VOCs adsorbent and preparation method thereof
By regulating the pH value and optimizing the crystallization process, combining cerium ion exchange and silanization treatment, a 13X type molecular sieve with high silicon-aluminum ratio was prepared, which solved the problem of insufficient adsorption performance of existing VOCs adsorbents and achieved efficient and stable VOCs Adsorption effect.
Patent Information
- Application Number
- CN202410976190.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-19
AI Technical Summary
The specific surface area and pore capacity of existing VOCs adsorbents are small, making it difficult to meet the VOCs adsorption requirements.
By accurately adjusting the pH value during the reaction process, optimizing the crystallization and aging process, a 13X type molecular sieve with high silicon-aluminum ratio was prepared, and cerium ion exchange, alkali treatment and silanization treatment were performed to obtain VOCs adsorbent with excellent adsorption properties. .
It significantly improves the adsorption efficiency and stability of VOCs adsorbents, is suitable for industrial emissions and indoor air purification, and provides efficient and environmentally friendly VOCs removal technology.
Smart Images

Figure BDA0004954579230000101 
Figure BDA0004954579230000111
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of adsorption materials, and in particular to a VOCs adsorbent and a preparation method thereof. Background Art
[0002] Molecular sieve is a kind of aluminosilicate, which has the characteristics of uniform pore size, regular crystal structure, rich pore system, large specific surface area, and good thermal stability. It is considered to be the preferred adsorbent material for removing oxygen-containing compounds from olefins. Among them, FAU type (X, Y type) molecular sieve has a pore size of about 0.74nm. In particular, X type molecular sieve can better remove oxygen-containing compound impurities from olefins, and has been widely studied and applied in industrial practice.
[0003] 13X molecular sieve is a typical X-type molecular sieve, its chemical formula is Na2O·Al2O3·2.45SiO2·6.0H2O, and its pore size is The uniform and ordered microporous structure in its structure enables the 13X molecular sieve to achieve more precise molecular screening. The size and shape of the micropores can highly specifically adsorb molecules of a specific size and shape while excluding other molecules, which is very valuable in the separation and purification process in the chemical industry. For example, in the field of gas separation, the 13X molecular sieve can effectively separate target gases such as oxygen, nitrogen or carbon dioxide from a mixed gas flow. Secondly, the large specific surface area provides more active adsorption sites, increasing the adsorption capacity of the 13X molecular sieve. This means that within the same physical volume, the 13X molecular sieve can adsorb more substances, thereby improving the processing rate and efficiency. This feature is particularly important in the fields of liquid or gas purification, catalyst carriers, and storage media.
[0004] Therefore, the 13X molecular sieve, which has uniform and ordered micropores, large specific surface area and large pore capacity, not only shows great potential in the traditional fields of chemical industry, oil and gas processing, but also shows broad application prospects in emerging fields such as environmental protection, clean energy and life sciences. For example, in the production of pharmaceuticals and fine chemicals, 13X molecular sieve can be used to improve the purity and yield of products; in the treatment of industrial waste gas, it can be used as an adsorbent to effectively remove harmful gases and volatile organic compounds (VOCs).
[0005] At present, with the intensification of industrialization, the emission of VOCs in the air continues to increase, posing a serious threat to human health and the environment, and VOCs removal technology is also in urgent need of development. Commonly used VOCs removal technologies include adsorption, catalytic combustion, etc. Among them, the adsorption method is widely used because of its simple operation and low cost. As mentioned above, 13X molecular sieve has become the preferred adsorbent for VOCs removal due to its good thermal stability and large pore size. However, the traditional 13X molecular sieve still has room for improvement in the adsorption efficiency of certain VOCs.
[0006] Based on this, how to provide a VOCs adsorbent with large specific surface area, large pore volume and excellent VOCs adsorption performance and a preparation method thereof is one of the important issues faced in this field. Summary of the invention
[0007] The main purpose of the present invention is to provide a VOCs adsorbent and a preparation method thereof, so as to solve the problem that the existing VOCs adsorbent has a small specific surface area and pore capacity and is difficult to meet the VOCs adsorption requirements.
[0008] In order to achieve the above-mentioned purpose, the present invention provides a method for preparing a VOCs adsorbent, which comprises: step S1, mixing a silicon source and an aluminum source to obtain a mixture gel; step S2, adjusting the pH of the mixture gel to 8.5-12.5, and performing a first crystallization treatment to obtain a crystallized product; step S3, subjecting the crystallized product to an aging treatment and a second crystallization treatment in sequence to obtain a 13X molecular sieve; step S4, subjecting the 13X molecular sieve to a cerium ion exchange treatment, an alkali treatment and a silanization treatment in sequence to obtain a VOCs adsorbent.
[0009] Furthermore, in step S4, the cerium ion exchange treatment includes: immersing the 13X molecular sieve in a cerium ion solution, performing an ion exchange reaction, and drying after the reaction to obtain an ion exchange molecular sieve; the alkali treatment includes: immersing the ion exchange molecular sieve in an alkaline solution, performing an alkali treatment, and obtaining an alkali-treated molecular sieve after a first calcination; the silanization treatment includes: immersing the alkali-treated molecular sieve in an alcohol solution of silane, performing a silanization treatment, and obtaining a VOCs adsorbent after a second calcination.
