh water environments. Patent No. CN116272419A provides a technology for thermally cross-linking MXene materials with hollow fiber membranes to alleviate the problem of easy shedding of MXene materials, but the operation is more complicated and the utilization rate of MXene materials is low.
[0004] In view of this, how to achieve good hydrophilicity, large water flux and high interception performance of ultrafiltration membrane while further improving the firmness between MXene material and the base membrane to achieve cost reduction and efficiency improvement is a technical problem that technical personnel in this field urgently need to solve. Summary of the invention
[0005] Based on the above problems, the present invention provides a PVDF hollow fiber composite membrane and a preparation method thereof. The PVDF hollow fiber composite membrane is prepared by a thermally induced phase separation method. While ensuring that the hydrophilicity, water permeability and interception performance of the PVDF hollow fiber composite membrane meet the use requirements, the firmness between the MXene material and the base membrane in the PVDF hollow fiber composite membrane is greatly improved, and the wear resistance of the PVDF hollow fiber composite membrane is further improved. The specific invention contents are as follows:
[0006] In a first aspect, the present invention provides a method for preparing a PVDF hollow fiber composite membrane, the preparation method comprising:
[0007] Dispersing MXene nanosheets in a dispersing solvent to obtain an outer layer casting solution containing 0.05 wt % to 2 wt % of MXene nanosheets;
[0008] The diluent and PVDF are mixed evenly to form an inner layer casting solution with a weight percentage of 20wt% to 30wt% of PVDF;
[0009] The outer layer casting liquid and the core liquid are placed in respective reaction kettles and transported to the spinneret through a gear pump. The inner layer casting liquid containing PVDF is extruded by high-temperature shearing and melt mixing through a twin-screw extruder. The three are combined at a three-channel spinneret and extruded through a spinneret plate. The membrane is solidified into a film under the action of a room temperature air section and a cooling bath to form a hollow fiber composite membrane precursor.
[0010] Removing the diluent in the pores of the hollow fiber composite membrane precursor by means of an extractant to obtain the PVDF hollow fiber composite membrane;
[0011] Wherein, the dispersing solvent is one or a mixture of ethanol, isopropanol, dimethylformamide, dimethylacetamide, and dimethyl sulfoxide; the diluent is composed of a solvent and a non-solvent of PVDF, and the solvent is selected from one or a mixture of tributyl citrate, triacetin, propylene carbonate, γ-butyrolactone, and diethylene glycol ethyl ether acetate; the non-solvent is selected from one or a mixture of tetradecanoic acid, hexadecanol, octadecyl alcohol, dioctyl adipate, and dioctyl sebacate;
[0012] Optionally, the outer layer casting liquid and the core liquid are placed in respective reaction kettles and transported to the spinneret through a gear pump, the inner layer casting liquid containing PVDF is extruded by high-temperature shearing and melt mixing through a twin-screw extruder, the three are combined at a three-channel spinneret, and then extruded through a spinneret, comprising:
[0013] The inner layer casting liquid is subjected to high-temperature shearing and melt mixing in the twin-screw extruder to obtain an inner layer casting liquid with a temperature of 200° C. to 250° C., and then extruded, and merged with the outer layer casting liquid and the core liquid at the three-channel spinneret, and extruded through the spinneret; wherein,
[0014] The extrusion pressure is 0.5-1 MPa, and the spinneret temperature is 180-230°C.
[0015] Optionally, the core liquid is selected from one or a mixture of more than one of glycerol, tributyl citrate, glyceryl triacetate, propylene carbonate, γ-butyrolactone and diethylene glycol ethyl ether acetate.
[0016] Optionally, the temperature of the core liquid is 170-270°C.
[0017] Optionally, the room temperature air segment duration is 10-100 ms.
[0018] Optionally, the cooling bath is composed of water and / or ethanol, and the temperature of the cooling bath is 5-50°C.
[0019] Optionally, in the diluent, the weight percentage of the non-solvent is 70 to 95%.
