PDA-CDs (at) Ag antibacterial ceramic membrane, preparation method thereof, ceramic membrane assembly and device

By forming a CDs@Ag nanocomposite antibacterial coating on the surface of the ceramic membrane, the problems of reducing the penetration flux of the ceramic membrane and embedding of antibacterial materials are solved, and efficient bacterial inhibition and bactericidal effects are achieved, and the application field of ceramic membranes is expanded.

CN118904113APending Publication Date: 2024-11-08科溢书忱(重庆)科技服务有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311196441.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-09-18
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

In sewage treatment and deep purification of drinking water, ceramic membranes have reduced penetration flux and poor user experience due to the accumulation of bacteria and viruses. In existing antibacterial measures, nanometal particles are easily embedded in ceramic particles, and the antibacterial effect is not obvious.

Method used

Carbon dots (CDs) and silver ions (Ag) are used to prepare CDs@Ag nanocomposites, combined with the adhesion properties of polydopamine, and an antibacterial coating is formed on the surface of the ceramic membrane to ensure that the antibacterial material is in direct contact with bacteria and avoid embedding problems.

Benefits of technology

Achieve significant antibacterial and bactericidal effects, with an antibacterial rate of more than 99.99%, extending the service life of ceramic membranes, improving water treatment efficiency and user experience, and expanding ceramic membranes in blood purification, medical intermediate filtration and food production Applications in other fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118904113A_ABST
    Figure CN118904113A_ABST
Patent Text Reader

Abstract

The invention discloses a PDA-CDs (at) Ag antibacterial ceramic membrane, a preparation method thereof, a ceramic membrane assembly and a device, and relates to the technical field of preparation and application of ceramic membranes, and the preparation method comprises the steps of preparation of CDs, preparation of a CDs (at) Ag nano-composite, preparation of a dopamine solution, preparation of a ceramic membrane with a PDA coating adhered to the surface and preparation of the PDA-CDs (at) Ag antibacterial ceramic membrane. The prepared CDs (at) Ag nano-composite is excellent in antibacterial performance, a PDA-CDs (at) Ag coating with the good antibacterial performance is formed on the surface of a ceramic membrane by means of the adhesion performance of polydopamine, the problem that an antibacterial material is embedded by the ceramic membrane does not exist, the CDs (at) Ag nano-composite directly makes contact with bacteria, the antibacterial and bactericidal effects are very obvious, and the antibacterial and bactericidal effects are good. When the PDA-CDs (at) Ag antibacterial ceramic membrane is applied to a ceramic membrane assembly and a ceramic membrane device, the antibacterial performance and the antibacterial lasting performance can be effectively improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of ceramic membrane preparation, and in particular to a PDA-CDs@Ag antibacterial ceramic membrane and a preparation method thereof, a ceramic membrane component and a device. Background Art

[0002] Ceramic membranes have been widely used in sewage treatment and deep purification of drinking water due to their high temperature resistance, acid and alkali resistance, easy cleaning, and long life. The main application of ceramic membranes in sewage treatment is to quickly separate the activated sludge from the water in the aerobic tank, thereby replacing the secondary sedimentation tank with a large footprint. It has the advantages of good effluent quality, small footprint, and high filtration efficiency. However, aerobic bacteria in the activated sludge are inevitably attached to the membrane surface and pore walls under the suction drive of the negative pressure pump. As time accumulates, the membrane pores are seriously blocked and the treatment efficiency is reduced. In the field of deep purification of drinking water, the high-precision aperture of the ceramic membrane is used as a screen to efficiently intercept the suspended solids such as rust, silt, colloids and two worms (Giardia and Cryptozoa), bacteria, and viruses attached to bacteria in tap water. Invisible pathogenic microorganisms such as viruses, infiltrate safe, clean, and hygienic drinking water. However, the intercepted pathogenic microorganisms accumulate on the membrane surface and pores, resulting in reduced permeation flux of the ceramic membrane and poor user experience. In addition, the main measure for modifying the ceramic membrane with antibacterial function in the prior art is to add nano-metal particles into the ceramic membrane matrix and separation layer during the preparation of the ceramic membrane, and then perform high-temperature sintering heat treatment. The problem is that the nano-metal particles are easily embedded in the ceramic particles, and the antibacterial effect is not obvious. Summary of the invention

