Preparation method of wastewater treatment agent and wastewater treatment method
By loading konjac glucomangan microspheres with magnesium oxide, zinc oxide and titanium dioxide, combined with pyrrole polymer and iminodisuccinic acid, a wastewater treatment agent was prepared, which solved the problem of dyes and heavy metals in printing and dyeing wastewater. It achieves efficient catalytic degradation and adsorption effects, protects the environment and saves water resources.
Patent Information
- Application Number
- CN202411046700.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-11-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The prior art is difficult to effectively treat dyes and heavy metal ions in printing and dyeing wastewater, resulting in environmental pollution and waste of water resources.
Using konjac glucomannan as the matrix, microspheres were prepared by emulsifying cross-linking method, and magnesium oxide, zinc oxide and titanium dioxide were supported on it to form catalyst microsheets, and then pyrrole and 3-chloropyrrole polymer were deposited to combine with sub-sub- Aminodisuccinic acid, wastewater treatment agent with catalytic degradation and adsorption properties were prepared.
This treatment agent can effectively degrade dyes in printing and dyeing wastewater under both light and ultraviolet conditions, and improves photocatalytic efficiency by expanding the spectrum absorption range. It also has excellent heavy metal ion adsorption performance, which significantly improves the treatment effect of wastewater.
Smart Images

Figure BDA0004973679730000091 
Figure BDA0004973679730000101
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of wastewater treatment, in particular to a preparation method of a wastewater treatment agent and a wastewater treatment method. Background Art
[0002] Printing and dyeing wastewater refers to wastewater discharged from printing and dyeing, wool dyeing and finishing, and silk factories that mainly process cotton, linen, chemical fibers and their blended products, and silk. The amount and quality of printing and dyeing wastewater vary depending on the type of fiber and the processing technology. Among them, the amount of wastewater from printing and dyeing factories is relatively large. Each ton of textiles consumed in printing and dyeing processing consumes 100 to 200 tons of water, most of which is discharged as wastewater. Printing and dyeing wastewater contains pollutants such as dyes, heavy metals, slurries, auxiliaries, and fiber impurities. It has the characteristics of large water volume, high content of organic pollutants, high alkalinity, and large changes in water quality. It is one of the difficult-to-treat industrial wastewaters. Based on the above problems, it is necessary to propose a preparation of a wastewater treatment agent. The wastewater treatment agent prepared by this method can well decompose the dyes in printing and dyeing wastewater, adsorb heavy metal ions in printing and dyeing wastewater, and achieve efficient and harmless treatment of printing and dyeing wastewater, which is of great significance to protecting the environment, saving water resources, and sustainable development. Summary of the invention
[0003] The object of the present invention is to provide a method for preparing a wastewater treatment agent and a wastewater treatment method to solve the problems existing in the prior art.
[0004] In order to solve the above technical problems, the present invention provides the following technical solutions:
[0005] The invention discloses a method for preparing a wastewater treatment agent. The method comprises the following steps: preparing konjac glucomannan into an emulsion, using epichlorohydrin as a crosslinking agent, and preparing konjac glucomannan microspheres by an emulsification and crosslinking method; loading a layer of magnesium oxide and zinc oxide on the konjac glucomannan microspheres, and then loading a layer of titanium dioxide, and removing the konjac glucomannan microspheres by high-temperature carbonization, and then crushing and ball milling to prepare catalyst micron sheets; polymerizing and depositing pyrrole and 3-chloropyrrole on the catalyst micron sheets to prepare polypyrrole catalyst micron sheets; and reacting the polypyrrole catalyst micron sheets with iminodisuccinic acid to prepare the wastewater treatment agent.
[0006] As an optimization, the preparation method of the wastewater treatment agent includes the following preparation steps:
[0007] (1) Konjac glucomannan and 3-5% acetic acid aqueous solution are mixed uniformly in a mass ratio of 1:(26-30) to prepare a dispersed phase; under the stirring conditions of 10-30° C. and 300-500 r / min, 0.6-0.8 times the mass of the dispersed phase is uniformly added dropwise to the continuous phase within 30 minutes, and then 0.6-0.8 times the mass of the dispersed phase is added with epichlorohydrin, the temperature is raised to 70-80° C., the stirring reaction is continued for 4-5 hours, centrifugation is performed, washing with anhydrous ethanol for 3-5 times, and drying at 50-60° C. under vacuum conditions for 7-8 hours to obtain konjac glucomannan microspheres;
[0008] (2) Konjac glucomannan microspheres, Mg 2+ / Zn 2+ The sol and deionized water are mixed uniformly in a mass ratio of 1: (3-4): (50-60), stirred at 55-65°C and 300-500r / min for 10-12h, centrifuged, placed in a muffle furnace, and calcined at 350-360°C for 5-6h under vacuum conditions to obtain MgO-ZnO catalytic microspheres; the MgO-ZnO catalytic microspheres and tetrabutyl titanate sol are mixed uniformly in a mass ratio of 1: (40-50), heated at 10-30°C and 300 ~500r / min stirring for 4~5h, centrifugal separation, placing in a muffle furnace, calcining at 490~510℃ for 2~3h under vacuum conditions, immersing in 50~60% ethanol aqueous solution, ultrasonically vibrating for 1~2h, centrifugal separation, and drying at 70~80℃ for 6~8h under vacuum conditions to obtain hollow catalytic microspheres; placing the hollow catalytic microspheres in a wall breaking machine for crushing, and then placing in a ball mill for 10~12h, passing through a mesh sieve to obtain catalyst micron sheets;
[0009] (3) The catalyst micron sheet, anhydrous ferric chloride and tetrahydrofuran were mixed uniformly in a mass ratio of 1:(0.04-0.06):(4-6), and ultrasonically dispersed for 1-2 hours to prepare a mixed solution; under a nitrogen atmosphere, at 0-2°C, 300-500 r / min stirring conditions, 1-1.2 times the mass of the mixed solution of pyrrole solution was uniformly added dropwise to the mixed solution within 25 minutes, and the stirring reaction was continued for 20-24 hours, and the mixture was allowed to stand at 10-30°C for 3-5 hours, filtered, and washed with anhydrous ethanol and deionized water for 3 times each. ~5 times, and dried at 60-70°C for 8-10 hours under vacuum conditions to obtain polypyrrole catalyst micron sheets; the polypyrrole catalyst micron sheets, iminodisuccinic acid, triethylamine, and N,N-dimethylformamide are mixed evenly in a mass ratio of 1:(2-3):(0.03-0.05):(8-10), stirred at 50-60°C and 300-500r / min for reaction for 3-4 hours, filtered, washed with deionized water for 3-5 times, and dried at 50-60°C for 8-10 hours under vacuum conditions to obtain a wastewater treatment agent.