[0020] Optionally, the MXene nanosheets are obtained by:
[0021] Dissolving LiF powder in 5-12 mol / L HCl solution to form an etchant;
[0022] Add MAX to the etchant, stir at 40-60° C. for 10-24 h, transfer to a nitrogen atmosphere for ultrasonication for 1-2 h, and then collect by centrifugation to obtain MXene nanosheets;
[0023] The mass ratio of the LiF to the MAX is 1:1.
[0024] In a second aspect, the present invention provides a PVDF hollow fiber composite membrane obtained by the preparation method described in the first aspect.
[0025] Optionally, the tensile strength of the PVDF hollow fiber composite membrane is: 4.14-4.55 MPa;
[0026] The pure water flux of the PVDF hollow fiber composite membrane is 1286.3-1463.7 L·m -2 ·h -1 ;
[0027] The elongation at break of the PVDF hollow fiber composite membrane is 127.1-151.3%;
[0028] The contamination rate of the PVDF hollow fiber composite membrane is 20.1-33.1%.
[0029] Compared with the prior art, the PVDF hollow fiber composite membrane and the preparation method thereof provided by the present invention have the following advantages:
[0030] The present invention provides a method for preparing PVDF hollow fiber composite membrane, wherein an outer layer casting liquid and a core liquid containing MXene nanosheets are placed in respective reaction kettles and transported to a spinneret through a gear pump, an inner layer casting liquid containing PVDF is sheared and melt-mixed and extruded through a twin-screw extruder at high temperature, the three are combined at a three-channel spinneret, extruded through a spinneret, cured into a membrane precursor, and subjected to extraction treatment, to finally obtain a PVDF hollow fiber composite membrane; the present invention successfully prepares a polyvinylidene fluoride hollow fiber composite membrane through a one-step method, the entire operation process is simple and reliable, and is more conducive to popularization and application.
[0031] In the preparation method provided by the present invention, the outer layer casting liquid and the inner layer casting liquid are hot-melted and tightly adhered under the action of high temperature and extrusion pressure, wherein the dispersion solvent of MXene can effectively dissolve in the solvent of PVDF and quickly vaporize and volatilize at high temperature, so that MXene is stably embedded in the surface of the PVDF membrane to form a firm inorganic MXene layer; the whole process is simple to operate. Compared with the general vacuum filtration (about 0.1MPa) method of loading MXene, the extrusion pressure of the present invention is 0.5-1MPa, which makes the MXene material more firmly combined with the PVDF membrane, and the MXene layer is not easy to fall off, which effectively improves the utilization rate of MXene and the flux and wear resistance of the PVDF hollow fiber composite membrane. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0033] Figure 1 The flowchart of the method for preparing the PVDF hollow fiber composite membrane provided by the embodiment of the present invention is shown;
[0034] Figure 2 The cross-sectional SEM image of the PVDF hollow fiber composite membrane provided in Example 1 of the present invention is shown;
[0035] Figure 3 The SEM image of the inner surface of the PVDF hollow fiber composite membrane provided in Example 1 of the present invention is shown;
[0036] Figure 4 The SEM image of the MXene material of the outer layer of the PVDF hollow fiber composite membrane provided in Example 1 of the present invention is shown;
[0037] Figure 5 The SEM image of the outer side of the cross section of the PVDF hollow fiber composite membrane provided in Example 1 of the present invention is shown;
[0038] Figure 6 The friction-wear curves of the PVDF hollow fiber composite membranes provided in Example 1 of the present invention and Comparative Example 1 are shown. DETAILED DESCRIPTION
[0039] The following examples are provided for a better understanding of the present invention, but are not intended to limit the best mode of implementation, nor to limit the content and protection scope of the present invention. Any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts shall fall within the protection scope of the present invention.
[0040] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the prior art can be used. The reagents and other instruments used without specifying the manufacturer are all conventional reagent products that can be purchased commercially.