[0003] In view of this, the purpose of the present invention is to provide a PDA-CDs@Ag antibacterial ceramic membrane. By preparing a CDs@Ag nanocomposite antibacterial material, a coating with good antibacterial properties is formed on the surface of the ceramic membrane with the help of the adhesion properties of polydopamine. There is no problem of the antibacterial material being embedded in the ceramic membrane. The CDs@Ag nanocomposite antibacterial material can directly contact with bacteria, and the antibacterial and bactericidal effects are very obvious.

[0004] To achieve the above object, the present invention also provides a method for preparing a PDA-CDs@Ag antibacterial ceramic membrane, and the specific steps are as follows:

[0005] 1) Preparation of carbon dots (CDs)

[0006] Take glycyrrhizic acid and citric acid and dissolve them in deionized water, transfer them to a polytetrafluoroethylene reactor, react at 160-180°C for 6-12 hours, cool to room temperature, centrifuge the reaction solution for 5-10 minutes, filter it with a 0.22μm filter membrane, and then dialyze the product with a 500Da ready-to-use dialysis bag for 24-48 hours to obtain a yellow powder, which is carbon dots (CDs). Glycyrrhizic acid, the active ingredient in the green natural compound licorice, is used as a carbon source, and citric acid, a compound rich in hydroxyl and carboxyl groups, is used as a dopant to synthesize CDs. The prepared CDs have good water solubility and stability, and exhibit excellent antibacterial activity.

[0007] 2) Preparation of CDs@Ag nanocomposites

[0008] Add dilute ammonia water to AgNO3 solution to prepare 0.1 mol / L [Ag(NH3)2]OH solution, add CDs prepared in step 1) to the aqueous solution to prepare 1-3 g / L CDs solution, mix the freshly prepared [Ag(NH3)2]OH solution and CDs solution in a volume ratio of 2:1, react for 10-30 min in a water bath at 80-100°C under magnetic stirring, cool to room temperature, centrifuge the obtained solution, and freeze-dry the precipitate at -80°C for 24-48 h to obtain a CDs@Ag nanocomposite.

[0009] 3) Preparation of dopamine solution

[0010] Dissolve tris(hydroxymethyl)aminomethane in deionized water at a ratio of 2 g / L to prepare dopamine-Tris buffer, adjust the solution pH to 8.5, then add dopamine (DA) in an amount of 1.5 to 2 times the mass of tris(hydroxymethyl)aminomethane, stir and dissolve, and obtain a dopamine solution.

[0011] 4) Preparation of ceramic membrane with PDA coating on the surface

[0012] Take the ceramic membrane substrate and immerse it in the dopamine solution prepared in step 3) to completely immerse the ceramic membrane substrate, and then place it in a constant temperature shaker to react for 3 hours to allow dopamine to polymerize to form polydopamine (PDA) and adhere to the surface of the ceramic membrane substrate. Then remove the solution, add deionized water to completely immerse the ceramic membrane substrate, and ultrasonicate for 5-10 minutes to remove non-adherent PDA particles to obtain a ceramic membrane with a PDA coating adhered to the surface.

[0013] 5) Preparation of PDA-CDs@Ag antibacterial ceramic membrane

[0014] The CDs@Ag nanocomposite prepared in step 2) is dispersed in deionized water to obtain a CDs@Ag nanocomposite solution, and then the CDs@Ag nanocomposite solution is evenly sprayed on the undried surface of the ceramic membrane with the PDA coating adhered thereto, and then dried at 60-70°C to obtain a PDA-CDs@Ag antibacterial ceramic membrane.