[0010] As an optimization, the model of the konjac glucomannan in step (1) is KJ-30.
[0011] As an optimization, the continuous phase in step (1) is prepared by uniformly mixing Span 80, sorbitan monooleate polyoxyethylene ether, and petroleum ether in a mass ratio of 1:1:(40-50).
[0012] As an optimization, the Mg in step (2) 2+ / Zn 2+ The sol is prepared by mixing zinc acetate, magnesium chloride, monoethanolamine and ethylene glycol methyl ether in a mass ratio of 1:(4-5):(1.4-1.6):(38-42), stirring at 55-65°C and 300-500 r / min for 2-3 hours, and standing for aging for 40-48 hours to obtain Mg 2+ / Zn 2+ Sol.
[0013] As an optimization, the tetrabutyl titanate sol in step (2) is prepared by uniformly mixing tetrabutyl titanate, triethanolamine, deionized water and anhydrous ethanol in a mass ratio of 1:(0.4-0.6):(0.1-0.2):(4-6), stirring at 75-85°C and 300-500 r / min for 2-3 hours, and standing and aging for 40-48 hours to obtain the tetrabutyl titanate sol.
[0014] As an optimization, the mesh size of the sieve in step (2) is 1800 to 2000 meshes.
[0015] As an optimization, the pyrrole solution in step (3) is prepared by mixing pyrrole, 3-chloropyrrole and tetrahydrofuran in a mass ratio of 1:(0.2-0.3):(4-6) to prepare the pyrrole solution.
[0016] Compared with the prior art, the beneficial effects achieved by the present invention are:
[0017] When preparing the wastewater treatment agent, the invention prepares konjac glucomannan into an emulsion, uses epichlorohydrin as a crosslinking agent, and adopts an emulsification crosslinking method to prepare konjac glucomannan microspheres; loads a layer of magnesium oxide and zinc oxide on the konjac glucomannan microspheres, and then loads a layer of titanium dioxide; carbonizes the konjac glucomannan microspheres at high temperature, and then crushes and ball-mills to prepare catalyst micron sheets; polymerizes and deposits pyrrole and 3-chloropyrrole on the catalyst micron sheets to prepare polypyrrole catalyst micron sheets; and reacts the polypyrrole catalyst micron sheets with iminodisuccinic acid to prepare the wastewater treatment agent.
[0018] Firstly, konjac glucomannan is prepared into an emulsion, and konjac glucomannan microspheres are prepared by an emulsification and cross-linking method with epichlorohydrin as a cross-linking agent; a layer of magnesium oxide and zinc oxide is loaded on the konjac glucomannan microspheres, and then a layer of titanium dioxide is loaded, and the template konjac glucomannan microspheres are carbonized and cleaned to remove the template konjac glucomannan microspheres to prepare hollow catalytic microspheres; the inner surface of the hollow catalytic microspheres is non-photosensitive catalyst magnesium oxide and zinc oxide, and the outer surface of the hollow catalytic microspheres is photosensitive catalyst titanium dioxide; the hollow catalytic microspheres are crushed, ball-milled, and sieved to prepare catalyst micron sheets; one side of the catalyst micron sheet is non-photosensitive catalyst magnesium oxide and zinc oxide, and the other side is photosensitive catalyst titanium dioxide, magnesium oxide and zinc oxide can catalytically degrade dyes in printing and dyeing wastewater under the condition of no light, and titanium dioxide can catalytically degrade dyes in printing and dyeing wastewater under the catalysis of ultraviolet light, so as to give the wastewater treatment agent excellent catalytic degradation performance of dyes.
