Preparation method of fiber aerogel composite material
By combining SiO2 aerogel with flame retardant organosilane, fiber aerogel composites are prepared, which solves the problems of flammability and poor mechanical properties of SiO2 aerogel, improves flame retardant performance and adhesion, and achieves high strength and fiber aerogel composite material with high thermal insulation effect.
Patent Information
- Application Number
- CN202410992614.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-08
AI Technical Summary
The application of SiO2 aerogel in the field of heat insulation is limited by its flammability, poor mechanical properties, poor adhesion and the impact of thermal insulation effect after falling off, and the addition of flame retardant will affect its mechanical properties.
Silicon sol is prepared by mixing ethyl orthosilicate and flame retardant organosilane with water and ethanol, performing hydrolysis and polymerization, and spraying it with impregnated fiber felts, aging and drying, forming a fiber aerogel composite material, and introducing Flame retardant elements and improve adhesion.
It improves the support strength and flame retardant properties of fiber aerogel composite materials, avoids the problem of easy powder loss, is simple and easy to operate, and is suitable for industrial production.
Smart Images

Figure BDA0004959268850000051 
Figure BDA0004959268850000061
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of aerogels, and in particular relates to a method for preparing a fiber aerogel composite material. Background Art
[0002] SiO2 aerogel has a unique three-dimensional nano-network structure (skeleton 2-5nm), high specific surface area (200-1000m 2 / g), high porosity (95%), can effectively inhibit solid-state heat conduction and gas convection heat transfer, has excellent thermal insulation properties, and is a solid material with the lowest thermal conductivity.
[0003] At present, there are still some difficulties in directly using SiO2 aerogel in the field of thermal insulation. The main reason is that ordinary SiO2 aerogel is flammable, has low density, high porosity, poor mechanical properties, low strength and high brittleness. In order to expand the application range of aerogel and make nanoporous aerogel thermal insulation materials with practical value, it is necessary to modify SiO2 aerogel to be flame retardant, reinforced and toughened. However, SiO2 aerogel has poor compatibility with flame retardants. Adding a large amount of flame retardants will affect the mechanical properties of SiO2 aerogel. In addition, SiO2 aerogel has poor adhesion to reinforcing matrix materials such as fibers, and there is a problem of easy powder loss in application. Ordinary masks cannot intercept aerogel powder, which is harmful to the body after inhalation; and it will affect its high-temperature thermal insulation effect after falling off. Summary of the invention
[0004] The purpose of the present invention is to provide a method for preparing a fiber aerogel composite material to solve the problem of poor mechanical properties of the fiber aerogel composite material.
[0005] The purpose of the present invention can be achieved through the following technical solutions:
[0006] A method for preparing a fiber aerogel composite material comprises the following steps:
[0007] The first step is to add ethyl orthosilicate and flame retardant organosilane into ethanol, stir and disperse, then add water, adjust the pH value to 2-3 with dilute hydrochloric acid, fully hydrolyze, then add ammonia water to adjust the pH value to 7-8, perform polymerization reaction, and obtain silica sol;
[0008] The second step is to spray the obtained silica sol onto the fiber felt, and after impregnation, the fiber felt is allowed to stand for aging at a temperature of 40° C. After aging, the fiber felt is dried at normal pressure.
[0009] Furthermore, in the first step, the molar ratio of tetraethyl orthosilicate, ethanol and water is 0.04-0.05:1.5:1.5; the mass ratio of tetraethyl orthosilicate and flame retardant organosilane is 8:2-3.
[0010] Furthermore, in the first step, the polymerization reaction is carried out until the viscosity reaches 6-8 mPa·s.
[0011] Furthermore, 0.5 mL of silica sol was sprayed and impregnated per cubic centimeter of the fiber felt.
[0012] Furthermore, in the second step, the conditions for drying at normal pressure are: drying at 50°C, 80°C, 100°C, 150°C and 200°C for 4 hours respectively, and then drying at 250°C to constant weight.
[0013] Furthermore, the fiber felt is formed by laying out inorganic ceramic fibers or weaving fiber bundles.
[0014] Furthermore, the inorganic ceramic fiber is any one of quartz fiber, aluminum silicate fiber, zirconium oxide fiber, aluminum oxide fiber, and mullite fiber.
[0015] Furthermore, the flame retardant organosilane is prepared by the following steps:
[0016] Under nitrogen protection, phenylphosphoryl decanediamine was added to N, N-dimethylformamide, the temperature was set to 45°C, 3-isocyanate propyl trimethoxy silane was added dropwise, the temperature was kept constant after the addition, and the reaction was continued with stirring for 4 hours. After the reaction was completed, low-boiling substances were removed by reduced pressure distillation to obtain flame-retardant organic silane, and the molar ratio of phenylphosphoryl decanediamine and 3-isocyanate propyl trimethoxy silane was 1:2. Phenylphosphoryl decanediamine was obtained by condensation reaction of phenylphosphoryl dichloride and 1,10-decanediamine at a molar ratio of 1:2.