[0010] Furthermore, the silicon source is selected from one or more of silica sol, tetraethyl orthosilicate, macroporous silica gel, silicon powder and white carbon black; the aluminum source is selected from one or more of sodium aluminate, pseudo-boehmite, aluminum sulfate and aluminum nitrate; the weight ratio of the silicon source to the aluminum source is (0.01-1.25):1.
[0011] Furthermore, the mixing process in step S1 is: mixing a silicon source and water to obtain a silicon-containing material, mixing an aluminum source and water to obtain an aluminum-containing material, and dropping the aluminum-containing material into the silicon-containing material to react to obtain a mixture gel; preferably, the reaction is carried out at 20 to 100° C. for 0.1 to 24 h; preferably, the dropping rate is 1 to 3 mL / min; more preferably, the dropping and reaction are both carried out under stirring conditions.
[0012] Furthermore, in step S2, the first crystallization treatment includes one-stage crystallization and two-stage crystallization; the temperature of the first-stage crystallization is 20-60°C, and the time is 4-24 hours; the temperature of the second-stage crystallization is 80-120°C, and the time is 6-48 hours; preferably, the temperature difference between the second-stage crystallization and the first-stage crystallization is ≥40°C.
[0013] Furthermore, in step S3, the aging reaction is to add the crystallized product to polyvinyl pyrrolidone and / or polyvinyl alcohol for aging; the temperature of the aging reaction is 20-100°C, and the time is 0.1-24h; the temperature of the second crystallization treatment is 60-105°C, and the time is 0.1-36h.
[0014] Furthermore, in step S4, the cerium ion solution is selected from one or more of cerium chloride, cerium nitrate, cerium citrate and cerium acetate; the molar concentration of cerium ions in the cerium ion solution is 0.48-0.52 mol / L; preferably, in the cerium ion solution, the amount of 13X molecular sieve added is 0.18-0.22 g / mL; preferably, the ion exchange reaction time is 22-26 h; preferably, the drying conditions are: 100-120°C, 6-24 h.
[0015] Furthermore, in step S4, the alkaline solution is selected from one or more of sodium hydroxide solution, potassium hydroxide solution and ammonia solution; the molar concentration of the alkaline solution is 2-2.5 mol / L; preferably, the alkali treatment time is 1-3 h; preferably, the conditions of the first calcination are: 400-600° C., 4-8 h.
[0016] Furthermore, in step S4, the silane is selected from one or more of ethyltriethoxysilane, methyltrimethoxysilane and acryltrimethoxysilane, and the alcohol is selected from one or more of ethanol, propanol and butanol; preferably, in the alcohol solution of silane, the volume ratio of silane to alcohol is 1:(8-10); preferably, the time of silanization treatment is 12-24h; preferably, the conditions of the second calcination are: 500-700°C, 2-4h.
[0017] Another aspect of the present invention provides a VOCs adsorbent, which is prepared by the above preparation method.
[0018] By applying the technical solution of the present invention, a molecular sieve with a high silicon-aluminum ratio, excellent specific surface area and pore capacity is first obtained by precisely controlling the pH value during the reaction and optimizing the design of the crystallization and aging process, and then the obtained molecular sieve is further subjected to cerium ion exchange treatment, alkali treatment and silanization treatment to obtain a VOCS adsorbent. The obtained VOCS adsorbent has excellent physical and chemical properties and environmental adaptability, and is suitable for environmental protection applications in multiple fields, especially industrial emissions and indoor air purification, providing an efficient and environmentally friendly technical solution for effectively controlling and reducing VOCs pollution. DETAILED DESCRIPTION
[0019] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below in conjunction with the embodiments.
[0020] As described in the background technology, there is a problem in the prior art that the specific surface area and pore volume of VOCs adsorbents are small, and it is difficult to meet the VOCs adsorption requirements. In order to solve the above technical problems, the present application provides a method for preparing a VOCs adsorbent, which comprises: step S1, mixing a silicon source and an aluminum source to obtain a mixture gel; step S2, adjusting the pH of the mixture gel to 8.5-12.5, and performing a first crystallization treatment to obtain a crystallized product; step S3, subjecting the crystallized product to an aging treatment and a second crystallization treatment in sequence to obtain a 13X molecular sieve; step S4, subjecting the 13X molecular sieve to a cerium ion exchange treatment, an alkali treatment and a silanization treatment in sequence to obtain a VOCs adsorbent.
