Preparation method of high-flux zirconia ceramic ultrafiltration membrane
By using a process of combining inorganic zirconium salt solution and microwave hydrothermal method in the preparation of ceramic ultrafiltration membranes, the problems of production efficiency and cost control in the prior art are solved, and the rapid and rapid zirconia ceramic ultrafiltration membranes are achieved. Economical preparation improves the quality and production competitiveness of the membrane layer.
Patent Information
- Application Number
- CN202410964179.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-11-08
Smart Images

Figure CN118904106A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of ultrafiltration membrane preparation, and specifically relates to a method for preparing a high-flux zirconia ceramic ultrafiltration membrane. Background Art
[0002] Ceramic membrane materials, with their excellent mechanical strength, chemical stability, long service life and outstanding anti-fouling ability, have established their position as ideal separation membrane materials in the field of industrial filtration. This typical inorganic membrane material performs well in handling challenging fluids and meeting demanding filtration requirements.
[0003] In the preparation process of ceramic ultrafiltration membrane, there are a variety of process technologies to choose from, including solid particle sintering method, sol-gel method, chemical vapor deposition method, hydrothermal method and thermal decomposition method, etc. Sol-gel method and hydrothermal method have been widely used in actual production due to their respective advantages.
[0004] One of the main limitations of the sol-gel method in the preparation of ceramic membranes is production efficiency. This method usually requires multiple coating and curing steps to form a membrane layer with the desired thickness. After each coating, you must wait for the sol to transform into a gel, which is not only time-consuming but also very sensitive to environmental conditions such as humidity and temperature. In addition, multiple coatings increase the chance of errors in the production process, which may result in uneven or defective membrane layers, which in turn affects the performance and consistency of the membrane.
[0005] Although the hydrothermal method can produce ceramic membranes with good crystallinity and mechanical strength, it also faces challenges in production efficiency. Hydrothermal synthesis needs to be maintained for a long time under high temperature and high pressure conditions, which places high demands on equipment and consumes relatively large amounts of energy. In addition, the post-processing steps of the hydrothermal method, including removing the product from the reactor, washing and drying, are also labor-intensive, limiting the overall production efficiency.
[0006] There is also the problem of cost control in the preparation process of sol-gel and hydrothermal methods. The chemical reagents and catalysts required for sol-gel methods are often expensive, while the special equipment and energy consumption required for hydrothermal methods will also increase production costs. These factors work together to limit the application of these methods in large-scale production.
[0007] In general, although the sol-gel method and hydrothermal method have significant advantages in the preparation of ceramic ultrafiltration membranes, their limitations in production efficiency cannot be ignored. Low production efficiency not only increases manufacturing costs, but also limits the competitiveness of these technologies in industrial-scale production. While pursuing more efficient production processes and reducing costs, finding and developing new preparation technologies or improving existing processes is the key to future development. Summary of the invention
[0008] The present invention aims to overcome the defects of the prior art and provide a method for preparing a high-flux zirconium oxide ceramic ultrafiltration membrane.
[0009] The technical solution of the present invention is as follows:
[0010] A method for preparing a high-flux zirconium oxide ceramic ultrafiltration membrane comprises the following steps:
[0011] (1) slowly adding an ammonia solution to an inorganic zirconium salt solution at 75-85° C. with stirring to adjust the pH value to between 9 and 11, performing solid-liquid separation, redispersing the obtained solid in water, and then adding nitric acid or hydrochloric acid for peptization to adjust the pH value to between 3 and 4 to obtain a transparent zirconium sol; the inorganic zirconium salt in the inorganic zirconium salt solution is selected from zirconium chloride, zirconium oxychloride and zirconium oxysulfate;
[0012] (2) adding glycerol with a final concentration of 0.8-1.2 wt % to the zirconium sol obtained in step (1), stirring evenly, placing in a microwave hydrothermal reactor, and performing microwave hydrothermal reaction at a pressure of 0.5-2 MPa for 1-2 h;
[0013] (3) cooling the material obtained in step (2) naturally and then subjecting it to shearing or ultrasonic treatment to obtain a translucent zirconium oxide sol;
[0014] (4) adding polyvinyl alcohol and hydroxyethyl cellulose to the zirconium oxide sol obtained in step (3), mixing thoroughly, and then adding an organosilicon defoamer to prepare a uniformly dispersed coating liquid;
[0015] (5) Apply the coating liquid obtained in step (4) on the porous ceramic membrane support, then dry at 80-120°C for 2-5h, then program the temperature to 500-800°C and keep it for 2-5h, and finally cool it naturally to obtain a zirconia ceramic ultrafiltration membrane.
