Preparation method of zirconium oxide-titanium oxide ceramic composite nanofiltration membrane
By employing a sol-microwave hydrothermal method and low-temperature calcination technology, the thermal stability and cracking problems of ceramic nanofiltration membranes were solved, and high-quality zirconium oxide-titanium oxide nanofiltration membranes were prepared, improving their separation performance and reliability at high temperatures.
Patent Information
- Application Number
- CN202410964175.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-11-08
AI Technical Summary
Existing sol-gel methods for preparing ceramic nanofiltration membranes suffer from reduced thermal stability and susceptibility to cracking, leading to decreased membrane performance at high temperatures and affecting their reliability and stability in industrial applications.
Zirconia-titanium oxide composite nanosol was prepared by sol-microwave hydrothermal method, and plasticizer and binder were added. Zirconia-titanium oxide nanofiltration membrane was prepared by low-temperature calcination and combined with microporous alumina ceramic membrane support to form a defect-free membrane layer.
A zirconia-titanium oxide nanosolution with uniform particle size was prepared in a short time. A defect-free, high-quality zirconia-titanium oxide nanofiltration membrane was prepared by low-temperature calcination, which improved the thermal stability and separation performance of the membrane.
Smart Images

Figure CN118904105A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of nanofiltration membrane preparation, and specifically relates to a method for preparing a zirconium oxide-titanium oxide ceramic composite nanofiltration membrane. Background Art
[0002] The sol-gel method is a key technology in the preparation of ceramic nanofiltration membranes, and is valued for its simplicity of preparation, ease of large-scale production, and flexible parameter control. This method can accurately control the chemical composition and pore structure of the ceramic membrane and produce nanofiltration membranes with specific separation properties, which are suitable for water treatment, chemical industry, and other fields that require high-precision separation technology.
[0003] However, there are some technical challenges in the process of preparing titanium dioxide nano-solutions by sol-gel method. The high shrinkage of the material during calcination is one of the main problems, which may cause cracks and defects in the film layer. In order to obtain a uniform and defect-free film layer, multiple coatings are usually required, which undoubtedly increases the complexity and cost of the production steps.
[0004] In addition, pure TiO 2 Porous ceramic membranes have limitations in temperature control. When the operating temperature exceeds its heat resistance limit, the micropores of the membrane may close, resulting in a decrease in thermal stability. This decrease directly affects the separation performance of the membrane, limiting its application in a wider temperature range. At high temperatures, the structure of the membrane material may change, affecting its long-term stability and efficiency.
[0005] The lack of thermal stability is also accompanied by the problem of easy cracking of the membrane layer. This physical damage will reduce the service life and separation efficiency of the membrane. Once cracking occurs, the integrity and separation function of the membrane layer will be irreversibly damaged. In industrial applications, this damage is usually difficult to repair and may require the replacement of the entire membrane, increasing operating costs and affecting production efficiency.
[0006] In general, the sol-gel method has significant advantages in the preparation of ceramic nanofiltration membranes, but the problems of reduced thermal stability and easy cracking are important challenges that this technology needs to face. The existence of these problems limits the full play of material performance and also affects the reliability and stability of ceramic nanofiltration membranes in specific industrial applications. Summary of the invention
[0007] The present invention aims to overcome the defects of the prior art and provide a method for preparing a zirconium oxide-titanium oxide ceramic composite nanofiltration membrane.