[0021] The present invention first prepares the molecular sieve by precisely controlling the pH value during the reaction process and optimizing the design of the crystallization and aging process. Specifically, after obtaining the mixture gel, the pH value is adjusted to 8.5-12.5, so that the silicon source and the aluminum source can be better mixed and reacted, thereby improving the silicon-aluminum ratio, specific surface area and pore capacity of the molecular sieve; the first crystallization treatment obtains a crystallized product, so that the crystal form of the molecular sieve is more complete and uniform, and the obtained crystallized product is aged to further optimize the crystal form and improve the structural stability, thereby improving the adsorption performance of the molecular sieve, and finally the second crystallization treatment is performed, which can further improve the integrity and uniformity of the molecular sieve crystal form, and ultimately improve the silicon-aluminum ratio, specific surface area and pore capacity of the molecular sieve. For the obtained 13X molecular sieve, cerium ions are introduced through ion exchange, one is to increase the specific surface area and pore volume of the molecular sieve, and the other is to increase the adsorption active sites; and, compared with other types of rare earth elements or transition metal elements, cerium has a unique 4f electronic structure. In the technical scheme of the present invention, it has a special role in adjusting the pore size of the molecular sieve and enhancing the adsorption activity, thereby being able to more effectively improve the adsorption efficiency of VOCs. Alkaline treatment is used to remove impurities that may be introduced during the ion exchange process, and the stability is effectively improved. Finally, through silanization treatment, siloxane groups are introduced to increase the service life. By strictly controlling the above process flow, a VOCs adsorbent with excellent adsorption and stability is obtained. The obtained 13X molecular sieve has a high silicon-aluminum ratio, a high silicon source utilization rate, and good selectivity. It can be regulated according to different adsorption molecules, thereby significantly reducing the carbon deposition rate of the molecular sieve and improving the diffusion performance of the adsorbent, thereby meeting the VOCs adsorption requirements in multiple fields.
[0022] In a typical embodiment, in step S4, the cerium ion exchange treatment includes: immersing the 13X molecular sieve in a cerium ion solution, performing an ion exchange reaction, and drying after the reaction to obtain an ion exchange molecular sieve; the alkali treatment includes: immersing the ion exchange molecular sieve in an alkaline solution, performing an alkali treatment, and obtaining an alkali-treated molecular sieve after a first calcination; the silanization treatment includes: immersing the alkali-treated molecular sieve in an alcohol solution of silane, performing a silanization treatment, and obtaining a VOCs adsorbent after a second calcination. For the obtained 13X molecular sieve, the cerium ion exchange treatment, alkali treatment and silanization treatment are sequentially performed in the above manner, which can significantly improve the adsorption performance and stability of the obtained VOCs adsorbent. Among them, the ion exchange reaction is carried out in a cerium ion solution, which can improve the efficiency of ion exchange, introduce as many adsorption active sites as possible, and optimize the pore structure; calcination after alkali treatment can remove moisture or organic matter introduced during the treatment process, which is beneficial to the subsequent silanization treatment, thereby effectively improving the structural stability; calcination again after silanization treatment is beneficial to the effective formation of a coating by the siloxane groups adsorbed during the silanization treatment, that is, providing a stable protective layer for the high pore capacity molecular sieve containing active sites, thereby improving its stability in use.
[0023] In the preparation process of 13X molecular sieve, in order to obtain a molecular sieve with a stable structure and a high silicon-aluminum ratio, in a preferred embodiment, the silicon source is selected from one or more of silica sol, tetraethyl orthosilicate, coarse-pore silica gel, silicon powder and white carbon black; the aluminum source is selected from one or more of sodium aluminate, pseudo-boehmite, aluminum sulfate and aluminum nitrate; the weight ratio of the silicon source to the aluminum source is (0.01-1.25):1. Specifically, the coarse-pore silica gel is C-type silica gel, and its chemical formula is mSiO2·nH2O. In principle, the silicon source and the aluminum source can use conventional types in the art, but the inventors have found through a large number of experiments that when the above-mentioned silicon sources and aluminum sources are mixed at a weight ratio of (0.01-1.25):1, the molecular sieve finally obtained has a higher silicon-aluminum ratio and a better pore structure, so that a VOCs adsorbent with excellent adsorption properties can be obtained in the subsequent preparation process.
[0024] On the basis of the above-mentioned silicon source and aluminum source, further, the process of mixing the two includes: mixing the silicon source and water to obtain a silicon-containing material, and mixing the aluminum source and water to obtain an aluminum-containing material; wherein the mixing of the silicon source and the water is completed after stirring at 20 to 60° C. for 0.1 to 12 hours, and the stirring speed is maintained at 200 to 800 rpm, and the concentration of the obtained silicon-containing material is 2 to 99 wt%; the mixing of the aluminum source and the water is completed after stirring at 20 to 60° C. for 0.1 to 12 hours, and the stirring speed is maintained at 200 to 800 rpm, and the concentration of the obtained silicon-containing material is 40 to 60 wt%. The aluminum-containing material is added dropwise to the silicon-containing material to react to obtain a mixed gel. The aluminum-containing material prepared according to the above conditions has better compatibility with the silicon-containing material, which is more convenient for the reaction between the two, and is more conducive to the formation of a 13X molecular sieve with a high aluminum-silicon ratio; in order to make the reaction more fully carried out, it is preferred that the reaction be carried out at 20 to 100 ° C for 0.1 to 24 hours; and, in order to make the contact between the silicon source and the aluminum source more sufficient during the reaction, the inventor has preferably added a dripping speed of 1 to 3 mL / min after a large number of experiments. Slow dripping at the above speed is conducive to more sufficient contact between the silicon source and the aluminum source during the reaction, thereby improving the synthesis yield and quality of the molecular sieve. In a more preferred embodiment, the dripping and reaction are both carried out under stirring conditions, so that the mixing and reaction of the silicon source and the aluminum source are more sufficient, thereby improving the synthesis yield of the 13X molecular sieve.