[0016] In a preferred embodiment of the present invention, in step (4), the final concentration of polyvinyl alcohol is 2-5 wt%.
[0017] In a preferred embodiment of the present invention, in step (4), the final concentration of hydroxyethyl cellulose is 0.1-0.3 wt %.
[0018] In a preferred embodiment of the present invention, in step (4), the final concentration of the organosilicon defoaming agent is 0.01-1 wt %.
[0019] In a preferred embodiment of the present invention, in step (4), the final concentration of polyvinyl alcohol is 2-5 wt %, the final concentration of hydroxyethyl cellulose is 0.1-0.3 wt %, and the final concentration of the organosilicon defoamer is 0.01-1 wt %.
[0020] Further preferably, in the step (4), the final concentration of polyvinyl alcohol is 2 wt %, the final concentration of hydroxyethyl cellulose is 0.1 wt %, and the final concentration of the organosilicon defoaming agent is 0.01 wt %.
[0021] In a preferred embodiment of the present invention, in step (1), the concentration of the zirconium oxychloride solution is 0.4-0.6 mol / L, and the concentration of the ammonia solution is 4-6 mol / L.
[0022] Further preferably, in step (1), the concentration of the zirconium oxychloride solution is 0.5 mol / L, and the concentration of the ammonia solution is 5 mol / L.
[0023] In a preferred embodiment of the present invention, in the step (5), the drying temperature rise rate is 1-3°C / min.
[0024] Further preferably, in step (5), the rate of programmed temperature increase is 1-5°C / min.
[0025] The beneficial effects of the present invention are as follows: the present invention uses inorganic zirconium salt as a raw material, firstly prepares zirconium sol as a precursor by a sol-gel method, adds glycerol as a dispersant, and then prepares a zirconium oxide nano-solution by a microwave hydrothermal method, then adds polyvinyl alcohol, hydroxyethyl cellulose and an organosilicon defoaming agent to prepare a coating liquid, which is dip-coated on a porous ceramic membrane, and after drying and calcining, a zirconium oxide ultrafiltration membrane layer is obtained, which provides a novel and quick way to prepare a high-throughput zirconium oxide ceramic ultrafiltration membrane. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 This is a scanning electron microscope photograph of the zirconia ceramic ultrafiltration membrane prepared in Example 1 of the present invention.
[0027] Figure 2 This is a scanning electron microscope photograph of the comparative zirconia ceramic ultrafiltration membrane prepared in Comparative Example 1 of the present invention.
[0028] Figure 3 This is a scanning electron microscope photograph of the comparative zirconia ceramic ultrafiltration membrane prepared in Comparative Example 2 of the present invention. DETAILED DESCRIPTION
[0029] The technical solution of the present invention is further illustrated and described below through specific implementation modes in combination with the accompanying drawings.
[0030] Example 1
[0031] (1) At 80°C and under stirring conditions, a 5 mol / L ammonia aqueous solution is slowly added to a 0.5 mol / L zirconium oxychloride solution to adjust its pH value to between 9 and 11, and then the solution is filtered. The obtained solid is redispersed in water, and then 1 mol / L nitric acid or hydrochloric acid is added for peptization to adjust its pH value to between 3 and 4, thereby obtaining a transparent zirconium sol.
[0032] (2) Add glycerol with a final concentration of 1 wt % to the zirconium sol obtained in step (1), and then put it into a microwave hydrothermal reactor for microwave hydrothermal reaction at a pressure of 0.5 MPa for 2 h.
[0033] (3) The material obtained in step (2) is naturally cooled and then subjected to ultrasonic treatment to obtain a translucent zirconium oxide sol.
[0034] (4) Add 2 wt% polyvinyl alcohol and 0.1 wt% hydroxyethyl cellulose to the zirconium oxide sol obtained in step (3), mix thoroughly, and then add 0.01 wt% organosilicon defoamer BYK028 to prepare a uniformly dispersed coating liquid.
[0035] (5) Apply the coating solution prepared in step (4) to a porous ceramic membrane support having an average pore size of 0.1 μm by dipping. Dry at 120°C for 5 h, with a heating rate of 3°C / min, then heat to 700°C at a rate of 3°C / min, keep the temperature constant for 3 h, and then cool naturally to obtain the following: Figure 1 The zirconia ceramic ultrafiltration membrane shown has a complete and defect-free membrane layer.
