Method for preparing ionic liquid loaded resin based on ultrasound and application of ionic liquid loaded resin

Through ultrasonic preparation and regeneration treatment, the problems of long synthesis time, high temperature and poor cycle stability of ionic liquid-loaded resins are solved, and more efficient resin preparation and regeneration are achieved, which significantly improves adsorption performance and cycle stability.

CN118904310AActive Publication Date: 2024-11-08WUHAN UNIV OF TECH
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202410988416.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-08
Estimated Expiration
2044-07-23

AI Technical Summary

Technical Problem

The existing ionic liquid-loaded resin synthesis methods have problems such as long synthesis time, high temperature and poor cycle stability, which leads to severe attenuation of adsorption amount and the adsorption amount of regenerated resin cannot reach the level of newly prepared resin.

Method used

The method of preparing ionic liquid-loaded resins by ultrasonication, by ultrasonic mixing of chloromethylated polystyrene resin, glycine and ultrapure water at 50-95°C, and soaking under low pressure to clean the resin, combined with magnetic stirring and Vacuum drying shortens the preparation time and improves the activity of the resin; during the regeneration process, the adsorption performance of the resin is restored by using ultrasonic cavitation effect and moisture curing, charge adjustment and water vapor annealing.

Benefits of technology

It significantly shortens the preparation time of ionic liquid-loaded resin, reduces the preparation temperature, improves the adsorption performance and cycle stability of the resin, restores the adsorption amount of the regenerated resin to or exceeds the initial value, and solves the attenuation of the adsorption amount and low regeneration efficiency. The problem.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118904310A_ABST
    Figure CN118904310A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of ionic liquid supported resin, in particular to a method for preparing ionic liquid supported resin based on ultrasound and application of the method, the preparation method comprises the following steps: S1, chloromethylated polystyrene resin, glycine and ultrapure water are subjected to ultrasonic mixing for 30-120 min at the temperature of 50-95 DEG C according to the solid-to-liquid ratio of 0.8-1.2 g: 4 g: 40 mL, magnetic stirring is started synchronously, and a mixed solution is obtained; and S2, filtering the mixed solution obtained in the step S1 at room temperature to obtain resin, flushing the resin for 3-5 times by using 10-30mL of absolute ethyl alcohol, and drying the flushed resin in a vacuum drying oven at 60-65 DEG C until the weight is constant to obtain the ionic liquid loaded resin. The ionic liquid loaded resin is applied to selective adsorption of phosphoric acid. Compared with a traditional flask and a constant-temperature magnetic stirring device, the preparation time can be remarkably shortened, the preparation temperature can be reduced, and the adsorption capacity of the prepared or regenerated ionic liquid loaded resin is far larger than that of resin prepared or regenerated through a conventional method.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of ionic liquid loaded resins, and in particular to a method for preparing ionic liquid loaded resins based on ultrasound and application thereof. Background Art

[0002] Ionic liquid loaded resin is synthesized by chemical grafting of ionic liquid and polymer. It is regarded as a new adsorption material with great potential due to its good cleanliness, high cycle stability and excellent selectivity. Its cleanliness is due to the fact that ionic liquid loaded resin has less impact on the environment compared with traditional liquid-liquid extraction, avoiding the volatilization of organic solvents and not causing turbidity and emulsification of the solution phase. Its selectivity is due to the fact that ionic liquid loaded resin with different functional groups can be prepared by different chemical agents and chemical grafting methods, so ionic liquid loaded resin with different selectivities can be designed.

[0003] Ionic liquid loaded resin is prepared by chemical grafting, and a stable chemical bond is formed between the ionic liquid and the resin, so the loss of ionic liquid during adsorption and desorption can be significantly reduced, which also ensures that the ionic liquid loaded resin has good cycle stability. Usually, the adsorption amount decreases by about 1% after each cycle, which is much lower than the traditional solvent impregnated resin. The existing ionic liquid loaded resin synthesis method is to use a three-necked flask and a constant temperature magnetic stirrer for synthesis, with a synthesis time of more than 8 hours and a synthesis temperature of more than 90°C. After a large number of cycles (generally more than 100 times), the adsorption amount of the ionic liquid loaded resin will decay to less than 80% of the initial amount. Regeneration requires the re-preparation of the ionic liquid loaded resin, and the adsorption amount of the regenerated resin cannot reach the level of the newly prepared ionic liquid loaded resin.

[0004] Therefore, the present invention determines to prepare ionic liquid loaded resin by ultrasound to solve the above problems. Summary of the invention

[0005] In order to solve the above problems, the present invention provides a method for preparing ionic liquid loaded resin based on ultrasound and application thereof.