[0025] In a typical embodiment, in step S2, the first crystallization treatment includes one-stage crystallization and two-stage crystallization; the temperature of the first stage crystallization is 20-60°C and the time is 4-24h; the temperature of the second stage crystallization is 80-120°C and the time is 6-48h; the first crystallization treatment is carried out in stages, which can further optimize the structure of the obtained crystallized product and improve its stability; the inventors have optimized the conditions of the above two-stage crystallization treatments through a large number of experiments, and found that crystallization under these conditions can better play the role of the two-stage crystallization, making the structure more complete and the crystal form more uniform. And, more preferably, the temperature difference between the second stage crystallization and the first stage crystallization is ≥40°C. After a large number of experiments, the inventors found that when the temperature difference between the second stage crystallization and the first stage crystallization is ≥40°C, the molar ratio of each component in the crystallized product can be further optimized, thereby effectively improving the adsorption.
[0026] During the first and second crystallization processes, the alkaline mixture gel undergoes structural rearrangement, and its structure gradually transforms into an ordered crystalline state, forming a molecular sieve with a specific pore structure. In a preferred embodiment, the molar ratio of each component in the crystallization product is: SiO2 / Al2O3=(0.01-6):1, Na2O / SiO2=(0.01-4.0):1, H2O / SiO2=(1.0-50.0):1. The crystallization product under this composition exhibits higher adsorption activity when a VOCs adsorbent is obtained through a subsequent preparation process.
[0027] In the technical solution provided by the present invention, after obtaining the crystallized product, it also includes aging the crystallized product. In a preferred embodiment, the aging reaction in step S3 is to add the crystallized product to polyvinyl pyrrolidone and / or polyvinyl alcohol for aging, and the temperature of the aging reaction is 20-100°C, and the time is 0.1-24h; because polyvinyl pyrrolidone and / or polyvinyl alcohol can be used as structure directing agents and crystal growth regulators, aging under the above conditions can further assist crystallization, optimize the crystal form, and significantly improve the structural stability of the obtained molecular sieve; at the same time, the inventors, through a large number of experiments, preferably the temperature of the second crystallization treatment is 60-105°C, and the time is 0.1-36h, and it is found that under this condition, a 13X molecular sieve with a more uniform crystal structure, a more uniform size, and a better specific surface area and pore structure is obtained.
[0028] In a preferred embodiment, the pH of the mixture gel in step S2 is 12, the temperature of the first crystallization is 40°C, the time is 12h, the temperature of the second crystallization is 95°C, the time is 24h, and the molar ratio of each component in the obtained crystallization product is: SiO2 / Al2O3=1.5:1, Na2O / SiO2=1.6:1, H2O / SiO2=32:1. The inventor has optimized this condition through a large number of experiments and found that the pore size arrangement of the VOCs adsorbent obtained at this time is more uniform, the specific surface area and pore volume are larger, and the performance is more excellent.
[0029] In several preferred embodiments, the silicon-aluminum ratio of the 13X molecular sieve is 2.2 to 2.9, and the pore volume is 0.35 to 0.5 cm 3 / g, specific surface area is 750~950m 2 / g, the molecular sieve with the above physicochemical properties obtained by the present invention, when prepared through the subsequent process flow to obtain the VOCs adsorbent, exhibits higher adsorption and stability, and can precisely control the adsorption target object.
[0030] In the process of ion exchange reaction, further, the cerium ion solution used is selected from one or more of cerium chloride, cerium nitrate, cerium citrate and cerium acetate; the molar concentration of cerium ions in the cerium ion solution is 0.48-0.52 mol / L; in principle, the cerium ion solution can be selected from the types commonly used in the art, and its concentration can also be adjusted arbitrarily, but for the reaction system in the technical solution provided by the present invention, the inventors have selected the above-mentioned types of cerium ion solutions and a molar concentration of cerium ions of 0.48-0.52 mol / L after a large number of experiments, and found that the cerium ion solution prepared under these conditions can make the obtained 13X type molecular sieve better dispersed therein, thereby increasing the probability of cerium ions entering the 13X pores and adsorbing, more effectively optimizing the pore structure, increasing the number of active sites, and ultimately showing higher adsorption. In order to make the 13X molecular sieve disperse more evenly and enhance the modification, it is preferred that the amount of 13X molecular sieve added to the cerium ion solution is 0.18-0.22 g / mL; and in order to make the ion exchange reaction more fully and obtain more active sites, the ion exchange reaction time is preferably 22-26 hours. After the ion exchange reaction, the obtained ion exchange molecular sieve is dried. In a preferred embodiment, the drying conditions are: 100-120°C, 6-24 hours, so as to effectively remove moisture and better protect the structure.
[0031] During the alkali treatment process, the alkaline solution is selected from one or more of sodium hydroxide solution, potassium hydroxide solution and ammonia solution; the molar concentration of the alkaline solution is 2-2.5 mol / L. Similarly, the type and concentration of the alkaline solution can be conventionally selected in principle, but after the above-mentioned alkaline solutions are introduced into the reaction system of the present invention at the above-mentioned molar concentration, they can be better adapted to the ion exchange molecular sieve at this time, thereby improving the effect of the alkali treatment; further preferably, the alkali treatment time is 1-3 hours, which is more conducive to the optimization of the pore structure; after the alkali treatment, the first calcination is performed so that the introduced Ce element can be better dispersed in the molecular sieve pores and its structure is optimized. In a typical embodiment, the conditions of the first calcination are: 400-600°C, 4-8 hours, so as to more effectively optimize the electronic structure and coordination environment of the Ce element, so that it can more accurately regulate the pore structure of the molecular sieve and improve the adsorption.