[0036] The zirconia ceramic ultrafiltration membrane prepared in this example has a retention rate of 97% for 1 g / L bovine serum albumin (molecular weight 67,000) and a flux of 402 LHM under the test conditions of room temperature and 0.1 MPa.
[0037] Example 2
[0038] (1) At 80°C and under stirring conditions, a 5 mol / L ammonia aqueous solution is slowly added to a 0.5 mol / L zirconium oxychloride solution to adjust its pH value to between 9 and 11, and then the solution is filtered. The obtained solid is redispersed in water, and then 1 mol / L nitric acid or hydrochloric acid is added for peptization to adjust its pH value to between 3 and 4, thereby obtaining a transparent zirconium sol.
[0039] (2) Add glycerol with a final concentration of 1 wt % to the zirconium sol obtained in step (1), and then put it into a microwave hydrothermal reactor to carry out microwave hydrothermal reaction at a pressure of 1 MPa for 2 h.
[0040] (3) The material obtained in step (2) is naturally cooled and then subjected to ultrasonic treatment to obtain a translucent zirconium oxide sol.
[0041] (4) Add 2 wt% polyvinyl alcohol and 0.1 wt% hydroxyethyl cellulose to the zirconium oxide sol obtained in step (3), mix thoroughly, and then add 0.01 wt% organosilicon defoamer BYK028 to prepare a uniformly dispersed coating liquid.
[0042] (5) Apply the coating liquid prepared in step (4) to a porous ceramic membrane support having an average pore size of 0.1 μm by dipping, dry at 120° C. for 5 h, and heat at a rate of 3° C. / min, then heat to 700° C. at a rate of 3° C. / min, keep constant temperature for 3 h, and then cool naturally to obtain a zirconium oxide ceramic ultrafiltration membrane.
[0043] The zirconia ceramic ultrafiltration membrane prepared in this example has a retention rate of 95% for 1 g / L bovine serum albumin (molecular weight 67,000) and a flux of 420 LHM under the test conditions of room temperature and 0.1 MPa.
[0044] Example 3
[0045] (1) At 80°C and under stirring conditions, a 5 mol / L ammonia aqueous solution is slowly added to a 0.5 mol / L zirconium oxychloride solution to adjust its pH value to between 9 and 11, and then the solution is filtered. The obtained solid is redispersed in water, and then 1 mol / L nitric acid or hydrochloric acid is added for peptization to adjust its pH value to between 3 and 4, thereby obtaining a transparent zirconium sol.
[0046] (2) Add glycerol with a final concentration of 1 wt % to the zirconium sol obtained in step (1), and then put it into a microwave hydrothermal reactor to carry out microwave hydrothermal reaction at a pressure of 2 MPa for 2 h.
[0047] (3) The material obtained in step (2) is naturally cooled and then subjected to ultrasonic treatment to obtain a translucent zirconium oxide sol.
[0048] (4) Add 2 wt% polyvinyl alcohol and 0.1 wt% hydroxyethyl cellulose to the zirconium oxide sol obtained in step (3), mix thoroughly, and then add 0.01 wt% organosilicon defoamer BYK028 to prepare a uniformly dispersed coating liquid.
[0049] (5) Apply the coating liquid prepared in step (4) to a porous ceramic membrane support having an average pore size of 0.1 μm by dipping, dry at 120° C. for 5 h, and heat at a rate of 3° C. / min, then heat to 700° C. at a rate of 3° C. / min, keep constant temperature for 3 h, and then cool naturally to obtain a zirconium oxide ceramic ultrafiltration membrane.
[0050] The zirconia ceramic ultrafiltration membrane prepared in this example has a retention rate of 90% for 1 g / L bovine serum albumin (molecular weight 67,000) and a flux of 462 LHM under the test conditions of room temperature and 0.1 MPa.
[0051] Comparative Example 1
[0052] (1) At 80°C and under stirring conditions, a 5 mol / L ammonia aqueous solution is slowly added to a 0.5 mol / L zirconium oxychloride solution to adjust its pH value to between 9 and 11, and then the solution is filtered. The obtained solid is redispersed in water, and then 1 mol / L nitric acid or hydrochloric acid is added for peptization to adjust its pH value to between 3 and 4, thereby obtaining a transparent zirconium sol.
[0053] (2) Add polyvinyl alcohol and hydroxyethyl cellulose at a final concentration of 2 wt % and 0.1 wt % respectively to the zirconium sol obtained in step (1), mix thoroughly, and then add silicone defoamer BYK028 at a final concentration of 0.01 wt % to prepare a uniformly dispersed coating liquid.