[0041] In a first aspect, the present invention provides a method for preparing a PVDF hollow fiber composite membrane. Figure 1 The flow chart of the preparation method of the PVDF hollow fiber composite membrane provided by the embodiment of the present invention is shown as follows: Figure 1 Said preparation method comprises:
[0042] S1, dispersing MXene nanosheets in a dispersing solvent to obtain an outer layer casting solution with a weight percentage of 0.05wt% to 2wt% of MXene nanosheets;
[0043] When this step is implemented, the dispersing solvent is selected from one or a mixture of ethanol, isopropanol, dimethylformamide, dimethylacetamide, and dimethyl sulfoxide;
[0044] S2, mixing the diluent and PVDF evenly to form an inner layer casting solution with a weight percentage of PVDF of 20wt% to 30wt%;
[0045] When this step is implemented, the diluent is composed of a solvent and a non-solvent of PVDF, wherein the solvent can be selected from one or a mixture of tributyl citrate, triacetin, propylene carbonate, γ-butyrolactone, and diethylene glycol ethyl ether acetate, and the weight percentage of the non-solvent is 70-95%, and specifically can be selected from one or a mixture of tetradecanoic acid, hexadecanol, octadecanol, dioctyl adipate, and dioctyl sebacate.
[0046] S3, the outer layer casting liquid and the core liquid are placed in respective reaction kettles and transported to the spinneret through a gear pump, the inner layer casting liquid containing PVDF is extruded by high-temperature shearing and melt mixing of a twin-screw extruder, the three are combined at a three-channel spinneret, extruded through a spinneret, and solidified into a film under the action of a room temperature air section and a cooling bath to form a hollow fiber composite membrane precursor;
[0047] During the implementation of this step, the inner layer casting liquid is subjected to high-temperature shearing and melt mixing in a twin-screw extruder to obtain an inner layer casting liquid with a temperature of 200°C to 250°C, which is then merged with the outer layer casting liquid and the core liquid at a three-channel spinneret. At this time, the temperature of the inner layer casting liquid reaches 200°C to 250°C, and the temperature of the core liquid reaches 170-270°C. When extruded through a spinneret (temperature of 180-230°C), the outer layer casting liquid and the inner layer casting liquid are hot-melted and tightly bonded under the action of high temperature and extrusion pressure, wherein the dispersed solvent in the outer layer casting liquid rapidly vaporizes and evaporates at high temperature, so that the MXene is stably embedded in the surface of the polyvinylidene fluoride membrane to form a firm inorganic MXene layer. Compared with the general method of loading MXene by vacuum filtration (about 0.1 MPa), the extrusion pressure of the present invention is 0.5-1 MPa, which makes the MXene material more firmly bonded to the PVDF membrane, and the MXene layer is not easy to fall off, effectively improving the utilization rate of MXene and the flux and wear resistance of the PVDF hollow fiber composite membrane.
[0048] When this step is implemented, the core liquid is selected from one or a mixture of glycerol, tributyl citrate, triacetin, propylene carbonate, γ-butyrolactone and diethylene glycol ethyl ether acetate; the room temperature air segment duration is 10-100ms; the cooling bath is composed of water and / or ethanol, and the temperature of the cooling bath is 5-50°C.
[0049] S4, removing the diluent in the pores of the hollow fiber composite membrane precursor by means of an extractant to obtain the PVDF hollow fiber composite membrane;
[0050] The embodiment of the present invention adopts the thermally induced phase separation method to prepare PVDF hollow fiber composite membrane, the outer layer casting liquid and the core liquid containing MXene nanosheets are placed in their respective reaction kettles and transported to the spinneret through a gear pump, the inner layer casting liquid containing PVDF is extruded by high-temperature shearing and melt mixing of a twin-screw extruder, the three are merged at the three-channel spinneret, extruded through a spinneret, solidified into a membrane precursor, and extracted to finally obtain a PVDF hollow fiber composite membrane; in this process, the dispersed solvent in the outer layer casting liquid can be miscible with the solvent in the inner layer casting liquid and has a relatively low boiling point, which makes the outer layer casting liquid and the inner layer casting liquid melt and fit tightly under the action of high temperature and extrusion pressure, the dispersed solvent therein rapidly vaporizes and volatilizes at high temperature, and MXene is stably embedded in the surface of the PVDF membrane to form a firm inorganic MXene layer.