[0019] Secondly, pyrrole and 3-chloropyrrole are oxidatively polymerized and deposited on catalyst microsheets to obtain polypyrrole catalyst microsheets, and chlorine atoms are introduced into the polypyrrole catalyst microsheets. Currently, most inorganic semiconductor materials can only absorb part of the ultraviolet light and cannot make full use of visible light. Polypyrrole is a conductive polymer with a large number of π-conjugated structures. It shows strong absorption in the range of ultraviolet light to visible light, which can expand the spectral absorption range and expand the photocatalytic response range of the wastewater treatment agent from the ultraviolet light region to the ultraviolet-visible light region, thereby improving the utilization efficiency of the wastewater treatment agent for sunlight, and further Improve the catalytic degradation performance of wastewater treatment agents on dyes in printing and dyeing wastewater; react the chlorine atoms on the polypyrrole catalyst micron sheets with the secondary amines on the iminodisuccinic acid to obtain the wastewater treatment agent, graft the iminodisuccinic acid onto the surface of the polypyrrole catalyst micron sheets, introduce a large number of carboxylic acid groups on the surface of the polypyrrole catalyst micron sheets, the carboxylic acid groups can chelate the heavy metal ions in the printing and dyeing wastewater, giving the wastewater treatment agent excellent heavy metal ion adsorption performance, the nitrogen atoms on the pyrrole ring can provide lone pairs of electrons to form complexes with metal ions, and further improve the wastewater treatment agent's ability to adsorb heavy metal ions. DETAILED DESCRIPTION
[0020] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0021] Example 1
[0022] A method for preparing a wastewater treatment agent, the method comprising the following steps:
[0023] (1) Konjac glucomannan and 3% acetic acid aqueous solution are mixed in a mass ratio of 1:26 to prepare a dispersed phase; Span 80, sorbitan monooleate polyoxyethylene ether, and petroleum ether are mixed in a mass ratio of 1:1:40 to prepare a continuous phase; under the stirring conditions of 10°C and 300 r / min, 0.6 times the mass of the dispersed phase is uniformly added to the continuous phase within 30 minutes, and then 0.6 times the mass of the dispersed phase is added. Epichlorohydrin is heated to 70°C, and the reaction is continued with stirring for 5 hours, centrifuged, washed with anhydrous ethanol for 3 times, and dried at 50°C under vacuum conditions for 8 hours to obtain konjac glucomannan microspheres;
[0024] (2) Zinc acetate, magnesium chloride, monoethanolamine, and ethylene glycol methyl ether were mixed uniformly in a mass ratio of 1:4:1.4:38, stirred at 55°C and 300 r / min for 3 h, and allowed to stand for 40 h to obtain Mg 2+ / Zn 2+ Sol; Konjac glucomannan microspheres, Mg 2+ / Zn 2+ The sol and deionized water were mixed uniformly in a mass ratio of 1:3:50, stirred at 55°C and 300 r / min for 12 h, centrifuged, placed in a muffle furnace, and calcined at 350°C for 6 h under vacuum conditions to obtain MgO-ZnO catalytic microspheres; tetrabutyl titanate, triethanolamine, deionized water, and anhydrous ethanol were mixed uniformly in a mass ratio of 1:0.4:0.1:4, stirred at 75°C and 300 r / min for 3 h, and aged for 40 h to obtain tetrabutyl titanate sol; MgO-ZnO catalytic The microspheres and tetrabutyl titanate sol are uniformly mixed in a mass ratio of 1:40, stirred at 10°C and 300r / min for 5h, centrifuged, placed in a muffle furnace, calcined at 490°C for 3h under vacuum conditions, immersed in a 50% ethanol aqueous solution, ultrasonically vibrated for 1h, centrifuged, and dried at 70°C for 8h under vacuum conditions to obtain hollow catalytic microspheres; the hollow catalytic microspheres are placed in a wall breaking machine for crushing, and then placed in a ball mill for 10h, and passed through a 1800-mesh sieve to obtain catalyst micron sheets;
[0025] (3) The catalyst micron sheet, anhydrous ferric chloride and tetrahydrofuran were mixed at a mass ratio of 1:0.04:4, and ultrasonically dispersed for 1 hour to prepare a mixed solution; pyrrole, 3-chloropyrrole and tetrahydrofuran were mixed at a mass ratio of 1:0.2:4 to prepare a pyrrole solution, and under a nitrogen atmosphere, at 0°C and 300 r / min stirring conditions, 1 times the mass of the mixed solution of the pyrrole solution was uniformly added dropwise to the mixed solution within 25 minutes, and the stirring reaction was continued for 24 hours. The mixture was allowed to stand at 0°C for 5 h, filtered, washed with anhydrous ethanol and deionized water for 3 times each, and dried at 60°C for 10 h under vacuum conditions to obtain polypyrrole catalyst micron sheets; polypyrrole catalyst micron sheets, iminodisuccinic acid, triethylamine, and N,N-dimethylformamide were evenly mixed in a mass ratio of 1:2:0.03:8, stirred at 50°C and 300 r / min for 4 h, filtered, washed with deionized water for 3 times, and dried at 50°C for 10 h under vacuum conditions to obtain a wastewater treatment agent.
