Adsorbent precursor for lithium ion recovery, preparation method and adsorbent
By depositing a dense carbon film in the titanium adsorbent, the stability problem during desorption of titanium adsorbent is solved, its service life and lithium ion adsorption capacity are improved, and it is suitable for a variety of lithium resource recovery scenarios.
Patent Information
- Application Number
- CN202411037566.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-31
AI Technical Summary
Titanium-based adsorbents are prone to dissolving, rupture or collapse when desorbing in solution, affecting their recycling life.
A dense carbon film is deposited in a titanium-based adsorbent by chemical vapor deposition. By mixing the titanium source and the lithium source at high temperature and reacting with the gaseous carbon source, a stable adsorbent precursor is formed and activated by acid liquid. Adsorbent recovered from lithium ions.
It significantly improves the service life and stability of the adsorbent, reduces the chemical interface reaction of Ti, and enhances the adsorption capacity of lithium ions. It is suitable for the extraction and recycling of salt lake brine, lithium deposited mother liquor and lithium waste liquid.
Smart Images

Figure BDA0004971509010000071
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of lithium extraction from salt lakes, and specifically to an adsorbent precursor, a preparation method and an adsorbent for lithium ion recovery. Background Art
[0002] my country has huge reserves of lithium resources, and the Qinghai and Tibet salt lakes have rich lithium resources. In the technology of lithium extraction from salt lakes, lithium adsorbents play a vital role. Lithium adsorbents can effectively and selectively adsorb lithium ions from brine and separate them from other metal ions such as magnesium ions. At present, the lithium adsorbents used in China are mainly divided into organic adsorbents and inorganic adsorbents. Inorganic adsorbents can be further divided into ion sieve adsorbents, titanium adsorbents and natural mineral adsorbents.
[0003] Titanium-based adsorbents are new adsorbents for lithium extraction from salt lakes. Their main application system is the hydrochloric acid desorption system. The core skeleton of titanium-based adsorbents is prone to dissolution, rupture or collapse when desorbed in the solution, which seriously affects the recycling of the adsorbent. Therefore, it is necessary to design a titanium-based adsorbent with a long service life. Summary of the invention
[0004] The purpose of the present application is to provide a titanium-based adsorbent with a long service life.
[0005] To achieve the above objectives, the technical solution adopted in the present application is: to provide a method for preparing an adsorbent precursor for lithium ion recovery, comprising the following steps: S1: mixing a titanium source and a lithium source in a dispersion medium to obtain a raw material slurry; S2: spray drying the raw material slurry, and crushing the dried powder to obtain a raw material powder; S3: placing the raw material powder in a chemical vapor deposition furnace, and introducing a gaseous carbon source at high temperature for reaction and carbon film deposition to obtain the adsorbent precursor for lithium ion recovery.
[0006] As a preference, the lithium source and the titanium source are mixed in a molar ratio of lithium to titanium of 0.8 to 2.0.
[0007] As another preference, the lithium source and the titanium source are mixed in a molar ratio of lithium to titanium of 2.
[0008] As another preference, the gaseous carbon source is one of methane, ethylene, acetylene, vaporized ethanol, vaporized acetone, and vaporized toluene.
[0009] As another preference, the gaseous carbon source is acetylene.
[0010] As another preference, the reaction temperature in step S3 is 500-900° C., and the reaction time is 3-10 h.
[0011] As another preferred embodiment, in the step S3, an inert gas is also introduced into the vapor deposition furnace.
[0012] More preferably, in the step S1, wet grinding is performed so that the titanium source and the lithium source are uniformly mixed in the dispersion medium.
[0013] Provided is an adsorbent precursor for lithium ion recovery, which is prepared by any of the above-mentioned preparation methods.
[0014] An adsorbent for lithium ion recovery is obtained by activating the adsorbent precursor for lithium ion recovery with acid.
[0015] Compared with the prior art, the beneficial effects of this application are:
[0016] (1) The adsorbent precursor for lithium ion recovery of the present application uses chemical vapor deposition to modify a dense carbon film in the adsorbent, which is beneficial to improving the service life and stability of the adsorbent;
[0017] (2) The adsorbent precursor for lithium ion recovery of the present application has a simple preparation method and easy-to-obtain raw materials, which is suitable for large-scale mass production. The adsorbent is suitable for lithium extraction and lithium recovery in salt lake brine, lithium precipitation mother liquor, lithium-containing waste liquid, etc., and has a wide range of applications. DETAILED DESCRIPTION
[0018] Below, the present application is further described in conjunction with specific implementation methods. It should be noted that, under the premise of no conflict, the various embodiments or technical features described below can be arbitrarily combined to form new embodiments.