[0051] In some embodiments, the MXene nanosheets are obtained by:
[0052] Dissolving LiF powder in 5-12 mol / L HCl solution to form an etchant;
[0053] Add MAX to the etchant, stir at 40-60° C. for 10-24 h, transfer to a nitrogen atmosphere for ultrasonication for 1-2 h, and then collect by centrifugation to obtain MXene nanosheets;
[0054] The mass ratio of the LiF to the MAX is 1:1.
[0055] In a second aspect, the present invention provides a PVDF hollow fiber composite membrane obtained by the preparation method described in the first aspect.
[0056] Optionally, the tensile strength of the PVDF hollow fiber composite membrane is: 4.14-4.55 MPa;
[0057] The pure water flux of the PVDF hollow fiber composite membrane is 1286.3-1463.7 L·m -2 ·h -1 ;
[0058] The elongation at break of the PVDF hollow fiber composite membrane is 127.1-151.3%;
[0059] The contamination rate of the PVDF hollow fiber composite membrane is 20.1-33.1%.
[0060] In order to enable those skilled in the art to more clearly understand the present invention, a PVDF hollow fiber composite membrane and a preparation method thereof according to the present invention are now described in detail through the following examples.
[0061] Example 1
[0062] Preparation of MXene nanosheets: 1g LiF and 50ml 12mol HCl were mixed and stirred in a polytetrafluoroethylene beaker for 0.5h, and then 1g MAX was added to the mixed solution of LiF+HCl and stirred at 40℃ for 24h. Then, the mixture was ultrasonicated for 2h under nitrogen atmosphere and centrifuged at 5000rpm for 1h to obtain MXene nanosheets.
[0063] Preparation of casting solution: adding MXene nanosheets to ethanol to prepare 0.5 g / L MXene outer layer casting solution; uniformly mixing polyvinylidene fluoride, tributyl citrate and dioctyl adipate to obtain inner layer casting solution, wherein the mass fraction of each component in the inner layer casting solution is as follows: 21 wt% polyvinylidene fluoride, 57 wt% tributyl citrate and 22% dioctyl adipate;
[0064] The outer layer casting liquid and the core liquid are placed in respective reaction kettles and transported to the spinneret through a gear pump, the inner layer casting liquid is extruded by high-temperature shearing and melt mixing through a twin-screw extruder, the inner and outer layer casting liquids are combined with the inner core liquid at a three-channel spinneret, and extruded through a spinneret, wherein the melting temperature is 200°C, the extrusion speed is 60m / min, the spinneret temperature is 180°C, the pressure is 0.5MPa, and the core liquid in the spinneret is triacetin, and the temperature is 180°C;
[0065] The hollow fiber was immersed in a room temperature of 25°C for 50ms, and then immersed in a water bath of 40°C for cooling for 3s to achieve solidification and membrane formation to finally obtain a hollow fiber membrane precursor;
[0066] The hollow fiber membrane precursor is immersed in ethanol at 65° C. to remove the diluent, and then the polyvinylidene fluoride hollow fiber composite membrane is obtained after drying.
[0067] Example 2
[0068] The step (2) of Example 1 in which MXene nanosheets are added to ethanol to prepare a 0.5 g / L MXene outer layer casting solution is changed to adding MXene nanosheets to ethanol to prepare a 0.1 g / L MXene outer layer casting solution, and other conditions remain unchanged.
[0069] Example 3
[0070] The step (2) of Example 1 in which MXene nanosheets are added to ethanol to prepare a 0.5 g / L MXene outer layer casting solution is changed to adding MXene nanosheets to ethanol to prepare a 1 g / L MXene outer layer casting solution, and other conditions remain unchanged.