[0008] The technical solution of the present invention is as follows:
[0009] A method for preparing a zirconium oxide-titanium oxide ceramic composite nanofiltration membrane comprises the following steps:
[0010] (1) adding glycerol to a mixed solution containing an organic zirconium alkoxide with a concentration of 0.05-0.5 mol / L and an organic titanium alkoxide with a concentration of 0.05-0.5 mol / L, performing a hydrolysis reaction at 60-80° C. with stirring for 2-3 hours, then performing solid-liquid separation, re-dispersing the solid in water, adding nitric acid for peptization and making the pH value of the peptized solution 1-2, to obtain a Zr-Ti composite sol; in the above mixed solution, the molar ratio of Zr to Ti is 1:5-10;
[0011] (2) subjecting the Ti-Zr composite sol obtained in step (1) to ultrasonic treatment, then adding EDTA, stirring evenly, placing it in a microwave hydrothermal reaction device with a filling degree of 70%, and keeping the reaction at a pressure of 0.5 MPa for 2 h. After cooling, a Zr-Ti composite nano-solution with uniform particle size is obtained;
[0012] (3) adding a plasticizer and a binder to the Zr-Ti composite nano-solution obtained in step (2), and then adding silicone defoamer, mixing, and obtaining a coating solution; the plasticizer is polyethylene glycol with a weight average molecular weight of 350-450, and the binder is a cellulose compound with a molecular weight of 6000-10000;
[0013] (4) Apply the coating liquid prepared in step (3) on the porous alumina ceramic membrane support, raise the temperature to 80-120°C at a humidity of 30-40%, and then keep it warm and dry for 2-5 hours, then raise the temperature to 350-600°C and keep it warm and calcine for 2-5 hours, and cool it to obtain the product.
[0014] In a preferred embodiment of the present invention, the organic zirconium alkoxide is zirconium isopropoxide or zirconium n-butoxide.
[0015] More preferably, the organic zirconium alkoxide is zirconium isopropoxide.
[0016] In a preferred embodiment of the present invention, the organic titanium alkoxide is titanium isopropoxide or titanium n-butoxide.
[0017] More preferably, the organic titanium alkoxide is titanium n-butoxide.
[0018] In a preferred embodiment of the present invention, the cellulose compound is hydroxymethyl cellulose, hydroxyethyl cellulose or hydroxypropyl cellulose.
[0019] More preferably, the cellulose compound is hydroxymethyl cellulose.
[0020] In a preferred embodiment of the present invention, the organic zirconium alkoxide is zirconium isopropoxide, the organic titanium alkoxide is titanium n-butoxide, and the cellulose compound is hydroxymethyl cellulose.
[0021] In a preferred embodiment of the present invention, in the step (2), the EDTA is added to a final concentration of 0.5-2wt%; in the step (3), the plasticizer and the binder are added to a final concentration of 3-10wt% and 0.1-1wt%, respectively, and the silicone defoamer is added to a final concentration of 0.01-0.1wt%.
[0022] Further preferably, the step (4) is: apply the coating liquid prepared in step (3) on the porous alumina ceramic membrane support, heat it to 80-120°C at a rate of 1-3°C / min at a humidity of 30-40%, and then keep it warm and dry for 2-5h, then heat it to 350-600°C at a rate of 1-5°C / min, keep it warm and calcine for 2-5h, and cool it to obtain.
[0023] The beneficial effects of the present invention are:
[0024] 1. The present invention uses a sol-microwave hydrothermal method to prepare a zirconium oxide-titania composite nano-solution, and obtains a zirconium oxide-titania nanofiltration membrane layer by adding a plasticizer and a binder and calcining at a low temperature.
[0025] 2. The present invention prepares zirconium oxide-titania sol by sol-microwave hydrothermal method, prepares zirconium oxide-titania nano solution with uniform particle size in a short reaction time, and prepares defect-free, high-quality zirconium oxide-titania nanofiltration membrane by dipping, drying and calcining steps. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 The following are scanning electron microscope photographs of the zirconium oxide-titania ceramic nanofiltration membranes prepared in Examples 1 to 3 of the present invention.
[0027] Figure 2 This is a scanning electron microscope photograph of the composite ceramic nanofiltration membrane prepared in Comparative Example 1 of the present invention.
[0028] Figure 3 This is a scanning electron microscope photograph of the composite ceramic nanofiltration membrane prepared in Comparative Example 2 of the present invention.
[0029] Figure 4 This is a scanning electron microscope photograph of the composite ceramic nanofiltration membrane prepared in Comparative Example 3 of the present invention. DETAILED DESCRIPTION
[0030] The technical solution of the present invention is further illustrated and described below through specific implementation modes in combination with the accompanying drawings.