[0032] During the silanization treatment, the silane is selected from one or more of ethyltriethoxysilane, methyltrimethoxysilane and propenyltrimethoxysilane. Compared with other types of silane, these types of silane have better affinity with the surface of the alkali-treated molecular sieve, thereby achieving more effective adsorption, which is conducive to forming a complete and high-coverage protective layer. The alcohol is selected from one or more of ethanol, propanol and butanol; in a typical embodiment, the volume ratio of silane to alcohol in the alcohol solution of silane is 1: (8-10), so that the alkali-treated molecular sieve can be better dispersed therein and the contact between silane and the alkali-treated molecular sieve is enhanced; more preferably, the silanization treatment time is 12-24 hours to make the silanization more sufficient; preferably, the conditions for the second calcination are: 500-700°C, 2-4 hours.
[0033] Another aspect of the present invention provides a VOCs adsorbent, which is prepared by the above preparation method. The obtained VOCs adsorbent has excellent physical and chemical properties and environmental adaptability, and is suitable for a variety of environments, especially industrial emissions and indoor air purification, thereby providing an effective technical solution and technical support for the adsorption of VOCs.
[0034] The VOCs adsorbent prepared by the present invention has a good adsorption effect on coal gasification waste gas, petrochemical waste gas, etc., especially chemical waste gas with ethylene as the main component.
[0035] The present application is further described in detail below in conjunction with specific embodiments. These embodiments should not be construed as limiting the scope of protection claimed in the present application.
[0036] Unless otherwise defined, all professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.
[0037] Example 1
[0038] A method for preparing a VOCs adsorbent:
[0039] 1. Preparation of 13X molecular sieve:
[0040] 21.0g silica sol (mass fraction of 30%) was dissolved in 36.0g deionized water, and pretreated at 25°C in a closed reactor for 1 hour to obtain a silicon-containing material; 24g aluminum sulfate was dissolved in 18.0g deionized water, and stirred at 25°C for 1 hour to obtain an aluminum-containing material; the aluminum-containing material was slowly added dropwise to the silicon-containing material (the dropping speed was 1mL / min), and continued to stir at 60°C for 8 hours to obtain a mixture gel; 6.74g sodium hydroxide was dissolved in 36g deionized water dispersion and added to the mixture gel until the pH value was 12 to obtain a gel slurry solution, which was placed in a hydrothermal reactor for two-stage control. Warm crystallization, the first stage crystallization temperature is 40°C, the time is 12 hours, the second stage crystallization temperature is 95°C, the time is 24 hours, and a 13X crystallized product is obtained (the molar ratio of each component is: SiO2 / Al2O3=1.5:1, Na2O / SiO2=1.6:1, H2O / SiO2=32:1); the crystallized product is mixed with 1g of polyvinyl pyrrolidone, and then stirred and aged at 60°C for 12h, and then placed in a hydrothermal reactor at a crystallization temperature of 98°C for 24h for final crystallization, and the obtained product is filtered and washed to pH 7, and dried at 90°C to obtain a 13X molecular sieve.
[0041] 2. Preparation of VOCs adsorbent:
[0042] Take 50g of the 13X molecular sieve prepared in Example 1 after drying (drying conditions are 80°C, 12h), soak it in 250mL of 0.5mol / L cerium nitrate (Ce(NO3)3) solution for 24 hours of ion exchange reaction, and then dry it at 110°C for 12 hours to obtain an ion exchange molecular sieve. Then soak the ion exchange molecular sieve in a 2mol / L sodium hydroxide (NaOH) solution for 2 hours, and then calcine it at 500°C for 4 hours in air to obtain an alkali-treated molecular sieve. After that, soak the alkali-treated molecular sieve in a mixed solution containing 50mL ethyltriethoxysilane (TEOS) and 450mL ethanol for 12 hours, dry it again, and calcine it at 600°C for 3 hours to form a VOCs adsorbent.
[0043] Example 2
[0044] A method for preparing a VOCs adsorbent:
[0045] 1. Preparation of 13X molecular sieve:
[0046] 1g of silicon powder was dissolved in 18g of deionized water, and pretreated at 25°C in a closed reactor for 1 hour to obtain a silicon-containing material; at the same time, 12g of aluminum nitrate was dissolved in 18.0g of deionized water, and stirred at 35°C for 1 hour to prepare an aluminum-containing material. The prepared aluminum-containing material was slowly added dropwise to the silicon-containing material (the dropping speed was 2mL / min), and continued to stir at 50°C for 6 hours to obtain a mixture gel; 2g of sodium hydroxide was dissolved in 36g of deionized water to obtain a dispersion, and added to the mixture gel until the pH value was 11.8 to obtain a gel slurry solution, which was then transferred to a hydrothermal reactor to perform a two-stage temperature-controlled crystallization process: the first stage crystallization temperature was set at 50°C and lasted for 14 hours; the second stage crystallization temperature was controlled at 100°C and maintained for 14 hours. The mixture was kept for 18 hours to obtain a 13X crystallized product (wherein the molar ratio of each component is: SiO2 / Al2O3=0.6:1, Na2O / SiO2=3:1, H2O / SiO2=20:1); the crystallized product was mixed with 1 g of polyvinyl alcohol, and then stirred and aged at 60°C for 12 hours, and then placed in a hydrothermal reactor at a crystallization temperature of 95°C for 24 hours for final crystallization. The obtained product was filtered and washed to a pH of 7, and dried at 90°C to obtain a 13X molecular sieve.