[0071] Example 4
[0072] The step (2) of Example 1 in which the MXene nanosheets are added to ethanol to prepare a 0.5 g / L MXene outer layer casting solution is replaced by adding the MXene nanosheets to dimethylformamide to prepare a 0.5 g / L MXene outer layer casting solution, while other conditions remain unchanged.
[0073] Example 5
[0074] The step (2) of adding MXene nanosheets to ethanol to prepare a 0.5 g / L MXene outer layer casting solution in Example 1 was changed to the step (2) of adding MXene nanosheets to dimethyl sulfoxide to prepare a 0.5 g / L MXene outer layer casting solution, and other conditions remained unchanged.
[0075] Example 6
[0076] The melting temperature in step (3) of Example 1 was changed from 200° C. to 250° C., while other conditions remained unchanged.
[0077] Example 7
[0078] The spinneret temperature in step (3) of Example 1 was changed from 180°C to 230°C, while other conditions remained unchanged.
[0079] Example 8
[0080] The extrusion speed in step (3) in Example 1 was changed from 60 m / min to 30 m / min, while other conditions remained unchanged.
[0081] Example 9
[0082] The polyvinylidene fluoride hollow fiber composite membrane obtained in Example 1 was placed in pure water for 30 minutes of ultrasonic treatment, and its morphology and performance were tested after drying.
[0083] Comparative Example 1
[0084] (1) preparing a casting solution: uniformly mixing polyvinylidene fluoride, tributyl citrate and dioctyl adipate to obtain an inner layer casting solution, wherein the mass fractions of the components in the inner layer casting solution are as follows: 21 wt % of polyvinylidene fluoride, 57 wt % of tributyl citrate and 22 wt % of dioctyl adipate;
[0085] (2) the inner layer casting liquid is extruded by high-temperature shearing and melt mixing through a twin-screw extruder, wherein the melt temperature is 200° C., the extrusion speed is 60 m / min, the spinneret temperature is 180° C., the pressure is 0.5 MPa, and the core liquid in the spinneret is triacetin at a temperature of 180° C.;
[0086] (3) immersing the hollow fiber in a room temperature of 25° C. for 50 ms, and then immersing it in a water bath of 40° C. for cooling for 3 s to achieve solidification and membrane formation to finally obtain a hollow fiber membrane precursor;
[0087] (4) The hollow fiber membrane precursor is immersed in ethanol at 65° C. to remove the diluent, and then dried to obtain a polyvinylidene fluoride hollow fiber membrane.
[0088] Comparative Example 2
[0089] After the MXene outer layer casting solution in Example 1 is prepared, it is loaded on the polyvinylidene fluoride hollow fiber membrane prepared in Comparative Example 1 by filter pressing, and the operating pressure is 0.1 MPa.
[0090] Comparative Example 3
[0091] The concentration of the MXene outer layer casting solution in Example 1 was increased from 0.5 g / L to 1 g / L, and loaded on the hollow fiber membrane prepared in Comparative Example 1 by filter pressing, with an operating pressure of 0.1 MPa.
[0092] Comparative Example 4
[0093] The operating pressure of Comparative Example 2 was changed from 0.1 MPa to 0.5 MPa, while other conditions remained unchanged.
[0094] Comparative Example 5
[0095] The polyvinylidene fluoride hollow fiber composite membrane obtained in Comparative Example 2 was placed in pure water for 30 minutes of ultrasonic treatment, and its morphology and performance were tested after drying.
[0096] The morphology and performance of the polyvinylidene fluoride hollow fiber composite membranes in the examples and comparative examples were characterized by the following test methods:
[0097] 1. Scanning electron microscope image
[0098] The sample membrane was sampled multiple times, and the thickness of the outer MXene layer and the thickness of the microporous main layer were directly measured by scanning electron microscopy. The arithmetic mean was calculated as the thickness. The sampling times were 5 times, and the calculation results are shown in Table 1.