[0026] Example 2
[0027] A method for preparing a wastewater treatment agent, the method comprising the following steps:
[0028] (1) Konjac glucomannan and 4% acetic acid aqueous solution are mixed in a mass ratio of 1:28 to prepare a dispersed phase; Span 80, sorbitan monooleate polyoxyethylene ether, and petroleum ether are mixed in a mass ratio of 1:1:45 to prepare a continuous phase; under stirring conditions of 20° C. and 400 r / min, 0.7 times the mass of the dispersed phase is uniformly added to the continuous phase within 30 minutes, and then 0.7 times the mass of the dispersed phase epichlorohydrin is added, the temperature is raised to 75° C., the reaction is continued with stirring for 4.5 hours, centrifuged, washed with anhydrous ethanol 4 times, and dried at 55° C. under vacuum conditions for 7.5 hours to obtain konjac glucomannan microspheres;
[0029] (2) Zinc acetate, magnesium chloride, monoethanolamine, and ethylene glycol methyl ether were mixed uniformly in a mass ratio of 1:4.5:1.5:40, stirred at 60°C and 400 r / min for 2.5 h, and allowed to stand for 44 h to obtain Mg 2+ / Zn 2+ Sol; Konjac glucomannan microspheres, Mg 2+ / Zn 2+Sol and deionized water were mixed uniformly in a mass ratio of 1:3.5:55, stirred at 60°C and 400r / min for 11h, centrifuged, placed in a muffle furnace, and calcined at 355°C for 5.5h under vacuum conditions to obtain MgO-ZnO catalytic microspheres; tetrabutyl titanate, triethanolamine, deionized water, and anhydrous ethanol were mixed uniformly in a mass ratio of 1:0.5:0.15:5, stirred at 80°C and 400r / min for 2.5h, and aged for 44h to obtain tetrabutyl titanate sol; MgO-ZnO catalyst The catalytic microspheres and tetrabutyl titanate sol are uniformly mixed in a mass ratio of 1:45, stirred at 20°C and 400r / min for 4.5h, centrifuged, placed in a muffle furnace, calcined at 500°C for 2.5h under vacuum conditions, immersed in an ethanol aqueous solution with a mass fraction of 55%, ultrasonically vibrated for 1.5h, centrifuged, and dried at 75°C for 7h under vacuum conditions to obtain hollow catalytic microspheres; the hollow catalytic microspheres are placed in a wall breaking machine for crushing, and then placed in a ball mill for 11h, and passed through a 1900-mesh sieve to obtain catalyst micron sheets;
[0030] (3) The catalyst micron flakes, anhydrous ferric chloride, and tetrahydrofuran were mixed uniformly at a mass ratio of 1:0.05:5, and ultrasonically dispersed for 1.5 hours to prepare a mixed solution; pyrrole, 3-chloropyrrole, and tetrahydrofuran were mixed uniformly at a mass ratio of 1:0.25:5 to prepare a pyrrole solution, and under a nitrogen atmosphere, at 1°C and 400 r / min stirring conditions, 1.1 times the mass of the mixed solution of the pyrrole solution was uniformly added dropwise to the mixed solution within 25 minutes, and the stirring reaction was continued for 22 hours. The mixture was allowed to stand at 20 °C for 4 h, filtered, washed with anhydrous ethanol and deionized water for 4 times each, and dried at 65 °C under vacuum for 9 h to obtain polypyrrole catalyst micron sheets; polypyrrole catalyst micron sheets, iminodisuccinic acid, triethylamine, and N,N-dimethylformamide were uniformly mixed in a mass ratio of 1:2.5:0.04:9, stirred at 55 °C and 400 r / min for 3.5 h, filtered, washed with deionized water for 4 times, and dried at 55 °C under vacuum for 9 h to obtain a wastewater treatment agent.
[0031] Example 3
[0032] A method for preparing a wastewater treatment agent, the method comprising the following steps:
[0033] (1) Konjac glucomannan and 5% acetic acid aqueous solution are mixed in a mass ratio of 1:30 to prepare a dispersed phase; Span 80, sorbitan monooleate polyoxyethylene ether, and petroleum ether are mixed in a mass ratio of 1:1:50 to prepare a continuous phase; under stirring conditions of 30° C. and 500 r / min, 0.8 times the mass of the dispersed phase is uniformly added dropwise to the continuous phase within 30 minutes, and then 0.8 times the mass of the dispersed phase is added. Epichlorohydrin is heated to 80° C. and stirred for 4 hours, centrifuged, washed with anhydrous ethanol for 5 times, and dried at 60° C. under vacuum conditions for 7 hours to obtain konjac glucomannan microspheres;