[0015] Carbon dots are a new type of zero-dimensional nanomaterials with an average particle size of less than 10nm. They have attracted much attention due to their small size, easy synthesis, excellent fluorescence properties and good biocompatibility. Carbon dots can produce reactive oxygen, inhibit bacterial cell wall synthesis, and destroy bacterial DNA, so they have good antibacterial properties and will not cause bacteria to develop drug resistance. Compared with metal nanoparticles, carbon dots have lower cytotoxicity. However, the antibacterial properties of carbon dots are still far behind those of metal nanomaterials, while the use of metal nanomaterials is limited by their cytotoxicity. The present invention adopts a one-step hydrothermal method to synthesize CDs rich in carboxyl and hydroxyl functional groups, and uses CDs as a reducing agent and a stabilizer. Without adding additional reducing agents and stabilizing agents, a chemical precipitation method is used to prepare a CDs@Ag nanocomposite. The synthesized CDs@Ag nanocomposite with excellent antibacterial properties is then used to form a coating with good antibacterial properties on the surface of a ceramic membrane with the help of the adhesion properties of polydopamine. The coating not only has excellent antibacterial properties and long antibacterial persistence (Ag ions in the CDs@Ag nanocomposite can be slowly released, and carbon dots can generate active oxygen, inhibit bacterial cell wall synthesis, and destroy bacterial DNA, which can greatly improve the continuous antibacterial performance of the coating), but also has good biocompatibility and low cytotoxicity.

[0016] In some preferred embodiments, the mass volume ratio of glycyrrhizic acid, citric acid and deionized water in step 1) is 2:0.5-1:10-40, g:g:mL.

[0017] In some preferred embodiments, the mass fraction of the dilute ammonia water in step 2) is 20-28%, and the concentration of the AgNO3 solution is 0.5-1 mol / L.

[0018] In some preferred embodiments, the rotation speed of the centrifugation step in step 2) is 8000-12000 rpm, and the centrifugation time is 10-15 min.

[0019] In some preferred embodiments, the temperature of the constant temperature shaker in step 4) is 30-35°C, and the shaking speed is 45-65 rpm.

[0020] In some preferred embodiments, during the process of immersing the ceramic membrane in the prepared PDA solution in step 4), the ceramic membrane is immersed in the prepared PDA solution at a speed of 50-100 mm / min vertically to the liquid surface. The ceramic membrane is immersed in the liquid surface at a speed of 50-100 mm / min vertically to reduce the vibration of the solution during the immersion process, avoid the unevenness of the membrane layer caused by vibration, and is conducive to improving the smoothness of the membrane surface.

[0021] In some preferred embodiments, the concentration of the CDs@Ag nanocomposite solution in step 5) is 5 g / L. A CDs@Ag nanocomposite solution with too high a concentration will affect the sprayability, while a CDs@Ag nanocomposite solution with too low a concentration will affect the film-forming property. The CDs@Ag nanocomposite solution with a concentration of 5 g / L has excellent sprayability and film-forming property.

[0022] In some preferred embodiments, the CDs@Ag nanocomposite solution in step 5) is uniformly sprayed on the surface of the ceramic membrane with the PDA coating adhered thereto, and the thickness of the coating formed by drying is between 10 μm and 100 μm. When the coating has a more suitable thickness, it can stably exist on the surface of the ceramic membrane and maintain excellent antibacterial properties for a long time; when the coating thickness is too thick, the stability of the coating will deteriorate, and the coating will be easily damaged, thereby weakening its long-term antibacterial properties.

[0023] In addition, the present invention also provides a ceramic membrane assembly, which includes the PDA-CDs@Ag antibacterial ceramic membrane prepared by the above method.

[0024] In addition, the present invention also provides a device, which includes the above-mentioned ceramic membrane assembly, and the application of the device in water purification. The device can efficiently kill bacteria in water and pathogenic microorganisms such as viruses attached to bacteria that are invisible to the naked eye, and permeate safe, clean and hygienic drinking water, solving the problems of pathogenic microorganisms intercepted in the process of water purification treatment accumulating on the surface and pores of the ceramic membrane, resulting in reduced permeation flux of the ceramic membrane and poor user experience, etc., and can ensure the quality and efficiency of ceramic membrane water treatment for a long time, while effectively improving the service life of the ceramic membrane and reducing the cost of use.