[0099] As an example, Figure 2 The cross-sectional SEM image of the PVDF hollow fiber composite membrane provided in Example 1 of the present invention is shown; Figure 3 The SEM image of the inner surface of the PVDF hollow fiber composite membrane provided in Example 1 of the present invention is shown; Figure 4 The SEM image of the MXene material of the outer layer of the PVDF hollow fiber composite membrane provided in Example 1 of the present invention is shown; Figure 2-4 The SEM image shows that the polyvinylidene fluoride hollow fiber composite membrane prepared by the method of the present invention has a layer of tightly packed MXene nanosheets with a dense crystal cluster structure on its surface, and the inner layer is a transparent sponge-like porous membrane structure. The obtained composite membrane has higher flux and anti-pollution performance.
[0100] Figure 5 The SEM image of the cross section of the PVDF hollow fiber composite membrane provided in Example 1 of the present invention is shown. Figure 5 It can be seen that there is a dense layer at the junction of the outer layer and the inner layer of the polyvinylidene fluoride hollow fiber composite membrane obtained in the present invention. This is because during the preparation process, the inner and outer layer casting liquids are respectively allowed to enter the corresponding channels with the help of a three-channel spinneret, and the dispersed solvent in the outer layer casting liquid can be miscible with the PVDF solvent. The two are tightly bonded by hot melting under the action of high temperature and extrusion pressure at the spinneret, and then the dispersed solvent is rapidly vaporized and volatilized at high temperature. MXene can be more stably embedded in the surface of the inner PVDF membrane, and finally a dense layer is formed through phase separation, thereby further improving the stability of the composite membrane and the ability to retain pollutants.
[0101] 2. Determination of pore size
[0102] At room temperature of 25°C, a pore size analyzer (full-function membrane pore size analyzer, BSD-PBL, Beijing Best Instruments) was used to analyze the pore size.
[0103] 3. Determination of mechanical strength
[0104] The upper and lower ends of the sample film with a length of 50 mm were clamped on a tensile testing machine and tested using an AGS-J electronic universal testing machine. The tensile speed used was 250 mm / min. The tensile strength and elongation at break were measured. The measurement results are shown in Table 1.
[0105] 4. Determination of water contact angle
[0106] Select a sample film with a uniform inner and outer diameter of about 2 cm and place it in a 60℃ oven to dry for 1 hour. Use double-sided tape to stick the dried film flat on the surface of a glass slide. Then place the glass slide on the platform of the contact angle tester, drop about 0.1μL of pure water on the film by the drop method, and measure the static contact angle on the contact angle tester. Each film is measured at 3 different positions, and the arithmetic average of the static contact angle is taken to obtain the water contact angle of the sample film. The measurement results are shown in Table 1.
[0107] 5. Determination of pure water flux
[0108] The sample membrane and the membrane housing are packaged into an assembly, and the membrane assembly is used as a filter membrane. The pure water with a pressure of 0.1 MPa and a water temperature of 25°C is passed through the filter membrane. After stabilization for 30 minutes, the water output (V) at a certain time (t) is collected and measured. The effective area of the filter membrane through which the pure water passes is A. According to J w =Vt / A Calculate the pure water flux corresponding to the sample membrane (L·m -2 ·h -1 ), the measurement results are shown in Table 1.
[0109] 6. Determination of contamination rate
[0110] The hollow fiber membrane and the membrane housing are packaged into a membrane assembly, and the membrane assembly is used as a filter membrane. The pure water with a pressure of 0.1 MPa and a water temperature of 25°C is passed through the filter membrane. After stabilization for 30 minutes (t1), the water production per unit time (V1) is collected and measured. The effective area of the filter membrane through which the pure water passes is A1. According to J w = V1t1 / A1 Calculate the pure water flux corresponding to the hollow fiber membrane (L·m -2 ·h -1 ); The raw material liquid with a pressure of 0.1MPa and a temperature of 25°C is passed through the filter membrane. After the amount of permeate reaches 1000ml, the permeate volume (V2) of a certain time (t2) is collected and measured. The effective area of the filter membrane through which the raw material liquid passes is A2. According to J f= V2t2 / A2 Calculate the flux of bovine serum albumin solution corresponding to the sample membrane (L·m -2 ·h -1 ), wherein the raw material liquid is 1g / L bovine serum albumin solution, according to F=J f / J w ×100% to calculate the contamination rate (%) of the hollow fiber membrane. The measurement results are shown in Table 1.