[0031] Example 1
[0032] (1) adding glycerol with a final concentration of 0.05 mol / L to a mixed solution containing zirconium isopropoxide with a concentration of 0.05 mol / L and titanium n-butoxide with a concentration of 0.3 mol / L, performing a hydrolysis reaction at 60° C. for 2 h while stirring, then filtering to separate the solid and liquid, taking the filter cake layer and redispersing it in water, adding nitric acid to perform peptization and making the pH value of the peptized solution 1-2, to obtain a Zr-Ti composite sol;
[0033] (2) subjecting the Ti-Zr composite sol obtained in step (1) to ultrasonic treatment, then adding 1wt% EDTA (ethylenediaminetetraacetic acid), stirring evenly, placing in a microwave hydrothermal reaction device with a filling degree of 70%, and keeping the reaction at a pressure of 0.5MPa for 2h, and obtaining a Zr-Ti composite nano-solution with uniform particle size after cooling;
[0034] (3) adding PEG-400 and hydroxymethyl cellulose with a molecular weight of 6000-10000 to the Zr-Ti composite nano-solution prepared in step (2), and making the final concentrations of PEG-400 and hydroxymethyl cellulose 5wt% and 0.5wt%, respectively, and then adding silicone defoamer BYK028 to a final concentration of 0.05wt%, and mixing well to prepare a coating solution;
[0035] (4) applying the coating liquid prepared in step (3) to a porous alumina ceramic membrane support having an average pore size of 5 nm, heating the membrane to 100° C. at a rate of 2° C. / min at a humidity of 40%, drying the membrane at this temperature for 3 h, then heating the membrane to 500° C. at a rate of 2° C. / min, calcining the membrane at this temperature for 3 h, and cooling the membrane to obtain the following: Figure 1 The zirconia-titania ceramic composite nanofiltration membrane shown. Under the test conditions of room temperature and 0.6 MPa, the zirconia-titania ceramic composite nanofiltration membrane has a retention rate of 94% for 0.1% PEG1000 solution and a flux of 62 LHM.
[0036] Example 2
[0037] (1) adding glycerol with a final concentration of 0.05 mol / L to a mixed solution containing zirconium isopropoxide with a concentration of 0.05 mol / L and titanium n-butoxide with a concentration of 0.3 mol / L, performing a hydrolysis reaction at 60° C. for 2 h while stirring, then filtering to separate the solid and liquid, taking the filter cake layer and redispersing it in water, adding nitric acid to perform peptization and making the pH value of the peptized solution 1-2, to obtain a Zr-Ti composite sol;
[0038] (2) subjecting the Ti-Zr composite sol obtained in step (1) to ultrasonic treatment, then adding 1wt% EDTA (ethylenediaminetetraacetic acid), stirring evenly, placing in a microwave hydrothermal reaction device with a filling degree of 70%, keeping the temperature at 1MPa for 2h, and obtaining a Zr-Ti composite nano-solution with uniform particle size after cooling;
[0039] (3) adding PEG-400 and hydroxymethyl cellulose with a molecular weight of 6000-10000 to the Zr-Ti composite nano-solution prepared in step (2), and making the final concentrations of PEG-400 and hydroxymethyl cellulose 5wt% and 0.5wt%, respectively, and then adding silicone defoamer BYK028 to a final concentration of 0.05wt%, and mixing well to prepare a coating solution;
[0040] (4) applying the coating liquid prepared in step (3) to a porous alumina ceramic membrane support having an average pore size of 5 nm, heating the membrane to 100° C. at a rate of 2° C. / min at a humidity of 40%, drying the membrane at this temperature for 3 h, then heating the membrane to 500° C. at a rate of 2° C. / min, calcining the membrane at this temperature for 3 h, and cooling the membrane to obtain the following: Figure 1 The zirconia-titania ceramic composite nanofiltration membrane shown. Under the test conditions of room temperature and 0.6 MPa, the zirconia-titania ceramic composite nanofiltration membrane has a retention rate of 92% for 0.1% PEG1000 solution and a flux of 68 LHM.