[0019] The terms "including" and "having" and any variations thereof in the specification and claims of this application are intended to cover non-exclusive inclusions. For example, a process, method, system, product or apparatus comprising a series of steps or units is not necessarily limited to those steps or units explicitly listed, but may include other steps or units not explicitly listed or inherent to these processes, methods, products or apparatuses.
[0020] The present application provides an adsorbent precursor for lithium ion recovery, which is prepared using the following steps:
[0021] S1: mixing a titanium source and a lithium source in a dispersion medium to obtain a raw material slurry;
[0022] S2: spray drying the raw material slurry, and crushing the dried powder to obtain raw material powder;
[0023] S3: The raw material powder is placed in a chemical vapor deposition furnace, and a gaseous carbon source is introduced at high temperature for synthesis and carbon film deposition to obtain the adsorbent precursor for lithium ion recovery of the present application.
[0024] In some embodiments, the lithium source and the titanium source are mixed in a molar ratio of lithium to titanium of 0.8 to 2.0.
[0025] In a more preferred embodiment, the lithium source and the titanium source are mixed in a molar ratio of lithium to titanium of 2, so that the adsorbent has a better adsorption capacity.
[0026] The lithium source can be lithium carbonate, lithium hydroxide or a mixture of the two; the titanium source is titanium dioxide.
[0027] In some embodiments, the dispersion medium includes a dispersion solution and a dispersant, which is used to better and more evenly mix the titanium source and the lithium source. The dispersion solution can be water, ethanol, isopropanol, etc., and the dispersant can be polyethylene glycol, polypropylene pyrrolidone or glucose, etc.
[0028] In step S3, a titanium source and a lithium source are reacted in a high temperature environment of a chemical vapor deposition furnace to synthesize lithium metatitanate. Simultaneously, a gaseous carbon source is introduced into the chemical vapor deposition furnace to deposit a dense carbon film on the synthesized lithium metatitanate.
[0029] In the adsorbent precursor for lithium ion recovery of the present application, by depositing a dense carbon film on the adsorbent during the preparation process, the chemical interface reaction of Ti can be reduced, and its adsorption capacity for lithium ions can be improved. It also has better stability and longer service life and can be applied in more systems.
[0030] In some embodiments, the gaseous carbon source can be methane, ethylene, acetylene, vaporized ethanol, vaporized acetone, vaporized toluene, etc. The purity of the gaseous carbon source must be above 98%.
[0031] In a more preferred embodiment, the gaseous carbon source is acetylene, which can make the adsorbent have a better adsorption capacity.
[0032] In some embodiments, in step S3, the chemical vapor deposition furnace is set to 500-900° C., and the reaction time is 3-10 hours.
[0033] In some embodiments, an inert gas is introduced into the chemical vapor deposition furnace to exhaust the air in the furnace, serve as a carrier of the gaseous carbon source, and control the pressure in the furnace.
[0034] In some embodiments, step S1 mixes the lithium source and the titanium source into a raw material slurry by grinding.
[0035] The raw materials of the preparation method of the present application are widely available, easy to obtain, low in price, simple in process flow, and easy to scale up for mass production.
[0036] The present application provides an adsorbent precursor for lithium ion recovery, which is prepared using the above method and has the advantages of strong stability, long service life, good economic practicality, etc.
[0037] The present application also provides an adsorbent, which is obtained by activating the above-mentioned adsorbent precursor with an acid solution. The adsorbent of the present application can be used in lithium extraction from salt lakes, lithium extraction from lithium precipitation mother liquor, or lithium recovery from lithium-containing waste liquid. It has wide application, stable properties, and long service life.
[0038] The adsorbent precursor prepared by the above preparation method is dispersed in a dilute acid solution with a pH value of less than or equal to 2, stirred and activated for a period of time, and the powder is separated and dried to obtain an adsorbent for lithium ion recovery.
[0039] Example 1
[0040] An adsorbent precursor for lithium ion recovery is prepared according to the following steps:
[0041] S1: 554.4 g lithium carbonate, 600.0 g titanium dioxide and 30.0 g polyvinyl pyrrolidone were dissolved in 4 L ultrapure water, and transferred to a ball mill for wet grinding and mixing. The grinding material was zirconium oxide balls with a diameter of 0.1 to 1 mm, the rotation speed was 800 rpm, and the grinding and mixing time was 3 h to obtain a raw material slurry;
[0042] S2: spray drying the raw material slurry, setting the inlet temperature to 220±40°C and the outlet temperature to 100±10°C, and then air flow pulverizing the dried powder to obtain raw material powder;
[0043] S3: The raw material powder is placed in a vapor phase chemical deposition furnace, nitrogen is introduced, and acetylene is used as a gaseous carbon source, and the reaction is carried out at 700° C. for 8 hours to obtain the adsorbent precursor for lithium ion recovery in the present application.