[0017] At 0°C and under nitrogen protection, phenylphosphoryl dichloride and 1,10-decanediamine were mixed, the temperature was set to 60°C, and the mixture was reacted for 6 hours and then washed with water to obtain phenylphosphoryl decanediamine.
[0018] Beneficial effects of the present invention:
[0019] The invention provides a method for preparing a fiber aerogel composite material. In the preparation method, tetraethyl orthosilicate and flame-retardant organic silane are used as precursors, and the aerogel composite material is prepared by a sol-gel method. The obtained composite material has high supporting strength, and flame-retardant elements are introduced to improve the flame retardant performance of the aerogel composite material.
[0020] In the present invention, the fiber aerogel composite material is prepared by infiltrating the silica sol into the fiber felt through the impregnation method and then undergoing gel aging and other operations, which can avoid the problem of easy powder loss from the source. The method of the present invention has low environmental requirements, and the entire process is simple and easy to operate, and is suitable for industrial production. DETAILED DESCRIPTION
[0021] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0022] Example 1
[0023] This embodiment provides a method for preparing a fiber aerogel composite material, comprising the following steps:
[0024] In the first step, at a temperature of 0°C and under nitrogen protection, phenylphosphoryl dichloride and 1,10-decanediamine were mixed in a molar ratio of 1:2, the temperature was set to 60°C, the reaction was performed for 6 hours, and phenylphosphoryl decanediamine was obtained after washing with water and drying.
[0025] Under nitrogen protection, phenylphosphoryldecanediamine was added to N, N-dimethylformamide, the temperature was set to 45°C, 3-isocyanatepropyltrimethoxysilane was added dropwise, the temperature was kept unchanged after the addition, and the stirring reaction was continued for 4 hours. After the reaction was completed, low-boiling substances were removed by reduced pressure distillation to obtain a flame-retardant organic silane. The molar ratio of phenylphosphoryldecanediamine and 3-isocyanatepropyltrimethoxysilane was 1:2.
[0026] Tetraethyl orthosilicate and flame-retardant organosilane are added to ethanol, stirred and dispersed, and then water is added. The pH value is adjusted to 2 with dilute hydrochloric acid, and fully hydrolyzed for 8 hours. Then, ammonia water is added to adjust the pH value to 7.5, and a polymerization reaction is carried out. The reaction is carried out until the viscosity is 6 mPa·s to obtain a silica sol; wherein the molar ratio of tetraethyl orthosilicate, ethanol and water is 0.04:1.5:1.5; and the mass ratio of tetraethyl orthosilicate and flame-retardant organosilane is 8:2.
[0027] The second step is to spray the obtained silica sol on the fiber felt. Each cubic centimeter of the fiber felt is sprayed with 0.5 mL of silica sol. After impregnation, it is aged at 40°C. After aging, it is dried at normal pressure: dried at 50°C, 80°C, 100°C, 150°C and 200°C for 4 hours, and then dried at 250°C to constant weight. The fiber felt is obtained by laying out quartz fibers, with a density of 0.12 g·cm -3 .
[0028] Example 2
[0029] This embodiment provides a method for preparing a fiber aerogel composite material, comprising the following steps:
[0030] The first step is to add tetraethyl orthosilicate and the flame retardant organosilane prepared according to the method in Example 1 to ethanol, stir and disperse, add water, adjust the pH value to 3 with dilute hydrochloric acid, fully hydrolyze for 8 hours, then add ammonia water to adjust the pH value to 8, carry out polymerization reaction, and react until the viscosity is 8 mPa·s to obtain silica sol; wherein the molar ratio of tetraethyl orthosilicate, ethanol and water is 0.05:1.5:1.5; the mass ratio of tetraethyl orthosilicate and flame retardant organosilane is 8:2.
[0031] The second step is to spray the obtained silica sol on the fiber felt. Each cubic centimeter of the fiber felt is sprayed with 0.5 mL of silica sol. After impregnation, it is aged at 40°C. After aging, it is dried at normal pressure: dried at 50°C, 80°C, 100°C, 150°C and 200°C for 4 hours, and then dried at 250°C to constant weight. The fiber felt is obtained by laying out quartz fibers, with a density of 0.12 g·cm -3 .
[0032] Example 3
[0033] This embodiment provides a method for preparing a fiber aerogel composite material, comprising the following steps:
[0034] The first step is to add tetraethyl orthosilicate and the flame retardant organosilane prepared according to the method in Example 1 to ethanol, stir and disperse, add water, adjust the pH value to 3 with dilute hydrochloric acid, fully hydrolyze for 8 hours, then add ammonia water to adjust the pH value to 8, carry out polymerization reaction, and react until the viscosity is 8 mPa·s to obtain silica sol; wherein the molar ratio of tetraethyl orthosilicate, ethanol and water is 0.05:1.5:1.5; the mass ratio of tetraethyl orthosilicate and flame retardant organosilane is 8:2.5.
[0035] The second step is to spray the obtained silica sol on the fiber felt. Each cubic centimeter of the fiber felt is sprayed with 0.5 mL of silica sol. After impregnation, it is aged at 40°C. After aging, it is dried at normal pressure: dried at 50°C, 80°C, 100°C, 150°C and 200°C for 4 hours, and then dried at 250°C to constant weight. The fiber felt is obtained by laying out quartz fibers, with a density of 0.12 g·cm -3 .