[0034] (2) Zinc acetate, magnesium chloride, monoethanolamine, and ethylene glycol methyl ether were mixed uniformly in a mass ratio of 1:5:1.6:42, stirred at 65°C and 500 r / min for 2 h, and allowed to stand for 48 h to obtain Mg 2+ / Zn 2+ Sol; Konjac glucomannan microspheres, Mg 2+ / Zn 2+ The sol and deionized water were mixed uniformly in a mass ratio of 1:4:60, stirred at 65°C and 500r / min for 10h, centrifuged, placed in a muffle furnace, and calcined at 360°C for 5h under vacuum conditions to obtain MgO-ZnO catalytic microspheres; tetrabutyl titanate, triethanolamine, deionized water, and anhydrous ethanol were mixed uniformly in a mass ratio of 1:0.6:0.2:6, stirred at 85°C and 500r / min for 2h, and aged for 48h to obtain tetrabutyl titanate sol; MgO-ZnO catalytic The microspheres and tetrabutyl titanate sol are uniformly mixed in a mass ratio of 1:50, stirred at 30°C and 500r / min for 4h, centrifuged, placed in a muffle furnace, calcined at 510°C for 2h under vacuum conditions, immersed in a 60% ethanol aqueous solution, ultrasonically vibrated for 2h, centrifuged, and dried at 80°C for 6h under vacuum conditions to obtain hollow catalytic microspheres; the hollow catalytic microspheres are placed in a wall breaking machine for crushing, and then placed in a ball mill for 12h, and passed through a 2000-mesh sieve to obtain catalyst micron sheets;
[0035] (3) The catalyst micron flakes, anhydrous ferric chloride, and tetrahydrofuran were mixed uniformly at a mass ratio of 1:0.06:6, and ultrasonically dispersed for 2 hours to prepare a mixed solution; pyrrole, 3-chloropyrrole, and tetrahydrofuran were mixed uniformly at a mass ratio of 1:0.3:6 to prepare a pyrrole solution, and under a nitrogen atmosphere, at 2°C and 500 r / min stirring conditions, 1.2 times the mass of the mixed solution of the pyrrole solution was uniformly added dropwise to the mixed solution within 25 minutes, and the stirring reaction was continued for 20 hours. The mixture was allowed to stand at 30°C for 3 h, filtered, washed with anhydrous ethanol and deionized water for 5 times each, and dried at 70°C for 8 h under vacuum conditions to obtain polypyrrole catalyst micron sheets; polypyrrole catalyst micron sheets, iminodisuccinic acid, triethylamine, and N,N-dimethylformamide were evenly mixed in a mass ratio of 1:3:0.05:10, stirred at 60°C and 500 r / min for 3 h, filtered, washed with deionized water for 5 times, and dried at 60°C for 8 h under vacuum conditions to obtain a wastewater treatment agent.
[0036] Comparative Example 1
[0037] The difference between the preparation method of the wastewater treatment agent of Comparative Example 1 and Example 2 is that step (2) is different. Step (2) is modified as follows: zinc acetate, magnesium chloride, monoethanolamine, and ethylene glycol methyl ether are mixed uniformly in a mass ratio of 1:4.5:1.5:40, stirred at 60°C and 400r / min for 2.5h, and allowed to stand for aging for 44h to obtain Mg 2+ / Zn 2+ Sol; Konjac glucomannan microspheres, Mg 2+ / Zn 2+ The sol and deionized water were mixed uniformly in a mass ratio of 1:3.5:55, stirred at 60°C and 400r / min for 11h, centrifuged, placed in a muffle furnace, calcined at 355°C for 5.5h under vacuum conditions, immersed in an ethanol aqueous solution with a mass fraction of 55%, ultrasonically vibrated for 1.5h, centrifuged, and dried at 75°C for 7h under vacuum conditions to obtain hollow catalytic microspheres; the hollow catalytic microspheres were placed in a wall breaking machine for crushing, and then placed in a ball mill for 11h, and passed through a 1900 mesh sieve to obtain catalyst micron sheets. The remaining steps are the same as in Example 2.
[0038] Comparative Example 2
[0039] The difference between the preparation method of the wastewater treatment agent of Comparative Example 2 and Example 2 lies in the difference in step (2). Step (2) is modified as follows: tetrabutyl titanate, triethanolamine, deionized water, and anhydrous ethanol are mixed uniformly in a mass ratio of 1:0.5:0.15:5, stirred at 80°C and 400 r / min for 2.5 h, and allowed to stand for aging for 44 h to obtain tetrabutyl titanate sol; konjac glucomannan microspheres and tetrabutyl titanate sol are mixed uniformly in a mass ratio of 1:45 , stirring at 20°C, 400r / min for 4.5h, centrifugation, placing in a muffle furnace, calcining at 500°C for 2.5h under vacuum conditions, immersing in a 55% ethanol aqueous solution, ultrasonically vibrating for 1.5h, centrifugation, and drying at 75°C for 7h under vacuum conditions to obtain hollow catalytic microspheres; the hollow catalytic microspheres are placed in a wall breaking machine for crushing, and then placed in a ball mill for 11h, and passed through a 1900 mesh sieve to obtain catalyst micron sheets. The remaining steps are the same as in Example 2.