[0025] In addition, due to the excellent antibacterial properties of PDA-CDs@Ag antibacterial ceramic membrane, as well as good biocompatibility, low cytotoxicity, good hydrophilicity and other excellent properties; therefore, a ceramic membrane substrate with appropriate pore size is first selected to prepare PDA-CDs@Ag antibacterial ceramic membranes with different pore size distributions according to the above method. The obtained PDA-CDs@Ag antibacterial ceramic membrane can also be used in blood purification, pharmaceutical intermediate filtration, food production and other fields, which can effectively expand the application fields of ceramic sheets.

[0026] Beneficial effects of the present invention:

[0027] 1. The CDs@Ag nanocomposite prepared by the present invention has excellent antibacterial properties. With the help of the adhesion properties of polydopamine, a stable PDA-CDs@Ag coating is formed on the surface of the ceramic membrane. There is no problem of the CDs@Ag nanocomposite antibacterial material being embedded in the ceramic membrane, and the CDs@Ag nanocomposite is in direct contact with bacteria, and the antibacterial and bactericidal effects are very obvious.

[0028] 2. In the coating of the antibacterial ceramic film of the present invention, the Ag ions in the CDs@Ag nanocomposite can be slowly released, and the carbon dots can generate active oxygen, inhibit bacterial cell wall synthesis, and destroy bacterial DNA, which can greatly improve the continuous antibacterial performance of the coating, and the antibacterial rate reaches more than 99.99%.

[0029] 3. The antibacterial ceramic membrane of the present invention has excellent properties such as good biocompatibility, low cytotoxicity, and good hydrophilicity. It can not only be used for water purification, but also can be widely used in blood purification, pharmaceutical intermediate filtration, food production and other fields, effectively expanding the application field of ceramic sheets. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 This is the SEM image of the PDA-CDs@Ag antibacterial ceramic membrane of the present invention;

[0031] Figure 2 This is a pore size distribution curve of the PDA-CDs@Ag antibacterial ceramic membrane of the present invention;

[0032] Figure 3 This is the antibacterial experimental diagram of the PDA-CDs@Ag antibacterial ceramic membrane of the present invention. DETAILED DESCRIPTION

[0033] The present invention will be described in detail below with reference to embodiments:

[0034] Example 1

[0035] The preparation method of the PDA-CDs@Ag antibacterial ceramic film of this embodiment is as follows:

[0036] 1) Preparation of CDs

[0037] Weigh 10 g of oxalic acid and 2.5 g of citric acid, add them into 50 mL of deionized water to dissolve, transfer them into a polytetrafluoroethylene reactor, react at 160 ° C for 6 h, cool to room temperature, centrifuge the reaction solution for 5 min, filter it with a 0.22 μm filter membrane, and then dialyze the product with a 500 Da ready-to-use dialysis bag for 24 h to remove small molecules. The yellow powder obtained is CDs.

[0038] 2) Preparation of CDs@Ag nanocomposites

[0039] Dilute ammonia water with a mass fraction of 20% was added to a 0.5 mol / L AgNO3 solution to prepare a 0.1 mol / L [Ag(NH3)2]OH solution, and CDs was added to the aqueous solution to prepare a 1 g / L CDs solution. The freshly prepared [Ag(NH3)2]OH solution and the CDs solution were mixed in a volume ratio of 2:1, and reacted for 10 min under magnetic stirring in an 80°C water bath. After cooling to room temperature, the resulting solution was centrifuged at 8000 rpm for 10 min, and the precipitate was freeze-dried at -80°C for 24 h to obtain a CDs@Ag nanocomposite.

[0040] 3) Preparation of dopamine solution

[0041] Dissolve tris(hydroxymethyl)aminomethane in deionized water at a ratio of 2 g / L to prepare dopamine-Tris buffer, adjust the solution pH to 8.5, then add dopamine 1.5 times the mass of tris(hydroxymethyl)aminomethane, stir and dissolve, and obtain a dopamine solution.

[0042] 4) Preparation of ceramic membrane with PDA coating on the surface

[0043] The ceramic membrane was immersed in the prepared PDA solution vertically at a speed of 50 mm / min so that the ceramic membrane substrate was completely immersed, and then placed in a constant temperature shaker for reaction for 3 hours (the temperature of the constant temperature shaker was 30°C and the shaker speed was 45 rpm) to allow dopamine to polymerize to form polydopamine (PDA) and adhere to the surface of the ceramic membrane substrate. The PDA solution was then removed, deionized water was added to completely immerse the ceramic membrane substrate, and ultrasonic treatment was performed for 5 minutes to remove non-adherent PDA particles to obtain a ceramic membrane with a PDA coating adhered to the surface.