[0111] 7. Determination of surface mechanical strength
[0112] The friction-wear test in the Keysight G200 nanoindenter was used to characterize the strength of the hollow fiber membrane surface at the nanoscale. The hollow fiber membrane was cut into samples of 1cm*0.3cm in size, fixed on the surface of a glass sheet with double-sided tape and compacted, and then the glass sheet was fixed on the sample stage for testing. A downward pressure of 500μN was applied to the needle, and the sample surface was rubbed 20 times with a length of 200μm. The wear resistance of the membrane surface was judged according to the depth of the needle's penetration.
[0113] The friction-wear experiment can simulate the process of insoluble matter such as sand in water damaging the surface structure of the hollow fiber membrane in operation. As an example, Figure 6 The friction-wear curves of the PVDF hollow fiber composite membranes provided in Example 1 and Comparative Example 1 of the present invention are shown. Figure 6 From the friction-wear curves of Example 1 and Comparative Example 1, it can be found that in the 20 friction tests, the needle penetration depth of the membrane surface prepared in Example 1 is significantly less than that of the pure PVDF in Comparative Example 1. The penetration depth of most positions in Example 1 is almost below 100nm, while the maximum penetration depth in Comparative Example 1 is close to 500nm. This result shows that the hollow fiber composite membrane prepared by the present invention can effectively improve the wear resistance of the membrane surface, reduce the degree of damage to the membrane surface during operation, and improve the service life of the membrane.
[0114] Table 1 Structure and performance characterization results of examples and comparative examples
[0115]
[0116] Analyzing the data in Table 1, we can see that:
[0117] 1. By comparing Examples 1-9 and Comparative Examples 1-5, it can be seen that the preparation method provided by the present invention can improve the pure water flux and anti-pollution property of the polyvinylidene fluoride hollow fiber composite membrane without affecting the mechanical properties of the membrane. The pure water flux and pollution rate can reach 1463.7 L·m -2 ·h -1 and 20.1%, which are significantly better than the composite membrane obtained by conventional filter press method.
[0118] 2. From the comparison of Examples 1-9, it can be seen that the present invention can control the thickness of the MXene layer on the membrane surface by controlling the concentration of MXene in the casting solution, the type of dispersing solvent, the melting temperature, the spinneret temperature and the extrusion speed, thereby obtaining a composite membrane with high flux and low contamination rate.
[0119] 3. By comparing Examples 1 and 9 with Comparative Examples 2 and 5, it can be seen that the thickness of the MXene layer on the surface of the composite membrane obtained by the present invention changes very little after ultrasound, while the thickness of the MXene layer on the surface of the composite membrane obtained by the conventional filter press method is significantly shortened after ultrasound, which indicates that the MXene on the membrane surface has fallen off. The stability of the MXene material on the surface of the composite membrane obtained by the present invention is better than that of the composite membrane obtained by the conventional filter press method, which greatly reduces the risk of MXene material falling off.
[0120] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification.
[0121] For the method embodiments, for the sake of simplicity, they are all described as a series of action combinations, but those skilled in the art should know that the present invention is not limited by the order of the actions described, because according to the present invention, some steps can be performed in other orders or simultaneously. Secondly, those skilled in the art should also know that the embodiments described in the specification are all preferred embodiments, and the actions and components involved are not necessarily required by the present invention.
[0122] The above is a detailed introduction to a PVDF hollow fiber composite membrane and a preparation method thereof provided by the present invention. Specific examples are used herein to illustrate the principles and implementation methods of the present invention. The description of the above embodiments is only used to help understand the method of the present invention and its core idea; at the same time, for a general technician in this field, according to the idea of the present invention, there will be changes in the specific implementation method and application scope. In summary, the content of this specification should not be understood as a limitation on the present invention.