[0054] (3) Apply the coating solution prepared in step (2) to a porous ceramic membrane support having an average pore size of 0.1 μm by dipping. Dry at 120°C for 5 h, with a heating rate of 3°C / min, then heat to 700°C at a rate of 3°C / min, keep the temperature constant for 3 h, and then cool naturally to obtain the following: Figure 2 The comparative zirconia ceramic ultrafiltration membrane shown in the figure shows that the membrane layer is cracked and falling off.
[0055] The comparative zirconia ceramic ultrafiltration membrane prepared in this comparative example has a retention rate of 5% for 1 g / L bovine serum albumin (molecular weight 67,000) and a flux of 500 LHM under the test conditions of room temperature and 0.1 MPa.
[0056] Comparative Example 2
[0057] (1) At 80°C and under stirring conditions, a 5 mol / L ammonia aqueous solution is slowly added to a 0.5 mol / L zirconium oxychloride solution to adjust its pH value to between 9 and 11, and then the solution is filtered. The obtained solid is redispersed in water, and then 1 mol / L nitric acid or hydrochloric acid is added for peptization to adjust its pH value to between 3 and 4, thereby obtaining a transparent zirconium sol.
[0058] (2) Add glycerol with a final concentration of 1 wt % to the zirconium sol obtained in step (1), then put it into a hydrothermal reactor, heat it to 200° C. and keep it warm for 10 hours.
[0059] (3) The material obtained in step (2) is naturally cooled and then subjected to ultrasonic treatment to obtain a translucent zirconium oxide sol.
[0060] (4) Add 2 wt% polyvinyl alcohol and 0.1 wt% hydroxyethyl cellulose to the zirconium oxide sol obtained in step (3), mix thoroughly, and then add 0.01 wt% organosilicon defoamer BYK028 to prepare a uniformly dispersed coating liquid.
[0061] (5) Apply the coating solution prepared in step (4) to a porous ceramic membrane support having an average pore size of 0.1 μm by dipping. Dry at 120°C for 5 h, with a heating rate of 3°C / min, then heat to 700°C at a rate of 3°C / min, keep the temperature constant for 3 h, and then cool naturally to obtain the following: Figure 3 The comparative zirconia ceramic ultrafiltration membrane shown in FIG. 1 shows that the membrane layer is intact, but the membrane layer particles are larger, resulting in a larger pore size, as shown in Table 1.
[0062] The comparative zirconia ceramic ultrafiltration membrane prepared in this comparative example has a retention rate of 80% for 1 g / L bovine serum albumin (molecular weight 67,000) and a flux of 380 LHM under the test conditions of room temperature and 0.1 MPa.
[0063] Comparative Example 3
[0064] (1) At 80° C. and under stirring conditions, a 5 mol / L ammonia solution was slowly added to 250 ml of a 0.5 mol / L zirconium oxychloride solution to adjust its pH value to between 9 and 11. 1% glycerol was added to the obtained solution, which was then placed in a microwave hydrothermal reactor and subjected to microwave hydrothermal reaction at a pressure of 0.5 MPa for 2 h.
[0065] (2) The material obtained in step (1) is naturally cooled and then subjected to ultrasonic treatment to obtain a translucent zirconium oxide sol.
[0066] (3) Add 2 wt% polyvinyl alcohol and 0.1 wt% hydroxyethyl cellulose to the zirconium oxide sol obtained in step (2), mix thoroughly, and then add 0.01 wt% organosilicon defoamer BYK028 to prepare a uniformly dispersed coating liquid.
[0067] (4) The coating liquid prepared in step (3) was applied to a porous ceramic membrane support having an average pore size of 0.1 μm by dipping. The membrane was dried at 120° C. for 5 h at a heating rate of 3° C. / min, then heated to 700° C. at a rate of 3° C. / min, and then cooled naturally to obtain a comparative zirconium oxide ceramic ultrafiltration membrane after maintaining the temperature for 3 h.
[0068] The comparative zirconia ceramic ultrafiltration membrane prepared in this comparative example has a retention rate of 5% for 1 g / L bovine serum albumin (molecular weight 67,000) and a flux of 562 LHM under the test conditions of room temperature and 0.1 MPa.