[0044] 5) Preparation of PDA-CDs@Ag antibacterial ceramic membrane

[0045] The CDs@Ag nanocomposite was dispersed in deionized water at a ratio of 5 g / L to obtain a CDs@Ag nanocomposite solution, and then the CDs@Ag nanocomposite solution was evenly sprayed on the undried surface of the ceramic membrane with the PDA coating adhered thereto, and then dried at 60°C to form a coating with a thickness of about 10 μm, thereby obtaining a PDA-CDs@Ag antibacterial ceramic membrane.

[0046] Example 2

[0047] The preparation method of the PDA-CDs@Ag antibacterial ceramic film of this embodiment is as follows:

[0048] 1) Preparation of CDs

[0049] Weigh 10 g of glycyrrhizic acid and 4 g of citric acid, add them into 100 mL of deionized water to dissolve, transfer them into a polytetrafluoroethylene reactor, react at 170 ° C for 8 h, cool to room temperature, centrifuge the reaction solution for 8 min, filter it with a 0.22 μm filter membrane, and then dialyze the product with a 500 Da ready-to-use dialysis bag for 36 h to remove small molecules, and obtain a yellow powder, which is CDs.

[0050] 2) Preparation of CDs@Ag nanocomposites

[0051] Dilute ammonia water with a mass fraction of 25% was added to a 0.6 mol / L AgNO3 solution to prepare a 0.1 mol / L [Ag(NH3)2]OH solution, and CDs was added to the aqueous solution to prepare a 2 g / L CDs solution. The freshly prepared [Ag(NH3)2]OH solution and the CDs solution were mixed in a volume ratio of 2:1, and reacted for 20 minutes under magnetic stirring in a 90°C water bath. After cooling to room temperature, the resulting solution was centrifuged at 10,000 rpm for 12 minutes, and the precipitate was freeze-dried at -80°C for 36 hours to obtain a CDs@Ag nanocomposite.

[0052] 3) Preparation of dopamine solution

[0053] Dissolve tris(hydroxymethyl)aminomethane in deionized water at a ratio of 2 g / L to prepare dopamine-Tris buffer, adjust the solution pH to 8.5, then add dopamine 1.7 times the mass of tris(hydroxymethyl)aminomethane, stir and dissolve, and obtain a dopamine solution.

[0054] 4) Preparation of ceramic membrane with PDA coating on the surface

[0055] The ceramic membrane was immersed in the prepared PDA solution vertically at a speed of 80 mm / min so that the ceramic membrane substrate was completely immersed, and then placed in a constant temperature shaker for reaction for 3 hours (the temperature of the constant temperature shaker was 32°C and the shaker speed was 60 rpm) to allow dopamine to polymerize to form polydopamine (PDA) and adhere to the surface of the ceramic membrane substrate. The PDA solution was then removed, deionized water was added to completely immerse the ceramic membrane substrate, and ultrasonic treatment was performed for 8 minutes to remove non-adherent PDA particles to obtain a ceramic membrane with a PDA coating adhered to the surface.

[0056] 5) Preparation of PDA-CDs@Ag antibacterial ceramic membrane

[0057] The CDs@Ag nanocomposite was dispersed in deionized water at a ratio of 5 g / L to obtain a CDs@Ag nanocomposite solution, and then the CDs@Ag nanocomposite solution was evenly sprayed on the undried surface of the ceramic membrane with the PDA coating adhered thereto, and then dried at 65°C to form a coating with a thickness of about 50 μm, thereby obtaining a PDA-CDs@Ag antibacterial ceramic membrane.