[0044] Activating the adsorbent precursor: Weigh 20 g of the adsorbent precursor, add 1 L of 0.05 mol / L dilute sulfuric acid solution, stir, control the pH value to 1.00, activate for 4 hours, separate and dry to obtain an adsorbent for lithium ion recovery.
[0045] Example 2
[0046] The amount of lithium carbonate added in step S1 was adjusted to 416.4 g, and the other preparation steps were kept consistent with those in Example 1.
[0047] Example 3
[0048] The amount of lithium carbonate added in step S1 was adjusted to 346.5 g, and the other preparation steps were consistent with those in Example 1.
[0049] Example 4
[0050] An adsorbent precursor for lithium ion recovery is prepared according to the following steps:
[0051] S1: 221.7 g lithium carbonate, 600.0 g titanium dioxide and 35.0 g polyvinyl pyrrolidone were dissolved in 2.5 L ultrapure water, and transferred to a ball mill for wet grinding and mixing. The grinding material was zirconium oxide balls with a diameter of 0.1 to 1 mm, the rotation speed was 800 rpm, and the grinding and mixing time was 2 h to obtain a raw material slurry;
[0052] S2: spray drying the raw material slurry, setting the inlet temperature to 220±40°C and the outlet temperature to 100±10°C, and then air flow pulverizing the dried powder to obtain raw material powder;
[0053] S3: The raw material powder is placed in a vapor phase chemical deposition furnace, argon gas is introduced, and vaporized ethanol is used as a gaseous carbon source, and the reaction is carried out at 700° C. for 8 hours to obtain the adsorbent precursor for lithium ion recovery in the present application.
[0054] The steps of activating the adsorbent precursor are consistent with those in Example 1.
[0055] Example 5
[0056] The reaction time of step S3 was adjusted to 6.5 h, and the other preparation steps were kept consistent with those in Example 4.
[0057] Example 6
[0058] The reaction temperature of step S3 was adjusted to 900° C., the reaction time was adjusted to 8 h, and the other preparation steps were consistent with those in Example 1.
[0059] Comparative Example 1
[0060] Lithium metatitanate is synthesized using lithium carbonate and titanium dioxide. The lithium metatitanate is placed in a chemical vapor deposition furnace, nitrogen is introduced, and acetylene is used as a gaseous carbon source. The reaction is carried out at 700°C for 8 hours to obtain a post-deposition form of an adsorbent precursor.
[0061] The steps of activating the adsorbent precursor are consistent with those in Example 1.
[0062] Performance Testing
[0063] Simulated brine was prepared according to the concentration of each ion in Table 1 below, 20 g of the adsorbent material for lithium ions prepared in Examples 1 to 6 and Comparative Example 1 were weighed, and added to 2 L of brine for adsorption for 2 h. The tail liquid after adsorption by the adsorbent was tested for lithium content.
[0064] Table 1 Contents of various ions in simulated brine element <![CDATA[Na + ]]> <![CDATA[K + ]]> <![CDATA[Li + ]]> <![CDATA[Mg 2+ ]]> <![CDATA[Ca 2+ ]]> B Content (mg / L) 16501.5 2513.0 312.2 523.0 48.3 230.2
[0065] The adsorbent was desorbed using sulfuric acid with a concentration of 0.1 mol / L. The adsorbent after adsorbing lithium ions was dispersed in 1 L of sulfuric acid. The desorption time was 4 h. After the desorption was completed, the adsorbent and sulfuric acid were separated to obtain a desorbed solution, and the contents of lithium and titanium in the desorbed solution were tested.
[0066] The adsorbents of the examples and comparative examples were respectively subjected to the above-mentioned adsorption-desorption process for 5 times to observe the attenuation of the adsorbent capacity.
[0067] The relevant calculation formulas involved are as follows:
[0068] Adsorption capacity = (c 卤水Li -c 尾液Li )×V 卤水 / m 吸附剂
[0069] Desorption capacity = c 解吸液Li ×V 解吸液 / m 吸附剂
[0070] Dissolution rate = c 解吸液Ti ×V 解吸液 / (m 吸附剂 ×0.522)×100%
[0071] c 卤水Li ----Li concentration in brine, g / L
[0072] c 尾液Li ----Li concentration in adsorption tail liquid, g / L
[0073] V 卤水 ----Brine volume, L
[0074] m 吸附剂 ----Mass of adsorbent, g
[0075] c 解吸液Li ----Li concentration of desorption solution, g / L
[0076] V 解吸液 ----Desorption liquid volume, L
[0077] c 解吸液Ti ----Ti concentration of desorption liquid, g / L
[0078] The adsorption test results and average dissolution rate calculation results of each embodiment and comparative example 1 are recorded in the following Table 2.