[0006] A method for preparing an ionic liquid loaded resin based on ultrasound comprises the following steps:

[0007] S1. Ultrasonic mixing of chloromethylated polystyrene resin, glycine and ultrapure water at a solid-liquid ratio of 0.2-0.3 g:1 g:10 mL at 50-95° C. for 30-120 min, and simultaneously starting magnetic stirring to obtain a mixed solution;

[0008] Among them, the ultrasonic power is 100-500W, and the speed of magnetic stirring is 200-300r / min;

[0009] S2. Filter the mixed solution obtained in S1 at room temperature to obtain a resin, then rinse the resin 3 to 5 times with 10 to 30 mL of anhydrous ethanol, and dry the rinsed resin in a vacuum drying oven at 60 to 65° C. to a constant weight to obtain an ionic liquid-loaded resin.

[0010] Furthermore, the particle size of the chloromethylated polystyrene resin is 100-200 meshes, the crosslinking degree of divinylbenzene is 0.8-1.2%, and the chlorine content is 3.2-3.6 mmol / g.

[0011] Description: The particle size of chloromethylated polystyrene resin is conducive to improving the adsorption capacity and reactivity of the resin. The cross-linking degree of divinylbenzene determines the mechanical strength and chemical stability of chloromethylated polystyrene resin. A higher chlorine content may increase the hydrophilicity of the resin, but it may also increase its corrosiveness.

[0012] Furthermore, before performing S1, the chloromethylated polystyrene resin is pretreated, comprising the following steps:

[0013] The chloromethylated polystyrene resin is soaked in a 95% ethanol solution at a solid-liquid ratio of 1 g: 1.5-2.5 mL, filtered after soaking for 11-13 hours, and then the filtered chloromethylated polystyrene resin is rinsed with ultrapure water until no turbidity is produced, and then the rinsed chloromethylated polystyrene resin is dried in a vacuum drying oven at 60-65° C., and the pretreatment is completed.

[0014] Description: Ethanol can remove grease, dust and other contaminants on the surface of the resin, which helps to clean the resin and can affect the surface properties of the resin, making it more active and convenient for subsequent chemical reactions or processing.

[0015] Furthermore, the immersion is carried out in a container, and the air pressure in the container is set to 2.5-3.5 MPa during the first 1 / 4-1 / 3 period of immersion; the air pressure in the container is set to 8-10 MPa during the last 1 / 4-1 / 3 period of immersion; and the air pressure in the container is set to 0.5-1.5 MPa during the remaining period of immersion.

[0016] Description: Soaking the resin under low pressure can help remove bubbles on the surface of the resin, increase the contact area between the resin and the 95% ethanol solution, and promote the penetration of ethanol molecules into the resin, which helps to clean the resin surface and pores, remove impurities and residues, and create better conditions for subsequent treatment; further reducing the pressure can help to further clean the resin, promote the opening of the resin pore structure, and improve its permeability; finally, increasing the pressure can improve the penetration capacity of the 95% ethanol solution, making it easier for ethanol to enter the microporous structure of the resin. This helps to clean the resin more thoroughly and may promote the activation of functional groups inside the resin; in addition, high pressure can also cause changes in the microstructure inside the resin, such as the expansion of the pore size or the rearrangement of functional groups, thereby improving the overall activity of the resin.

[0017] The ionic liquid loaded resin prepared by any of the above methods is used to selectively adsorb phosphoric acid.

[0018] Furthermore, the ionic liquid loaded resin after selectively adsorbing phosphoric acid is regenerated.

[0019] Furthermore, the regeneration method is:

[0020] Under the conditions of 250-350W ultrasonic power and 70-80℃, the ionic liquid loaded resin after selectively adsorbing phosphate once or multiple times, glycine and ultrapure water are mixed in a solid-liquid ratio of 0.4-0.6g:1g:20mL, reacted for 1.5-2.5h and filtered to obtain the resin to be regenerated, rinsed the resin to be regenerated 3-5 times with 10-30mL anhydrous ethanol, and dried the rinsed resin in a vacuum drying oven at 60-65℃ to constant weight to obtain the regenerated ionic liquid loaded resin.

[0021] Description: The cavitation effect of ultrasound is used to expand the active interface sites inside the resin, promote the combination of organic chemicals with more active sites in the ionic liquid-loaded resin with severe adsorption performance loss, and thus achieve efficient regeneration of the ionic liquid-loaded resin.

[0022] Furthermore, the ionic liquid loaded resin after selectively adsorbing phosphoric acid is first activated, and the activation treatment method is:

[0023] First, the ionic liquid loaded resin after selective adsorption of phosphoric acid is moisture cured at a temperature of 18-22° C., an air humidity of 65-75%, and a time of 25-35 hours. After moisture curing, a charge regulator accounting for 0.05-0.08% of the resin mass is added and mixed for 10-15 minutes, and then the air humidity is adjusted to 80-85%, and moisture curing is continued for 15-20 hours. After moisture curing, a charge regulator accounting for 0.01-0.02% of the resin mass is added for 10-15 minutes, and then steam annealing is performed to complete the activation treatment.