[0041] Example 3
[0042] (1) adding glycerol with a final concentration of 0.05 mol / L to a mixed solution containing zirconium isopropoxide with a concentration of 0.05 mol / L and titanium n-butoxide with a concentration of 0.3 mol / L, performing a hydrolysis reaction at 60° C. for 2 h while stirring, then filtering to separate the solid and liquid, taking the filter cake layer and redispersing it in water, adding nitric acid to perform peptization and making the pH value of the peptized solution 1-2, to obtain a Zr-Ti composite sol;
[0043] (2) subjecting the Ti-Zr composite sol obtained in step (1) to ultrasonic treatment, then adding 1 wt% EDTA (ethylenediaminetetraacetic acid), stirring evenly, placing in a microwave hydrothermal reaction device with a filling degree of 70%, keeping the temperature at 2 MPa for 2 h, and obtaining a Zr-Ti composite nano-solution with uniform particle size after cooling;
[0044] (3) adding PEG-400 and hydroxymethyl cellulose with a molecular weight of 6000-10000 to the Zr-Ti composite nano-solution prepared in step (2), and making the final concentrations of PEG-400 and hydroxymethyl cellulose 5wt% and 0.5wt%, respectively, and then adding silicone defoamer BYK028 to a final concentration of 0.05wt%, and mixing well to prepare a coating solution;
[0045] (4) applying the coating liquid prepared in step (3) to a porous alumina ceramic membrane support having an average pore size of 5 nm, heating the membrane to 100° C. at a rate of 2° C. / min at a humidity of 40%, drying the membrane at this temperature for 3 h, then heating the membrane to 500° C. at a rate of 2° C. / min, calcining the membrane at this temperature for 3 h, and cooling the membrane to obtain the following: Figure 1 The zirconia-titania ceramic composite nanofiltration membrane shown. Under the test conditions of room temperature and 0.6 MPa, the zirconia-titania ceramic composite nanofiltration membrane has a retention rate of 90% and a flux of 72 LHM for 0.1% PEG1000 solution.
[0046] Comparative Example 1
[0047] (1) adding glycerol with a final concentration of 0.05 mol / L to a mixed solution containing zirconium isopropoxide with a concentration of 0.05 mol / L and titanium n-butoxide with a concentration of 0.3 mol / L, performing a hydrolysis reaction at 60° C. for 2 h while stirring, then filtering to separate the solid and liquid, taking the filter cake layer and redispersing it in water, adding nitric acid to perform peptization and making the pH value of the peptized solution 1-2, to obtain a Zr-Ti composite sol;
[0048] (2) adding PEG-400 and hydroxymethyl cellulose with a molecular weight of 6000-10000 to the Zr-Ti composite sol prepared in step (1), and making the final concentrations of PEG-400 and hydroxymethyl cellulose 5wt% and 0.5wt%, respectively, and then adding organosilicon defoamer BYK028 to a final concentration of 0.05wt%, mixing, and preparing a coating solution;
[0049] (3) applying the coating liquid prepared in step (2) to a porous alumina ceramic membrane support having an average pore size of 5 nm, heating the membrane to 100° C. at a rate of 2° C. / min at a humidity of 40%, drying the membrane at this temperature for 3 h, then heating the membrane to 500° C. at a rate of 2° C. / min, calcining the membrane at this temperature for 3 h, and cooling the membrane to obtain the following: Figure 2 The composite ceramic nanofiltration membrane shown. Under the test conditions of room temperature and 0.69 MPa, the rejection rate of 0.1% PEG1000 solution is 5% and the flux is 102 LHM.
[0050] Comparative Example 2
[0051] (1) Add 0.05 mol of glycerol to 0.05 mol of zirconium isopropoxide and 0.3 mol of titanium n-butoxide solution, add 1 L of deionized water for hydrolysis, react for 2 h at 60 ° C with stirring, and obtain a Zr-Ti composite solution;
[0052] (2) subjecting the Ti-Zr composite solution obtained in step (1) to ultrasonic treatment, then adding 1wt% EDTA (ethylenediaminetetraacetic acid), stirring evenly, placing in a microwave hydrothermal reaction device, with a filling degree of 70%, keeping the temperature at 0.5MPa for 2h, and cooling to obtain a Zr-Ti composite nano-solution with uniform particle size;
[0053] (3) adding PEG-400 and hydroxymethyl cellulose with a molecular weight of 6000-10000 to the Zr-Ti composite sol prepared in step (2), and making the final concentrations of PEG-400 and hydroxymethyl cellulose 5wt% and 0.5wt%, respectively, and then adding organosilicon defoamer BYK028 to a final concentration of 0.05wt%, and mixing well to prepare a coating solution;
[0054] (4) applying the coating liquid prepared in step (3) to a porous alumina ceramic membrane support having an average pore size of 5 nm, heating the membrane to 100° C. at a rate of 2° C. / min at a humidity of 40%, drying the membrane at this temperature for 3 h, then heating the membrane to 500° C. at a rate of 2° C. / min, calcining the membrane at this temperature for 3 h, and cooling the membrane to obtain the following: Figure 3 The composite ceramic nanofiltration membrane shown in the figure has an uneven surface and a small amount of cracks, that is, the particles that have not been prepared by the sol-gel method are subjected to microwave hydrothermal treatment, and the particles are larger, and the average pore size obtained reaches 10-20 nm, as shown in Table 1. Under the test conditions of room temperature and 0.69 MPa, the retention rate of 0.1% PEG1000 solution is 15%, and the flux is 132 LHM.