[0036] Example 4
[0037] Compared with Example 2, the dosage of tetraethyl orthosilicate and flame retardant organosilane is adjusted in this example, and the mass ratio of tetraethyl orthosilicate and flame retardant organosilane is 8:3; the other raw materials and preparation process are the same as those in Example 2.
[0038] Comparative Example 1
[0039] Compared with Example 2, this comparative example does not add flame retardant organosilane, and the remaining raw materials and preparation process remain the same as those in Example 2.
[0040] Comparative Example 2
[0041] Compared with Example 2, the flame retardant organic silane in this comparative example is replaced by a mixture of phenylphosphoryldecanediamine and 3-isocyanatepropyltrimethoxysilane of the same mass, wherein the molar ratio of phenylphosphoryldecanediamine to 3-isocyanatepropyltrimethoxysilane is 1:2, and the remaining raw materials and preparation process remain the same as in Example 2.
[0042] Performance tests were performed on Examples 1 to 4 and Comparative Examples 1 to 2;
[0043] Flame retardancy: tested according to UL-94 combustion rating;
[0044] Compression strength: The 20×20×20mm composite material sample was compressed at a loading rate of 1mm / min, and the compression direction was perpendicular to the fiber laying direction. Five samples were taken from each group of samples and the results were averaged. The calculation formula of the compression strength δ is as follows: δ=F / S; where F is the load and S is the compression area. Record and calculate the compression strength of the composite material sample at 3%, 5% and 10% deformation. The results are shown in Table 1:
[0045] Table 1
[0046]
[0047]
[0048] As can be seen from Table 1, by adding flame-retardant organosilane during the preparation process, the flame retardant properties of the composite material can be effectively improved. In addition, the introduction of benzene rings in the flame-retardant organosilane can reduce the degree of freedom of the silicone rubber molecular chain through its steric hindrance effect, thereby increasing the crosslinking density and then the strength; According to the results of the comparison between Example 2 and Comparative Example 2, it can be seen that the composite material obtained by mixing phenylphosphoryldecanediamine and 3-isocyanatepropyltrimethoxysilane with flame retardant effect has insufficient support strength. The reason is that the materials added in the form of a mixture have poor compatibility, resulting in the prepared fiber being in a relatively loose state, which also leads to a decrease in its flame retardant properties.
[0049] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.
[0050] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for preparing a fiber aerogel composite material, characterized in that: The steps include: The first step is to add ethyl orthosilicate and flame retardant organosilane into ethanol, stir and disperse, add water, adjust the pH value to 2-3 with dilute hydrochloric acid, fully hydrolyze, then add ammonia water to adjust the pH value to 7-8, perform polymerization reaction, and obtain silica sol; The second step is to spray the obtained silica sol to impregnate the fiber felt; after impregnation, the fiber felt is allowed to stand for aging at a temperature of 40°C; after aging, the fiber felt is dried at normal pressure.
2. The method for preparing a fiber aerogel composite material according to claim 1, characterized in that: In the first step, the molar ratio of tetraethyl orthosilicate, ethanol and water is 0.04-0.05:1.5:1.5; the mass ratio of tetraethyl orthosilicate and flame retardant organosilane is 8:2-3.
3. The method for preparing a fiber aerogel composite material according to claim 1, characterized in that: In the first step, polymerization is carried out until the viscosity reaches 6-8 mPa·s.
4. The method for preparing a fiber aerogel composite material according to claim 1, characterized in that: Each cubic centimeter of fiber felt is sprayed and impregnated with 0.5 mL of silica sol.
5. The method for preparing a fiber aerogel composite material according to claim 1, characterized in that: In the second step, the conditions for drying at normal pressure are: drying at 50° C., 80° C., 100° C., 150° C. and 200° C. for 4 h respectively, and then drying at 250° C. to constant weight.
6. The method for preparing a fiber aerogel composite material according to claim 1, characterized in that: The fiber felt is formed by laying out inorganic ceramic fibers or weaving fiber bundles.
7. The method for preparing a fiber aerogel composite material according to claim 6, characterized in that: The inorganic ceramic fiber is any one of quartz fiber, aluminum silicate fiber, zirconium oxide fiber, aluminum oxide fiber and mullite fiber.
8. The method for preparing a fiber aerogel composite material according to claim 1, characterized in that: The flame retardant organosilane is prepared by the following steps: Under nitrogen protection, phenylphosphoryldecanediamine was added to N,N-dimethylformamide, the temperature was set to 45°C, 3-isocyanatepropyltrimethoxysilane was added dropwise, the temperature was kept constant after the addition, and the reaction was continued with stirring for 4 hours to obtain a flame retardant organosilane; wherein the molar ratio of phenylphosphoryldecanediamine to 3-isocyanatepropyltrimethoxysilane was 1:2, and phenylphosphoryldecanediamine was obtained by condensation reaction of phenylphosphoryl dichloride and 1,10-decanediamine in a molar ratio of 1:2.