[0040] Comparative Example 3
[0041] The preparation method of the wastewater treatment agent of Comparative Example 3 is different from that of Example 2 in that step (3) is not performed, and step (2) is modified as follows: zinc acetate, magnesium chloride, monoethanolamine, and ethylene glycol methyl ether are uniformly mixed in a mass ratio of 1:4.5:1.5:40, stirred at 60°C, 400 r / min for 2.5 h, and allowed to stand for aging for 44 h to obtain Mg 2+ / Zn 2+ Sol; Konjac glucomannan microspheres, Mg 2+ / Zn 2+ Sol and deionized water were mixed uniformly in a mass ratio of 1:3.5:55, stirred at 60°C and 400r / min for 11h, centrifuged, placed in a muffle furnace, and calcined at 355°C for 5.5h under vacuum conditions to obtain MgO-ZnO catalytic microspheres; tetrabutyl titanate, triethanolamine, deionized water, and anhydrous ethanol were mixed uniformly in a mass ratio of 1:0.5:0.15:5, stirred at 80°C and 400r / min for 2.5h, and aged for 44h to obtain tetrabutyl titanate sol; MgO-ZnO catalyst The microspheres and tetrabutyl titanate sol are mixed uniformly in a mass ratio of 1:45, stirred at 20°C and 400r / min for 4.5h, centrifuged, placed in a muffle furnace, calcined at 500°C for 2.5h under vacuum conditions, immersed in an ethanol aqueous solution with a mass fraction of 55%, ultrasonically vibrated for 1.5h, centrifuged, and dried at 75°C for 7h under vacuum conditions to obtain hollow catalytic microspheres; the hollow catalytic microspheres are placed in a wall breaking machine for crushing, and then placed in a ball mill for 11h, and passed through a 1900 mesh sieve to obtain a wastewater treatment agent. The remaining steps are the same as in Example 2.
[0042] Comparative Example 4
[0043] The preparation method of the wastewater treatment agent of Comparative Example 4 is different from that of Example 2 only in step (3), and step (3) is modified as follows: the catalyst micron sheet, anhydrous ferric chloride, and tetrahydrofuran are mixed uniformly at a mass ratio of 1:0.05:5, and ultrasonically dispersed for 1.5 hours to prepare a mixed solution; pyrrole, 3-chloropyrrole, and tetrahydrofuran are mixed uniformly at a mass ratio of 1:0.25:5 to prepare a pyrrole solution, and under a nitrogen atmosphere, at 1°C, 400r / min stirring conditions, 1.1 times the mass of the mixed solution The pyrrole solution is uniformly added dropwise to the mixed solution within 25 minutes, and the stirring reaction is continued for 22 hours, and the mixture is allowed to stand at 20°C for 4 hours, filtered, washed with anhydrous ethanol and deionized water 4 times each, and dried at 65°C for 9 hours under vacuum conditions to prepare a wastewater treatment agent. The remaining steps are the same as those of Example 2.
[0044] Test Example 1
[0045] Testing of catalytic degradation performance of dyes
[0046] Test method:
[0047] Weigh 0.1 g of methyl orange solid and dissolve it in 500 ml of deionized water. Use a 1000 ml volumetric flask to make up to 5 mg / L of methyl orange mother solution. Take 0.5 ml, 1 ml, 2 ml, 3 ml, 4 ml, 5 ml and 10 ml of the mother solution and dilute them to 100 ml respectively. Use an ultraviolet spectrophotometer to measure the absorbance at 464 nm. Draw a linear regression equation with the solution concentration as the X-axis and the measured absorbance as the Y-axis.
[0048] Add 0.01g of wastewater treatment agent sample and 100ml of 400mg / L methyl orange solution into a conical flask, stir and shake at 25℃ and 200r / min for 3h under light-proof conditions; after the shaking, filter through a 0.22μm filter membrane, take 1ml of the sample and dilute it to 20ml, measure its absorbance, and use the absorbance data to calculate the dye removal rate under light-proof conditions.
[0049] Add 0.01g of wastewater treatment agent sample and 100ml of 400mg / L methyl orange solution to a conical flask, stir and shake for 3h at 200r / min at 25℃ under sunlight; after shaking, filter through a 0.22μm filter membrane, take 1ml of sample and dilute to 20ml, measure its absorbance, and calculate the dye removal rate under illumination using the absorbance data. The results are shown in Table 1.
[0050] Table 1
[0051]
[0052]
[0053] From the comparison of the experimental data of Examples 1 to 3 and Comparative Examples 1 to 4 in Table 1, it can be found that the wastewater treatment agent prepared by the present invention has good catalytic degradation performance for dyes in printing and dyeing wastewater.
[0054] By comparison, the dye removal rate under the light-proof condition of Examples 1 to 3 is greater than the dye removal rate under the light-proof condition of Comparative Example 2, indicating that konjac glucomannan is formulated into an emulsion, and epichlorohydrin is used as a cross-linking agent to prepare konjac glucomannan microspheres by emulsification and cross-linking; a layer of magnesium oxide and zinc oxide is loaded on the konjac glucomannan microspheres, and then a layer of titanium dioxide is loaded, and the template konjac glucomannan microspheres are carbonized and cleaned to remove the template to prepare hollow catalytic microspheres; the inner surface of the hollow catalytic microspheres is non-photosensitive catalyst magnesium oxide and zinc oxide, and the outer surface of the hollow catalytic microspheres is photosensitive catalyst titanium dioxide; the hollow catalytic microspheres are crushed, ball-milled, and sieved to prepare catalyst micron sheets; one side of the catalyst micron sheet is non-photosensitive catalyst magnesium oxide and zinc oxide, and the other side is photosensitive catalyst titanium dioxide, and magnesium oxide and zinc oxide can catalytically degrade dyes in printing and dyeing wastewater without light, giving the wastewater treatment agent excellent catalytic degradation of dye performance.