[0055] Comparative Example 3
[0056] (1) adding glycerol with a final concentration of 0.05 mol / L to a mixed solution containing zirconium isopropoxide with a concentration of 0.05 mol / L and titanium n-butoxide with a concentration of 0.3 mol / L, performing a hydrolysis reaction at 60° C. for 2 h while stirring, then filtering to separate the solid and liquid, taking the filter cake layer and redispersing it in water, adding nitric acid to perform peptization and making the pH value of the peptized solution 1-2, to obtain a Zr-Ti composite sol;
[0057] (2) The Ti-Zr composite solution obtained in step (1) is subjected to ultrasonic treatment, and then 1 wt% EDTA (ethylenediaminetetraacetic acid) is added, stirred evenly, and placed in a hydrothermal reactor with a filling degree of 70%, and kept at 200° C. for 10 h. After cooling, a Zr-Ti composite nano-solution with uniform particle size is obtained;
[0058] (3) adding PEG-400 and hydroxymethyl cellulose with a molecular weight of 6000-10000 to the Zr-Ti composite sol prepared in step (2), and making the final concentrations of PEG-400 and hydroxymethyl cellulose 5wt% and 0.5wt%, respectively, and then adding organosilicon defoamer BYK028 to a final concentration of 0.05wt%, and mixing well to prepare a coating solution;
[0059] (4) applying the coating liquid prepared in step (3) to a porous alumina ceramic membrane support having an average pore size of 5 nm, heating the membrane to 100° C. at a rate of 2° C. / min at a humidity of 40%, drying the membrane at this temperature for 3 h, then heating the membrane to 500° C. at a rate of 2° C. / min, calcining the membrane at this temperature for 3 h, and cooling the membrane to obtain the following: Figure 4 The composite ceramic nanofiltration membrane shown has a small amount of defects on its surface, that is, it is not subjected to microwave hydrothermal treatment, but directly subjected to hydrothermal treatment, and the average pore size of the obtained membrane layer is 7-10 nm, as shown in Table 1. Under the test conditions of room temperature and 0.69 MPa, the retention rate of 0.1% PEG1000 solution is 75%, and the flux is 48 LHM.
[0060] Comparative Example 4
[0061] (1) adding glycerol with a final concentration of 0.05 mol / L to a titanium n-butoxide solution with a concentration of 0.3 mol / L, performing a hydrolysis reaction at 60° C. with stirring for 2 h, then filtering to separate the solid and liquid, taking the filter cake layer and redispersing it in water, adding nitric acid to perform peptization and making the pH value of the peptized solution 1-2, to obtain a Ti sol;
[0062] (2) subjecting the Ti sol obtained in step (1) to ultrasonic treatment, then adding 1 wt % EDTA (ethylenediaminetetraacetic acid), stirring evenly, placing in a microwave hydrothermal reaction device with a filling degree of 70%, and keeping the reaction at a pressure of 0.5 MPa for 2 h, and obtaining a Ti nano-solution with uniform particle size after cooling;
[0063] (3) adding PEG-400 and hydroxymethyl cellulose with a molecular weight of 6000-10000 to the Ti nano-solution prepared in step (2), and making the final concentrations of PEG-400 and hydroxymethyl cellulose 5wt% and 0.5wt%, respectively, and then adding silicone defoamer BYK028 to a final concentration of 0.05wt%, and mixing well to prepare a coating solution;
[0064] (4) The coating liquid prepared in step (3) is applied to a porous alumina ceramic membrane support having an average pore size of 5 nm, and the temperature is raised to 100° C. at a rate of 2° C. / min at a humidity of 40%, and the temperature is kept warm and dried for 3 hours, and then the temperature is raised to 500° C. at a rate of 2° C. / min, and the temperature is kept warm and calcined for 3 hours, and cooled to obtain a titanium oxide ceramic nanofiltration membrane. The titanium oxide ceramic nanofiltration membrane has a retention rate of 91% for a 0.1% PEG1000 solution and a flux of 50 LHM under the test conditions of room temperature and 0.6 MPa.