[0047] 2. Preparation of VOCs adsorbent: The 13X molecular sieve prepared in Example 1 was replaced with the 13X molecular sieve prepared in this example, and the other conditions were the same as in Example 1.
[0048] Example 3
[0049] A method for preparing a VOCs adsorbent:
[0050] 1. Preparation of 13X molecular sieve:
[0051] 0.17g silicon powder was dissolved in 6g deionized water, and pretreated at 25°C for 1 hour in a sealed reactor to obtain a silicon-containing material; at the same time, 12g aluminum nitrate was dissolved in 18.0g deionized water, and stirred at 35°C for 1 hour to prepare an aluminum-containing material liquid. The aluminum-containing material was slowly added to the silicon-containing material (the drop rate was 1mL / min), and stirred at 100°C for 24 hours to obtain a mixture gel; 0.9g sodium hydroxide was dissolved in 6g deionized water to prepare a dispersion, and added to the mixture gel until the pH value was 12.5 to obtain a gel slurry solution, which was then transferred to a hydrothermal reactor for two-stage crystallization. First, crystallization was continued at 60°C for 24 hours, and then the temperature was increased to 120°C for crystallization reaction for 48 hours to obtain. To obtain a 13X crystallized product (wherein the molar ratio of each component is: SiO2 / Al2O3=0.1:1, Na2O / SiO2=4:1, H2O / SiO2=1:1); the crystallized product is mixed with 1g of polyvinyl alcohol, and then stirred and aged at 60°C for 12h, and then placed in a hydrothermal reactor at a crystallization temperature of 105°C and a time of 20h for final crystallization. The obtained product is filtered and washed to a pH of 7, and dried at 90°C to obtain a 13X molecular sieve.
[0052] 2. Preparation of VOCs adsorbent: The 13X molecular sieve prepared in Example 1 was replaced with the 13X molecular sieve prepared in this example, and the other conditions were the same as in Example 1.
[0053] Example 4
[0054] A method for preparing a VOCs adsorbent:
[0055] 1. Preparation of 13X molecular sieve:
[0056] Take 14.65g of ethyl orthosilicate and 36g of deionized water in a volume ratio of 1:1, and pretreat at 25°C in a closed reactor for 1 hour to obtain a silicon-containing material. At the same time, dissolve 12g of aluminum nitrate in 18.0g of deionized water and stir at 35°C for 1 hour to obtain an aluminum-containing material. After that, gradually add the aluminum-containing material dropwise to the silicon-containing material (the dropping speed is 3mL / min), and mix and stir at 20°C for 0.1 hour to prepare a mixture gel; dissolve 0.56g of sodium hydroxide in 6g of deionized water as a dispersion liquid, pour it into the mixture gel until the pH value is 8.5, obtain a gel slurry solution, and then transfer it to a hydrothermal reactor to perform a segmented crystallization reaction: first set the crystallization temperature to 20°C for 4 hours; then increase it to 80°C and maintain crystallization for 6 hours , and obtain a 13X crystallized product (wherein the molar ratio of each component is: SiO2 / Al2O3=2.5:1, Na2O / SiO2=0.1:1, H2O / SiO2=40:1); the crystallized product is mixed with 1g of polyvinyl alcohol, and then stirred and aged at 70°C for 15h, and then placed in a hydrothermal reactor at a crystallization temperature of 115°C and a time of 16h for final crystallization. The obtained product is filtered and washed to a pH of 7, and dried at 90°C to obtain a 13X molecular sieve.
[0057] 2. Preparation of VOCs adsorbent: The 13X molecular sieve prepared in Example 1 was replaced with the 13X molecular sieve prepared in this example, and the other conditions were the same as in Example 1.
[0058] Example 5
[0059] A method for preparing a VOCs adsorbent:
[0060] 1. The preparation process of 13X molecular sieve differs from that of Example 1 only in that: no two-stage crystallization is set, but the gel slurry solution is placed in a hydrothermal reactor, and the crystallization temperature is only 95° C. and the time is 24 hours to directly obtain the 13X crystallized product.
[0061] 2. Preparation of VOCs adsorbent: The 13X molecular sieve prepared in Example 1 was replaced with the 13X molecular sieve prepared in this example, and the other conditions were the same as in Example 1.
[0062] Example 6
[0063] A method for preparing a VOCs adsorbent:
[0064] 1. The preparation process of 13X molecular sieve is different from that of Example 1 only in that the two stages of crystallization conditions are different. In this example, the first stage of crystallization is at a temperature of 70° C. and a time of 3 hours, and the second stage of crystallization is at a temperature of 130° C. and a time of 5 hours.
[0065] 2. Preparation of VOCs adsorbent: The 13X molecular sieve prepared in Example 1 was replaced with the 13X molecular sieve prepared in this example, and the other conditions were the same as in Example 1.
[0066] Example 7
[0067] A method for preparing a VOCs adsorbent:
[0068] 1. Preparation of 13X molecular sieve: same as in Example 1.