[0058] Example 3

[0059] The preparation method of the PDA-CDs@Ag antibacterial ceramic film of this embodiment is as follows:

[0060] 1) Preparation of CDs

[0061] Weigh 10g of glycyrrhizic acid and 5g of citric acid, add them into 200mL of deionized water to dissolve, transfer them into a polytetrafluoroethylene reactor, react at 180℃ for 12h, cool to room temperature, centrifuge the reaction solution for 10min, filter it with a 0.22μm filter membrane, and then dialyze the product with a 500Da ready-to-use dialysis bag for 48h to remove small molecules, and obtain a yellow powder, which is carbon CDs.

[0062] 2) Preparation of CDs@Ag nanocomposites

[0063] Dilute ammonia water with a mass fraction of 28% was added to a 1 mol / L AgNO3 solution to prepare a 0.1 mol / L [Ag(NH3)2]OH solution, and CDs was added to the aqueous solution to prepare a 3 g / L CDs solution. The freshly prepared [Ag(NH3)2]OH solution and the CDs solution were mixed in a volume ratio of 2:1, and reacted for 30 minutes under magnetic stirring in a -100°C water bath. After cooling to room temperature, the resulting solution was centrifuged at 12000 rpm for 15 minutes, and the precipitate was freeze-dried at -80°C for 48 hours to obtain a CDs@Ag nanocomposite.

[0064] 3) Preparation of dopamine solution

[0065] Dissolve tris(hydroxymethyl)aminomethane in deionized water at a ratio of 2 g / L to prepare dopamine-Tris buffer, adjust the solution pH to 8.5, then add dopamine twice the mass of tris(hydroxymethyl)aminomethane, stir and dissolve, and obtain a dopamine solution.

[0066] 4) Preparation of ceramic membrane with PDA coating on the surface

[0067] The ceramic membrane was immersed in the prepared PDA solution vertically at a speed of 100 mm / min so that the ceramic membrane substrate was completely immersed, and then placed in a constant temperature shaker for reaction for 3 hours (the temperature of the constant temperature shaker was 35°C and the shaker speed was 65 rpm) to allow dopamine to polymerize to form polydopamine (PDA) and adhere to the surface of the ceramic membrane substrate. The PDA solution was then removed, deionized water was added to completely immerse the ceramic membrane substrate, and ultrasonic treatment was performed for 10 minutes to remove non-adherent PDA particles to obtain a ceramic membrane with a PDA coating adhered to the surface.

[0068] 5) Preparation of PDA-CDs@Ag antibacterial ceramic membrane

[0069] The CDs@Ag nanocomposite was dispersed in deionized water at a ratio of 5 g / L to obtain a CDs@Ag nanocomposite solution, and then the CDs@Ag nanocomposite solution was evenly sprayed on the undried surface of the ceramic membrane with the PDA coating adhered thereto, and then dried at 70°C to form a coating with a thickness of about 100 μm, thereby obtaining a PDA-CDs@Ag antibacterial ceramic membrane.

[0070] Comparative Example

[0071] The flat ceramic membrane purchased from Jiangsu Jiuwu Hi-Tech Co., Ltd. is a non-flat ceramic membrane sintered under high temperature conditions with a purity of 99% α-Al2O3: 1) Membrane shape: hollow plate; 2) Filtration method: external pressure or internal suction; 3) Material: α-Al2O3, ZrO2; 4) Standard pore size: 0.1-0.2um; 5) Pure water flux: 500-600L / (m·h·bar); 6) Use pH range: 0-14; 7) Use temperature: 0-80℃.

[0072] PDA-CDs@Ag antibacterial ceramic membrane performance test:

[0073] 1. Microscopic morphology observation

[0074] In order to characterize the microscopic morphology of the PDA-CDs@Ag antibacterial ceramic membrane prepared in the present invention, the PDA-CDs@Ag antibacterial ceramic membrane prepared in Examples 1-3 and the Jiuwu High-Tech flat ceramic membrane of the comparative example were characterized by SEM. The results are as follows: Figure 1 As shown, it can be seen that the surface of the PDA-CDs@Ag antibacterial ceramic film prepared by the preparation method of the present invention is smooth and has relatively obvious granular substances, that is, CDs@Ag nanocomposite antibacterial particles.