[0065] Table 1
[0066]
[0067] The above description is only a preferred embodiment of the present invention, and therefore cannot be used to limit the scope of the present invention. That is, equivalent changes and modifications made according to the patent scope of the present invention and the contents of the specification should still fall within the scope of the present invention.
Claims
1. A method for preparing a zirconium oxide-titania ceramic composite nanofiltration membrane, characterized in that: The steps include: (1) adding glycerol to a mixed solution containing an organic zirconium alkoxide with a concentration of 0.05-0.5 mol / L and an organic titanium alkoxide with a concentration of 0.05-0.5 mol / L, performing a hydrolysis reaction at 60-80° C. with stirring for 2-3 hours, then performing solid-liquid separation, re-dispersing the solid in water, adding nitric acid for peptization and making the pH value of the peptized solution 1-2, to obtain a Zr-Ti composite sol; in the above mixed solution, the molar ratio of Zr to Ti is 1:5-10; (2) subjecting the Ti-Zr composite sol obtained in step (1) to ultrasonic treatment, then adding EDTA, stirring evenly, placing it in a microwave hydrothermal reaction device with a filling degree of 70%, and keeping the reaction at a pressure of 0.5 MPa for 2 h. After cooling, a Zr-Ti composite nano-solution with uniform particle size is obtained; (3) adding a plasticizer and a binder to the Zr-Ti composite nano-solution obtained in step (2), and then adding silicone defoamer, mixing, and obtaining a coating solution; the plasticizer is polyethylene glycol with a weight average molecular weight of 350-450, and the binder is a cellulose compound with a molecular weight of 6000-10000; (4) Apply the coating liquid prepared in step (3) on the porous alumina ceramic membrane support, raise the temperature to 80-120°C at a humidity of 30-40%, and then keep it warm and dry for 2-5 hours, then raise the temperature to 350-600°C and keep it warm and calcine for 2-5 hours, and cool it to obtain the product.
2. The preparation method according to claim 1, characterized in that: The organic zirconium alkoxide is zirconium isopropoxide or zirconium n-butoxide.
3. The preparation method according to claim 2, characterized in that: The organic zirconium alkoxide is zirconium isopropoxide.
4. The preparation method according to claim 1, characterized in that: The organic titanium alkoxide is titanium isopropoxide or titanium n-butoxide.
5. The preparation method according to claim 4, characterized in that: The organic titanium alkoxide is titanium n-butoxide.
6. The preparation method according to claim 1, characterized in that: The cellulose compound is hydroxymethyl cellulose, hydroxyethyl cellulose or hydroxypropyl cellulose.
7. The preparation method according to claim 6, characterized in that: The cellulose compound is hydroxymethyl cellulose.
8. The preparation method according to claim 1, characterized in that: The organic zirconium alkoxide is zirconium isopropoxide, the organic titanium alkoxide is titanium n-butoxide, and the cellulose compound is hydroxymethyl cellulose.
9. The preparation method according to any one of claims 1 to 8, characterized in that: In the step (2), the EDTA is added to a final concentration of 0.5-2wt%; in the step (3), the plasticizer and the binder are added to a final concentration of 3-10wt% and 0.1-1wt%, respectively, and the organosilicon defoamer is added to a final concentration of 0.01-0.1wt%.
10. The preparation method according to claim 1, characterized in that: The step (4) is as follows: applying the coating liquid obtained in the step (3) on the porous alumina ceramic membrane support, heating the temperature to 80-120°C at a rate of 1-3°C / min at a humidity of 30-40%, and then drying the temperature for 2-5 hours, then heating the temperature to 350-600°C at a rate of 1-5°C / min, calcining the temperature for 2-5 hours, and cooling the temperature to obtain the product.