Claims
1. A method for preparing a PVDF hollow fiber composite membrane, characterized in that: The preparation method comprises: Dispersing MXene nanosheets in a dispersing solvent to obtain an outer layer casting solution containing 0.05 wt % to 2 wt % of MXene nanosheets; The diluent and PVDF are mixed evenly to form an inner layer casting solution with a weight percentage of 20wt% to 30wt% of PVDF; The outer layer casting liquid and the core liquid are placed in respective reaction kettles and transported to the spinneret through a gear pump. The inner layer casting liquid containing PVDF is extruded by high-temperature shearing and melt mixing through a twin-screw extruder. The three are combined at a three-channel spinneret and extruded through a spinneret plate. The membrane is solidified into a film under the action of a room temperature air section and a cooling bath to form a hollow fiber composite membrane precursor. Removing the diluent in the pores of the hollow fiber composite membrane precursor by means of an extractant to obtain the PVDF hollow fiber composite membrane; Wherein, the dispersing solvent is selected from one or a mixture of ethanol, isopropanol, dimethylformamide, dimethylacetamide, and dimethyl sulfoxide; The diluent is composed of a solvent and a non-solvent for PVDF, wherein the solvent is selected from one or a mixture of tributyl citrate, triacetin, propylene carbonate, γ-butyrolactone, and diethylene glycol ethyl ether acetate; and the non-solvent is selected from one or a mixture of myristic acid, hexadecanol, octadecanol, dioctyl adipate, and dioctyl sebacate.
2. The preparation method according to claim 1, characterized in that: The outer layer casting liquid and the core liquid are placed in respective reaction kettles and transported to the spinneret through a gear pump, the inner layer casting liquid containing PVDF is extruded by high-temperature shearing and melt mixing through a twin-screw extruder, the three are combined at a three-channel spinneret, and then extruded through a spinneret, including: The inner layer casting liquid is subjected to high-temperature shearing and melt mixing in the twin-screw extruder to obtain an inner layer casting liquid with a temperature of 200° C. to 250° C., and then extruded, and merged with the outer layer casting liquid and the core liquid at the three-channel spinneret, and extruded through the spinneret; wherein, The extrusion pressure is 0.5-1 MPa, and the spinneret temperature is 180-230°C.
3. The preparation method according to claim 1, characterized in that: The core liquid is selected from one or a mixture of glycerol, tributyl citrate, triacetin, propylene carbonate, γ-butyrolactone and diethylene glycol ethyl ether acetate.
4. The preparation method according to claim 1, characterized in that: The temperature of the core liquid is 170-270°C.
5. The preparation method according to claim 1, characterized in that: The room temperature air segment duration is 10-100ms.
6. The preparation method according to claim 1, characterized in that: The cooling bath is composed of water and / or ethanol, and the temperature of the cooling bath is 5-50°C.
7. The preparation method according to claim 1, characterized in that: In the diluent, the weight percentage of the non-solvent is 70-95%.
8. The preparation method according to claim 1, characterized in that: The MXene nanosheets are obtained by the following method: Dissolving LiF powder in 5-12 mol / L HCl solution to form an etchant; Add MAX to the etchant, stir at 40-60° C. for 10-24 h, transfer to a nitrogen atmosphere for ultrasonication for 1-2 h, and then collect by centrifugation to obtain MXene nanosheets; The mass ratio of the LiF to the MAX is 1:
1.
9. A PVDF hollow fiber composite membrane obtained by the preparation method according to any one of claims 1 to 8.
10. The PVDF hollow fiber composite membrane according to claim 9, characterized in that: The tensile strength of the PVDF hollow fiber composite membrane is: 4.14-4.55MPa; The pure water flux of the PVDF hollow fiber composite membrane is 1286.3-1463.7 L·m -2 ·h -1 ; The elongation at break of the PVDF hollow fiber composite membrane is 127.1-151.3%; The contamination rate of the PVDF hollow fiber composite membrane is 20.1-33.1%.