[0075] 2. Pore size distribution test

[0076] In order to test the pore size distribution of the PDA-CDs@Ag antibacterial ceramic membrane prepared by the present invention, the PDA-CDs@Ag antibacterial ceramic membranes of Examples 1-3 and the Jiuwu High-Tech flat ceramic membrane of the comparative example were tested using a membrane pore size analyzer. The test results are as follows: Figure 2 As shown. It can be seen that the pore size distribution of the PDA-CDs@Ag antibacterial ceramic membrane prepared in Examples 1-3 is mainly concentrated in 0.08-0.12μm, and the pore size distribution of the Jiuwu High-Tech flat ceramic membrane is mainly concentrated in 0.1-0.2μ. It can be seen that the pore size of the PDA-CDs@Ag antibacterial ceramic membrane of the present invention is slightly smaller than that of the comparative example. Therefore, the PDA-CDs@Ag antibacterial ceramic membrane is completely suitable for use in the field of water purification treatment.

[0077] 3. Conventional performance parameter testing

[0078] The pure water flux, compressive strength and porosity of the PDA-CDs@Ag antibacterial ceramic membranes prepared in Examples 1-3 and the Jiuwu High-Tech flat ceramic membrane of the comparative example were tested respectively. The test results are shown in Table 1.

[0079] Table 1 Conventional performance parameter testing

[0080] Test items Pure water flux L / (m·h·bar) Compressive strength / MPa Porosity / % Example 1 1260.16 32.14 61.22 Example 2 1130.58 34.95 60.71 Example 3 1067.20 29.67 58.38 Comparative Example 583.92 22.70 46.25

[0081] It can be seen from the test results in Table 1 that the pure water flux of the PDA-CDs@Ag antibacterial ceramic membranes prepared in Examples 1-3 are all above 1000L / (m·h·bar), the compressive strength is all around 30MPa, and the porosity is about 60%, which has significant advantages over the flat ceramic membranes of the comparative example.

[0082] 4. Antibacterial performance test

[0083] A quantitative antibacterial rate experiment (oscillation method) was adopted, and the PDA-CDs@Ag antibacterial ceramic membrane prepared in Examples 1-3 was taken as the experimental group, the Jiuwu High-Tech flat ceramic membrane of the comparative example was taken as the control group, and a blank group was set up. Take 15 test tubes and divide them into 5 groups, each group has 3 test tubes, and each group of 3 test tubes is added with 15 ml of three different bacterial suspensions (Escherichia coli, Salmonella, Shigella dysenteriae). The Jiuwu High-Tech flat ceramic membrane of the control group is added to one of the test tubes containing 15 ml of different bacterial suspensions, and the PDA-CDs@Ag antibacterial ceramic membrane prepared in Example 1-3 is added to three of the test tubes containing 15 ml of different bacterial suspensions. The remaining group of test tubes containing 15 ml of different bacterial suspensions is not added with any material as a blank group. After the three bacteria are cultured for 18 hours, the original bacterial solution is diluted 100,000 times step by step, and 50 μL of the diluted bacterial suspension is evenly coated on the surface of the solid culture medium. After culturing in a cell culture incubator at 37°C for 24 hours, the antibacterial effects on the three different bacteria are as follows. Figure 3 shown.

[0084] Then count and calculate the antibacterial rate, and the antibacterial rate of the PDA-CDs@Ag antibacterial ceramic membrane prepared in Examples 1-3 against three different bacteria reached more than 99.99%, while the control group Jiuwu High-Tech flat ceramic membrane had no obvious antibacterial effect on the three different bacteria. Among them, the antibacterial rate = (NSC-NS) / NSC×100% (where NSC is the number of colonies in the blank group, and NS is the number of colonies in the test group). It can be seen that the PDA-CDs@Ag antibacterial ceramic membrane prepared by the present invention has very excellent bactericidal performance and can meet the purpose of killing common bacteria in water.

[0085] The above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit the present invention. Although the present invention is described in detail with reference to the preferred embodiments, it should be understood by those skilled in the art that the technical solutions of the present invention may be modified or replaced by equivalents without departing from the purpose and scope of the technical solutions of the present invention, which should be included in the scope of the claims of the present invention. The technologies not described in detail in the present invention are known technologies.