[0069] 2. The preparation process of the VOCs adsorbent differs from that of Example 1 only in that the amount of 13X molecular sieve used is 37.5 g (ie, the amount of 13X molecular sieve added to the cerium ion solution is 0.15 g / mL), and the ion exchange reaction time is 20 h.
[0070] Example 8
[0071] A method for preparing a VOCs adsorbent:
[0072] 1. Preparation of 13X molecular sieve: same as in Example 1.
[0073] 2. The preparation process of the VOCs adsorbent differs from that of Example 1 only in that the amount of 13X molecular sieve used is 62.5 g (ie, the amount of 13X molecular sieve added to the cerium ion solution is 0.25 g / mL), and the ion exchange reaction time is 28 h.
[0074] Comparative Example 1
[0075] A method for preparing a VOCs adsorbent:
[0076] The only difference between this comparative example and Example 1 is that: no 13X molecular sieve is prepared, but 50 g of 5A molecular sieve is directly used to replace the 13X molecular sieve to prepare the VOCs adsorbent.
[0077] Comparative Example 2
[0078] A method for preparing a VOCs adsorbent:
[0079] 1. Preparation of 13X molecular sieve: same as in Example 1.
[0080] 2. The preparation process of the VOCs adsorbent differs from that of Example 1 only in that, in the ion exchange reaction step, cerium nitrate (Ce(NO3)3) solution is not used, but lanthanum nitrate (La(NO3)3) solution of the same volume and molar concentration is used.
[0081] Comparative Example 3
[0082] A method for preparing a VOCs adsorbent:
[0083] 1. Preparation of 13X molecular sieve: same as in Example 1.
[0084] 2. The preparation process of the VOCs adsorbent is different from that of Example 1 only in that the alkali-treated molecular sieve obtained after the alkali treatment is not subjected to silanization treatment, but is directly used as the VOCs adsorbent.
[0085] Comparative Example 4
[0086] A method for preparing a VOCs adsorbent:
[0087] 1. The preparation process of 13X molecular sieve is different from that of Example 1 only in that during the process of adjusting the pH value of the mixture gel with sodium hydroxide solution, the pH value of the mixture gel is adjusted to 13.5 to obtain a gel slurry solution.
[0088] 2. Preparation of VOCs adsorbent: The 13X molecular sieve prepared in Example 1 was replaced with the 13X molecular sieve prepared in this comparative example, and the other conditions were the same as in Example 1.
[0089] Comparative Example 5
[0090] A method for preparing a VOCs adsorbent:
[0091] 1. The preparation process of 13X molecular sieve is different from that of Example 1 only in that during the process of adjusting the pH value of the mixture gel by using sodium hydroxide solution, the pH value of the mixture gel is adjusted to 7.5 to obtain a gel slurry solution.
[0092] 2. Preparation of VOCs adsorbent: The 13X molecular sieve prepared in Example 1 was replaced with the 13X molecular sieve prepared in this comparative example, and the other conditions were the same as in Example 1.
[0093] Comparative Example 6
[0094] A method for preparing a VOCs adsorbent:
[0095] 1. Preparation of 13X molecular sieve: same as in Example 1.
[0096] 2. Preparation of VOCs adsorbent: Take 50g of the 13X molecular sieve prepared in Example 1 after drying (drying conditions are 80°C, 12h), soak it in a mixed solution containing 50mL ethyltriethoxysilane (TEOS) and 450mL ethanol for 12 hours, dry it again and calcine it at 600°C for 3 hours to obtain a silanized molecular sieve. Then soak the silanized molecular sieve in a 2mol / L sodium hydroxide (NaOH) solution for 2 hours, and then calcine it at 500°C for 4 hours in air to obtain an alkali-treated molecular sieve. After that, soak the alkali-treated molecular sieve in 250mL of 0.5mol / L cerium nitrate (Ce(NO3)3) solution for 24 hours of ion exchange reaction, and then dry it at 110°C for 12 hours to form a VOCs adsorbent.
[0097] That is, the only difference between this comparative example and Example 1 is that the steps of silanization treatment and cerium ion exchange treatment are swapped.
[0098] Performance Test:
[0099] The silicon-aluminum ratio of 13X molecular sieve is measured by X-ray fluorescence spectrometry (XRF).
[0100] Pore capacity of 13X molecular sieve and VOCs adsorbent: BET test method.
[0101] Specific surface area of 13X molecular sieve and VOCs adsorbent: BET test method.
[0102] Adsorption performance of VOCs adsorbent: Fixed bed adsorption experiment: Ethylene is taken as the adsorption object, passed through a fixed bed containing adsorbent, and the concentration changes through the bed are monitored. The adsorption capacity is determined by the weight of adsorbed ethylene (mg) / weight of adsorbent (g), and the unit is mg / g.
[0103] The various properties of the 13X molecular sieve and VOCs adsorbent obtained in the above embodiments and comparative examples were tested respectively, and the results are shown in Table 1.
[0104] Table 1
[0105]
[0106]
[0107] From the above description, it can be seen that the above embodiments of the present invention achieve the synthesis of molecular sieves with high silicon-aluminum ratio, excellent specific surface area and pore capacity, and obtain VOCS adsorbents with excellent physicochemical properties and adsorption performance.