[0079] Table 2 Performance test results of Examples 1 to 6 and Comparative Example 1
[0080] By analyzing the performance test results of Examples 1 to 6 and Comparative Example 1, it is found that the dissolution rate of an adsorbent for lithium ion recovery of the present application is significantly reduced after the surface is modified with a dense carbon layer, and the capacity of the adsorbent decays slowly in a sulfuric acid environment, indicating that the dense carbon film on the surface of the adsorbent enhances the adsorbent's tolerance to sulfuric acid and reduces the titanium dissolution loss of the adsorbent during the desorption process.
[0081] Analysis of the performance test results of Examples 1 to 3 shows that the lithium-titanium ratio in the synthetic raw materials affects both the adsorption capacity and the dissolution rate of the adsorbent. When the lithium-titanium ratio in Example 1 is 2, a better adsorption capacity of the adsorbent can be obtained.
[0082] Analysis of the performance test results of Example 4 and Example 5 shows that by extending the reaction time in step S3, the dissolution rate of the adsorbent is slightly reduced, and the stability of the adsorbent in the sulfuric acid system is slightly enhanced.
[0083] Analysis of the performance test results of Example 1 and Example 6 shows that increasing the reaction temperature of step S3 slightly reduces the dissolution rate of the adsorbent and decreases the adsorption capacity.
[0084] The adsorbent for lithium ion recovery prepared in the present application can maintain a good adsorption capacity after 5 rounds of recycling in a sulfuric acid system, has less dissolution loss, significantly enhanced stability, and significantly improved service life.
[0085] The above describes the basic principles, main features and advantages of the present application. Those skilled in the art should understand that the present application is not limited by the above embodiments, and the above embodiments and the specification only describe the principles of the present application. The present application may have various changes and improvements without departing from the spirit and scope of the present application, and these changes and improvements fall within the scope of the present application for which protection is sought. The scope of protection claimed by the present application is defined by the attached claims and their equivalents.
Claims
1. A method for preparing an adsorbent precursor for lithium ion recovery, It is characterized in that The steps include: S1: mixing a titanium source and a lithium source in a dispersion medium to obtain a raw material slurry; S2: spray drying the raw material slurry and crushing the dried powder to obtain raw material powder; S3: The raw material powder is placed in a chemical vapor deposition furnace, and a gaseous carbon source is introduced at high temperature to carry out reaction and carbon film deposition, so as to obtain the adsorbent precursor for lithium ion recovery.
2. The method for preparing an adsorbent precursor for lithium ion recovery according to claim 1, It is characterized in that The lithium source and the titanium source are mixed in a molar ratio of lithium to titanium of 0.8 to 2.
0.
3. The method for preparing an adsorbent precursor for lithium ion recovery according to claim 2, It is characterized in that The lithium source and the titanium source are mixed in a molar ratio of lithium to titanium of 2.
4. The method for preparing an adsorbent precursor for lithium ion recovery according to claim 1, It is characterized in that The gaseous carbon source is one of methane, ethylene, acetylene, vaporized ethanol, vaporized acetone, and vaporized toluene.
5. The method for preparing an adsorbent precursor for lithium ion recovery according to claim 4, It is characterized in that The gaseous carbon source is acetylene.
6. The method for preparing an adsorbent precursor for lithium ion recovery according to claim 1, It is characterized in that The reaction temperature in step S3 is 500-900° C., and the reaction time is 3-10 hours.
7. The method for preparing an adsorbent precursor for lithium ion recovery according to claim 4, It is characterized in that In the step S3, an inert gas is also introduced into the vapor deposition furnace.
8. The method for preparing an adsorbent precursor for lithium ion recovery according to claim 1, It is characterized in that In the step S1, the titanium source and the lithium source are uniformly mixed in the dispersion medium by wet grinding.
9. An adsorbent precursor for lithium ion recovery, It is characterized in that The method is prepared according to any one of claims 1 to 7.
10. An adsorbent for lithium ion recovery, It is characterized in that The adsorbent precursor for lithium ion recovery according to claim 9 is obtained by acid activation.
Citation Information
Patent Citations
Preparation method of coated and doped lithium manganate composite positive electrode material by vapor deposition
CN103794758A
Lithium titanate / carbon composite material and method for preparing material
CN104638255A
Lithium iron phosphate / carbon composite material for power battery, and preparation method and application of lithium iron phosphate / carbon composite material
CN106532013A
Lithium titanate silicon-based composite negative electrode material and preparation method thereof
CN111900352A
Preparation method of carbon-based lithium adsorption electrode for liquid lithium resource extraction