Claims

1. A method for preparing a PDA-CDs@Ag antibacterial ceramic membrane, characterized in that: The specific steps are as follows: 1) Preparation of CDs: Glycyrrhizic acid and citric acid were dissolved in deionized water, and then transferred to a polytetrafluoroethylene reactor, reacted at 160-180°C for 6-12 hours, cooled to room temperature, centrifuged for 5-10 minutes, and filtered with a 0.22 μm filter membrane. The product was then dialyzed with a 500 Da ready-to-use dialysis bag for 24-48 hours to obtain a yellow powder, which is CDs; 2) Preparation of CDs@Ag nanocomposite: dilute ammonia water is added to AgNO3 solution to prepare 0.1 mol / L [Ag(NH3)2]OH solution, CDs prepared in step 1) is added to the aqueous solution to prepare 1-3 g / L CDs solution, freshly prepared [Ag(NH3)2]OH solution and CDs solution are mixed in a volume ratio of 2:1, reacted in a water bath at 80-100°C with magnetic stirring for 10-30 min, cooled to room temperature, centrifuged the obtained solution, and freeze-dried the precipitate at -80°C for 24-48 h to obtain CDs@Ag nanocomposite; 3) Preparation of dopamine solution: dissolve tris(hydroxymethyl)aminomethane in deionized water at a ratio of 2 g / L to prepare dopamine-Tris buffer, adjust the solution pH to 8.5, then add dopamine in an amount of 1.5-2 times the mass of tris(hydroxymethyl)aminomethane, stir and dissolve, and obtain a dopamine solution; 4) Preparation of a ceramic membrane with a PDA coating adhered to the surface: immerse the ceramic membrane substrate in the dopamine solution prepared in step 3) to completely immerse the ceramic membrane substrate, and then place it in a constant temperature shaker to react for 3 hours, then remove the solution, add deionized water to completely immerse the ceramic membrane substrate, and ultrasonicate for 5-10 minutes to obtain a ceramic membrane with a PDA coating adhered to the surface; 5) Preparation of PDA-CDs@Ag antibacterial ceramic membrane: The CDs@Ag nanocomposite prepared in step 2) is dispersed in deionized water to obtain a CDs@Ag nanocomposite solution, and then the CDs@Ag nanocomposite solution is evenly sprayed on the undried surface of the ceramic membrane with the PDA coating adhered thereto, and then dried at 60-70°C to obtain a PDA-CDs@Ag antibacterial ceramic membrane.

2. The preparation method according to claim 1, characterized in that The mass volume ratio of glycyrrhizic acid, citric acid and deionized water in step 1) is 2:0.5-1:10-40, g:g:mL.

3. The preparation method according to claim 2, characterized in that: The mass fraction of the dilute ammonia water in step 2) is 20-28%, and the concentration of the AgNO3 solution is 0.5-1 mol / L.

4. The preparation method according to claim 3, characterized in that: The rotation speed of the centrifugation step in step 2) is 8000-12000 rpm, and the centrifugation time is 10-15 min.

5. The preparation method according to claim 4, characterized in that: The temperature of the constant temperature shaker in step 4) is 30-35°C, and the shaking speed is 45-65 rpm.

6. The preparation method according to claim 5, characterized in that: In step 4), during the process of immersing the ceramic membrane into the prepared PDA solution, the ceramic membrane is immersed in the prepared PDA solution vertically at a speed of 50-100 mm / min.

7. The preparation method according to claim 6, characterized in that: The concentration of the CDs@Ag nanocomposite solution in step 5) is 5 g / L.

8. The preparation method according to claim 7, characterized in that: In step 5), the CDs@Ag nanocomposite solution is uniformly sprayed on the surface of the ceramic film with the PDA coating adhered thereto, and then dried to form a coating with a thickness between 10 μm and 100 μm.

9. The PDA-CDs@Ag antibacterial ceramic membrane prepared by the preparation method according to any one of claims 1 to 8.

10. A ceramic membrane assembly, characterized in that: The ceramic membrane assembly includes the PDA-CDs@Ag antibacterial ceramic membrane as described in claim 9.

11. A device, characterized in that: The device comprises the ceramic membrane module according to claim 10.

12. Use of the device as claimed in claim 11 in water purification.