[0055] By comparison, the dye removal rate under the illumination conditions of Examples 1 to 3 is greater than the dye removal rate under the illumination conditions of Comparative Example 1, indicating that konjac glucomannan is formulated into an emulsion, and epichlorohydrin is used as a cross-linking agent to prepare konjac glucomannan microspheres by an emulsification cross-linking method; a layer of magnesium oxide and zinc oxide is loaded on the konjac glucomannan microspheres, and then a layer of titanium dioxide is loaded, and the template konjac glucomannan microspheres are carbonized and cleaned to remove the template to prepare hollow catalytic microspheres; the inner surface of the hollow catalytic microspheres is non-photosensitive catalyst magnesium oxide and zinc oxide, and the outer surface of the hollow catalytic microspheres is photosensitive catalyst titanium dioxide; the hollow catalytic microspheres are crushed, ball-milled, and sieved to prepare catalyst micron sheets; one side of the catalyst micron sheet is non-photosensitive catalyst magnesium oxide and zinc oxide, and the other side is photosensitive catalyst titanium dioxide, and titanium dioxide can catalytically degrade dyes in printing and dyeing wastewater under the catalysis of ultraviolet light, giving the wastewater treatment agent excellent catalytic degradation of dye performance.
[0056] By comparison, the dye removal rates under the illumination conditions of Examples 1 to 3 are greater than the dye removal rates under the illumination conditions of Comparative Example 3, indicating that pyrrole and 3-chloropyrrole are oxidatively polymerized and deposited on catalyst microsheets to prepare polypyrrole catalyst microsheets, and chlorine atoms are introduced into the polypyrrole catalyst microsheets; currently most inorganic semiconductor materials can only absorb part of the ultraviolet light and cannot make full use of visible light. Polypyrrole is a conductive polymer with a large number of π-conjugated structures, and exhibits strong absorption in the range from ultraviolet light to visible light, which can expand the spectral absorption range, and expand the photocatalytic response range of the wastewater treatment agent from the ultraviolet light region to the ultraviolet-visible light region, thereby improving the utilization efficiency of the wastewater treatment agent for sunlight, and further improving the catalytic degradation performance of the wastewater treatment agent for dyes in printing and dyeing wastewater.
[0057] Test Example 2
[0058] Test of heavy metal ion adsorption performance
[0059] Test method: Mix lead nitrate and deionized water at a mass ratio of 1:2000 to prepare a lead nitrate aqueous solution. Add 0.01g of wastewater treatment agent to 100ml of lead nitrate aqueous solution, stir and shake at 25℃, 200r / min for 3h; after shaking, use a pipette to draw 0.5mL of filtered lead nitrate aqueous solution, and then dilute to 5mL with 2% nitric acid aqueous solution. Use atomic absorption spectrometry to measure the remaining lead ion concentration in the lead nitrate aqueous solution and calculate the heavy metal adsorption rate; heavy metal adsorption rate = (heavy metal original concentration - heavy metal residual concentration) / heavy metal original concentration × 100%. The results are shown in Table 2.
[0060] Table 2
[0061] Heavy metal adsorption rate (%) Heavy metal adsorption rate (%) Example 1 96.67 Comparative Example 1 95.97 Example 2 97.06 Comparative Example 2 96.12 Example 3 96.58 Comparative Example 3 27.31 Comparative Example 4 65.58
[0062] From the comparison of the experimental data of Examples 1 to 3 and Comparative Examples 1 to 4 in Table 2, it can be found that the wastewater treatment agent prepared by the present invention has good performance in adsorbing heavy metal ions.
[0063] By comparison, the heavy metal adsorption rates of Examples 1 to 3 are greater than those of Comparative Examples 3 to 4, indicating that pyrrole and 3-chloropyrrole are oxidatively polymerized and deposited on catalyst microsheets to prepare polypyrrole catalyst microsheets, and chlorine atoms are introduced into the polypyrrole catalyst microsheets; the chlorine atoms on the polypyrrole catalyst microsheets are reacted with the secondary amines on iminodisuccinic acid to prepare the wastewater treatment agent, iminodisuccinic acid is grafted onto the surface of the polypyrrole catalyst microsheet, and a large number of carboxylic acid groups are introduced onto the surface of the polypyrrole catalyst microsheet. The carboxylic acid groups can chelate heavy metal ions in printing and dyeing wastewater, giving the wastewater treatment agent excellent heavy metal ion adsorption performance, and the nitrogen atoms on the pyrrole ring can provide lone pairs of electrons to form complexes with metal ions, further improving the performance of the wastewater treatment agent in adsorbing heavy metal ions.
[0064] The specific implementation methods described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific implementation method of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.
Claims
1. A method for preparing a wastewater treatment agent, characterized in that: The preparation method of the wastewater treatment agent comprises the following steps: loading titanium dioxide onto MgO-ZnO catalytic microspheres, removing konjac glucomannan microspheres through high temperature carbonization, and then crushing, ball milling, and sieving to obtain catalyst micron sheets; polymerizing and depositing pyrrole and 3-chloropyrrole on the catalyst micron sheets to obtain polypyrrole catalyst micron sheets; and reacting the polypyrrole catalyst micron sheets with iminodisuccinic acid to obtain the wastewater treatment agent; The MgO-ZnO catalytic microspheres are prepared by loading magnesium oxide and zinc oxide onto konjac glucomannan microspheres; The konjac glucomannan microspheres are prepared by preparing konjac glucomannan into an emulsion, using epichlorohydrin as a crosslinking agent, and using an emulsification crosslinking method.