[0108] It should be noted that the terms "first", "second", etc. in the specification and claims of the present application are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the terms used in this way can be interchangeable where appropriate, so that the embodiments of the present application described herein can be implemented in an order other than those described herein, for example.
[0109] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a VOCs adsorbent, characterized in that: The preparation method of the VOCs adsorbent comprises: Step S1, mixing a silicon source and an aluminum source to obtain a mixture gel; Step S2, adjusting the pH of the mixture gel to 8.5-12.5, and then performing a first crystallization treatment to obtain a crystallized product; Step S3, subjecting the crystallized product to an aging treatment and a second crystallization treatment in sequence to obtain a 13X molecular sieve; Step S4, subjecting the 13X molecular sieve to cerium ion exchange treatment, alkali treatment and silanization treatment in sequence to obtain the VOCs adsorbent.
2. The method for preparing a VOCs adsorbent according to claim 1, characterized in that: In step S4: The cerium ion exchange treatment comprises: immersing the 13X molecular sieve in a cerium ion solution to perform an ion exchange reaction, and drying after the reaction to obtain an ion exchange molecular sieve; The alkali treatment comprises: soaking the ion exchange molecular sieve in an alkaline solution, performing the alkali treatment, and obtaining the alkali treated molecular sieve after a first calcination; The silanization treatment comprises: immersing the alkali-treated molecular sieve in an alcohol solution of silane, performing the silanization treatment, and obtaining the VOCs adsorbent after a second calcination.
3. The method for preparing a VOCs adsorbent according to claim 1 or 2, characterized in that: The silicon source is selected from one or more of silica sol, tetraethyl orthosilicate, macroporous silica gel, silicon powder and white carbon black; the aluminum source is selected from one or more of sodium aluminate, pseudo-boehmite, aluminum sulfate and aluminum nitrate; the weight ratio of the silicon source to the aluminum source is (0.01-1.25):
1.
4. The method for preparing a VOCs adsorbent according to any one of claims 1 to 3, characterized in that: The mixing process in step S1 is: mixing the silicon source and water to obtain a silicon-containing material, mixing the aluminum source and water to obtain an aluminum-containing material, and dropping the aluminum-containing material into the silicon-containing material to react to obtain the mixture gel; Preferably, the reaction is carried out at 20 to 100° C. for 0.1 to 24 h; Preferably, the dripping speed is 1 to 3 mL / min; More preferably, the dropping and the reaction are both carried out under stirring conditions.
5. The method for preparing a VOCs adsorbent according to any one of claims 1 to 4, characterized in that: In step S2, the first crystallization process includes a first stage crystallization and a second stage crystallization; The temperature of the first stage of crystallization is 20 to 60° C. and the time is 4 to 24 hours; The temperature of the second stage crystallization is 80-120°C and the time is 6-48h; Preferably, the temperature difference between the second-stage crystallization and the first-stage crystallization is ≥40°C.
6. The method for preparing a VOCs adsorbent according to any one of claims 1 to 5, characterized in that: In step S3, The aging reaction is to add the crystallized product into polyvinyl pyrrolidone and / or polyvinyl alcohol for aging; the aging reaction temperature is 20 to 100° C. and the time is 0.1 to 24 hours; The temperature of the second crystallization treatment is 60-105° C., and the time is 0.1-36 hours.
7. The method for preparing a VOCs adsorbent according to claim 2, characterized in that: The cerium ion solution in step S4 is selected from one or more of cerium chloride, cerium nitrate, cerium citrate and cerium acetate; the molar concentration of cerium ions in the cerium ion solution is 0.48-0.52 mol / L; Preferably, in the cerium ion solution, the amount of the 13X molecular sieve added is 0.18 to 0.22 g / mL; Preferably, the ion exchange reaction time is 22 to 26 hours; Preferably, the drying conditions are: 100-120° C., 6-24 h.
8. The method for preparing a VOCs adsorbent according to claim 2 or 7, characterized in that: The alkaline solution in step S4 is selected from one or more of sodium hydroxide solution, potassium hydroxide solution and ammonia solution; the molar concentration of the alkaline solution is 2-2.5 mol / L; Preferably, the alkali treatment time is 1 to 3 hours; Preferably, the first calcination is carried out at 400-600° C. for 4-8 hours.
9. The method for preparing a VOCs adsorbent according to claim 2, 7 or 8, characterized in that: In step S4, the silane is selected from one or more of ethyltriethoxysilane, methyltrimethoxysilane and propenyltrimethoxysilane, and the alcohol is selected from one or more of ethanol, propanol and butanol; Preferably, in the alcohol solution of silane, the volume ratio of the silane to the alcohol is 1:(8-10); Preferably, the silanization treatment time is 12 to 24 hours; Preferably, the second calcination is carried out at 500-700° C. for 2-4 h.
10. A VOCs adsorbent, characterized in that: The VOCs adsorbent is prepared by the preparation method described in any one of claims 1 to 9.
Citation Information
Patent Citations
Preparation method for small-grain Y type molecular sieve
CN104828838A
Preparation method for small-grain Y type molecular sieve
CN104828839A
Modified X-type molecular sieve with low silica-alumina ratio, and preparation method and application thereof
CN108117090A
Hierarchical pore ZSM-5 molecular sieve for VOCs adsorption and preparation method and application thereof
CN115259177A
Preparation method of semiconductor VOCs waste gas adsorbent
CN116251564A