[0069] The effects of the nanofiltration membranes obtained in the above comparative example and the embodiment are compared as shown in the following table:
[0070] Preparation method Film Pore size (nm) Mass loss after calcination at 400℃ (%) Comparative Example 1 Sol-Gel Method Easy to crack 20-40 40% Comparative Example 2 Sol-hydrothermal method Complete film 20-40 17% Comparative Example 3 Microwave hydrothermal method Complete film 60-80 14% Example 1 Sol-microwave hydrothermal method Complete film 12-15 13% Example 2 Sol-microwave hydrothermal method Complete film 16-20 11% Example 3 Sol-microwave hydrothermal method Complete film 20-25 8%
[0071] Note: Mass loss after calcination at 400°C (%): The nanoparticle solutions prepared by different methods were dried at 100°C, ground into powder, 10g of powder was weighed and put into a crucible, and the temperature was raised to 400°C at a rate of 3°C / min, kept warm for 3h, cooled to room temperature, and the mass of the powder was weighed C1, and the mass loss (%) = (1-C1 / 10) × 100%. It can be seen from Table 1 that after microwave hydrothermal treatment, the mass loss after calcination at 400°C can be reduced due to the higher crystallinity and lower water content, and the film cracking caused by the volatilization of crystal water and organic matter during the calcination process can be prevented. In addition, as the microwave pressure increases, the particle size increases and the calcination mass loss decreases.
[0072] The above description is only a preferred embodiment of the present invention, and therefore cannot be used to limit the scope of the present invention. That is, equivalent changes and modifications made according to the patent scope of the present invention and the contents of the specification should still fall within the scope of the present invention.
Claims
1. A method for preparing a high-throughput zirconium oxide ceramic ultrafiltration membrane, characterized in that: The steps include: (1) slowly adding an ammonia solution to an inorganic zirconium salt solution at 75-85° C. with stirring to adjust the pH value to between 9 and 11, performing solid-liquid separation, redispersing the obtained solid in water, and then adding nitric acid or hydrochloric acid for peptization to adjust the pH value to between 3 and 4 to obtain a transparent zirconium sol; the inorganic zirconium salt in the inorganic zirconium salt solution is selected from zirconium chloride, zirconium oxychloride and zirconium oxysulfate; (2) adding glycerol with a final concentration of 0.8-1.2 wt % to the zirconium sol obtained in step (1), stirring evenly, placing in a microwave hydrothermal reactor, and performing microwave hydrothermal reaction at a pressure of 0.5-2 MPa for 1-2 h; (3) cooling the material obtained in step (2) naturally and then subjecting it to shearing or ultrasonic treatment to obtain a translucent zirconium oxide sol; (4) adding polyvinyl alcohol and hydroxyethyl cellulose to the zirconium oxide sol obtained in step (3), mixing thoroughly, and then adding an organosilicon defoamer to prepare a uniformly dispersed coating liquid; (5) Apply the coating liquid obtained in step (4) on the porous ceramic membrane support, then dry at 80-120°C for 2-5h, then program the temperature to 500-800°C and keep it for 2-5h, and finally cool it naturally to obtain a zirconia ceramic ultrafiltration membrane.
2. The preparation method according to claim 1, characterized in that: In the step (4), the final concentration of polyvinyl alcohol is 2-5 wt %.
3. The preparation method according to claim 1, characterized in that: In the step (4), the final concentration of hydroxyethyl cellulose is 0.1-0.3 wt %.
4. The preparation method according to claim 1, characterized in that: In the step (4), the final concentration of the organosilicon defoamer is 0.01-1 wt %.
5. The preparation method according to claim 1, characterized in that: In the step (4), the final concentration of polyvinyl alcohol is 2-5wt%, the final concentration of hydroxyethyl cellulose is 0.1-0.3wt%, and the final concentration of the organosilicon defoamer is 0.01-1wt%.
6. The preparation method according to claim 5, characterized in that: In the step (4), the final concentration of polyvinyl alcohol is 2 wt %, the final concentration of hydroxyethyl cellulose is 0.1 wt %, and the final concentration of the organosilicon defoamer is 0.01 wt %.
7. The preparation method according to any one of claims 1 to 6, characterized in that: In the step (1), the concentration of the zirconium oxychloride solution is 0.4-0.6 mol / L, and the concentration of the ammonia solution is 4-6 mol / L.
8. The preparation method according to claim 7, characterized in that: In the step (1), the concentration of the zirconium oxychloride solution is 0.5 mol / L, and the concentration of the ammonia solution is 5 mol / L.
9. The preparation method according to claim 1, characterized in that: In the step (5), the drying temperature rise rate is 1-3°C / min.
10. The preparation method according to claim 9, characterized in that: In the step (5), the rate of the programmed temperature increase is 1-5°C / min.