2. The method for preparing a wastewater treatment agent according to claim 1, characterized in that: The preparation method of the wastewater treatment agent comprises the following preparation steps: (1) Konjac glucomannan and 3-5% acetic acid aqueous solution are mixed uniformly in a mass ratio of 1:(26-30) to prepare a dispersed phase; under the stirring conditions of 10-30° C. and 300-500 r / min, 0.6-0.8 times the mass of the dispersed phase is uniformly added dropwise to the continuous phase within 30 minutes, and then 0.6-0.8 times the mass of the dispersed phase is added with epichlorohydrin, the temperature is raised to 70-80° C., the stirring reaction is continued for 4-5 hours, centrifugation is performed, washing with anhydrous ethanol for 3-5 times, and drying at 50-60° C. under vacuum conditions for 7-8 hours to obtain konjac glucomannan microspheres; (2) Konjac glucomannan microspheres, Mg 2+ / Zn 2+ The sol and deionized water are mixed uniformly in a mass ratio of 1: (3-4): (50-60), stirred at 55-65°C and 300-500r / min for 10-12h, centrifuged, placed in a muffle furnace, and calcined at 350-360°C for 5-6h under vacuum conditions to obtain MgO-ZnO catalytic microspheres; the MgO-ZnO catalytic microspheres and tetrabutyl titanate sol are mixed uniformly in a mass ratio of 1: (40-50), heated at 10-30°C and 300 ~500r / min stirring for 4~5h, centrifugal separation, placing in a muffle furnace, calcining at 490~510℃ for 2~3h under vacuum conditions, immersing in 50~60% ethanol aqueous solution, ultrasonically vibrating for 1~2h, centrifugal separation, and drying at 70~80℃ for 6~8h under vacuum conditions to obtain hollow catalytic microspheres; placing the hollow catalytic microspheres in a wall breaking machine for crushing, and then placing in a ball mill for 10~12h, passing through a mesh sieve to obtain catalyst micron sheets; (3) The catalyst micron sheet, anhydrous ferric chloride and tetrahydrofuran were mixed uniformly in a mass ratio of 1:(0.04-0.06):(4-6), and ultrasonically dispersed for 1-2 hours to prepare a mixed solution; under a nitrogen atmosphere, at 0-2°C, 300-500 r / min stirring conditions, 1-1.2 times the mass of the mixed solution of pyrrole solution was uniformly added dropwise to the mixed solution within 25 minutes, and the stirring reaction was continued for 20-24 hours, and the mixture was allowed to stand at 10-30°C for 3-5 hours, filtered, and washed with anhydrous ethanol and deionized water for 3 times each. ~5 times, and dried at 60-70°C for 8-10 hours under vacuum conditions to obtain polypyrrole catalyst micron sheets; the polypyrrole catalyst micron sheets, iminodisuccinic acid, triethylamine, and N,N-dimethylformamide are mixed evenly in a mass ratio of 1:(2-3):(0.03-0.05):(8-10), stirred at 50-60°C and 300-500r / min for reaction for 3-4 hours, filtered, washed with deionized water for 3-5 times, and dried at 50-60°C for 8-10 hours under vacuum conditions to obtain a wastewater treatment agent.
3. The method for preparing a wastewater treatment agent according to claim 2, characterized in that: The model of the konjac glucomannan in step (1) is KJ-30.
4. The method for preparing a wastewater treatment agent according to claim 2, characterized in that: The continuous phase in step (1) is prepared by uniformly mixing Span 80, sorbitan monooleate polyoxyethylene ether and petroleum ether in a mass ratio of 1:1:(40-50).
5. The method for preparing a wastewater treatment agent according to claim 2, characterized in that: Step (2) Mg 2+ / Zn 2+ The sol is prepared by mixing zinc acetate, magnesium chloride, monoethanolamine and ethylene glycol methyl ether in a mass ratio of 1:(4-5):(1.4-1.6):(38-42), stirring at 55-65°C and 300-500 r / min for 2-3 hours, and standing for aging for 40-48 hours to obtain Mg 2+ / Zn 2+ Sol.
6. The method for preparing a wastewater treatment agent according to claim 2, characterized in that: The tetrabutyl titanate sol in step (2) is prepared by uniformly mixing tetrabutyl titanate, triethanolamine, deionized water and anhydrous ethanol in a mass ratio of 1:(0.4-0.6):(0.1-0.2):(4-6), stirring at 75-85°C and 300-500 r / min for 2-3 hours, and standing and aging for 40-48 hours to obtain the tetrabutyl titanate sol.
7. The method for preparing a wastewater treatment agent according to claim 2, characterized in that: The mesh size of the sieve in step (2) is 1800 to 2000 meshes.
8. The method for preparing a wastewater treatment agent according to claim 2, characterized in that: The pyrrole solution in step (3) is prepared by uniformly mixing pyrrole, 3-chloropyrrole and tetrahydrofuran in a mass ratio of 1:(0.2-0.3):(4-6) to prepare the pyrrole solution.
9. A method for treating wastewater, characterized in that: The wastewater treatment method comprises treating wastewater using a wastewater treatment agent prepared by the method for preparing a wastewater treatment agent as described in any one of claims 1 to 8.