[0024] Description: Moisture curing helps soften the resin, reduce internal stress, improve the flexibility and ductility of the resin, and can also help restore its ion exchange capacity to prepare for subsequent charge adjustment; charge adjustment can remove impurity ions adsorbed by the resin and reintroduce the required ions, so that the ion exchange sites of the resin can be effectively utilized and its selectivity and efficiency can be improved; water vapor annealing can help further remove residual solvents and impurities in the resin, while promoting structural reorganization inside the resin and improving its thermal stability and mechanical strength. Water vapor annealing also helps eliminate micropores and defects in the resin and improve its overall performance.

[0025] Furthermore, the charge regulator comprises, by mass percentage, 10-15% of diethanolamine, 1-3% of sulfonyloxyketone and the balance of vinyl acetate.

[0026] Description: Diethanolamine has good wettability and emulsification properties, and can effectively adjust the charge distribution of the resin. It can help improve the wettability of the resin and make the resin easier to react with other substances, thereby improving the efficiency of charge adjustment; sulfonyloxy ketone can participate in the chemical reaction of the resin as a catalyst, which can help accelerate the formation of ion exchange sites in the resin and improve the ion exchange capacity of the resin; vinyl acetate can undergo cross-linking reaction with the resin to improve the mechanical strength and heat resistance of the resin.

[0027] Furthermore, the relative humidity of the water vapor annealing is 55-65%, the temperature is 180-200° C., and the time is 10-30 minutes.

[0028] Note: If the relative humidity is too low, the resin may not be able to fully absorb moisture, resulting in poor annealing effect, affecting the activation degree and final performance of the resin. If the relative humidity is too high, the resin may absorb excessive water, resulting in structural changes or even damage, which is also not conducive to the activation of the resin. If the temperature is too low, it may not be enough to activate the chemical bonds in the resin, so that the performance of the resin cannot be effectively restored, while if the temperature is too high, it may cause the resin to decompose or deteriorate, destroy its structure and reduce its performance. If the time is too short, the resin may not be fully activated, while if the time is too long, the resin may be over-annealed, resulting in performance degradation.

[0029] Compared with the existing preparation method of ionic liquid loaded resin, the beneficial effects of the present invention are:

[0030] (1) The prior art synthesizes ionic liquid-loaded resins by water bath heating and magnetic stirring, but has the problems of long synthesis time and high reaction temperature, and the synthesis effect is unstable. The adsorption performance of the product varies significantly with the change of process parameters, which seriously hinders the industrial application of the process. Therefore, based on the relatively low energy consumption of ultrasound and the ability to produce strong mechanical vibration effects, cavitation effects, thermal effects, etc. at the solid-liquid interface, the present invention utilizes the cavitation effect of ultrasound to expand the active interface sites inside the resin, promotes the combination of organic chemical agents with more active sites in the ionic liquid-loaded resin with severely depleted adsorption performance, thereby achieving efficient regeneration of the ionic liquid-loaded resin. Compared with the traditional flask and constant temperature magnetic stirring device, the present invention can significantly shorten the preparation time and reduce the preparation temperature.

[0031] (2) The preparation method of the ionic liquid loaded resin of the present invention is to soak the resin in ethanol, first remove the grease, dust and other pollutants on the surface of the resin, which is helpful to clean the resin and can affect the surface properties of the resin, making it more active and convenient for subsequent chemical reactions. The resin is first soaked in a low-pressure environment, which can help remove bubbles on the surface of the resin and increase the contact area between the resin and the 95% ethanol solution by mass, thereby promoting the penetration of ethanol molecules into the resin, which is helpful to clean the resin surface and pores, remove impurities and residues, and create better conditions for subsequent treatment; further reducing the pressure is helpful to further clean the resin, and promote the opening of the resin pore structure to improve its permeability; finally, increasing the pressure can improve the penetration capacity of the 95% ethanol solution by mass, so that ethanol can more easily enter the microporous structure of the resin. This helps to clean the resin more thoroughly and may promote the activation of functional groups inside the resin; in addition, high pressure can also cause changes in the microstructure inside the resin, such as the expansion of the pore size or the rearrangement of functional groups, thereby improving the overall activity of the resin.

[0032] (3) When regenerating the ionic liquid loaded resin, the present invention first activates the ionic liquid loaded resin after selectively adsorbing phosphoric acid to improve the regeneration efficiency, wherein moisture curing helps soften the resin, reduce internal stress, improve the flexibility and ductility of the resin, and can also help restore its ion exchange capacity to prepare for subsequent charge adjustment; charge adjustment can remove impurity ions adsorbed by the resin and reintroduce the required ions, so that the ion exchange sites of the resin are effectively utilized, improving its selectivity and efficiency; water vapor annealing can help further remove residual solvents and impurities in the resin, while promoting structural reorganization inside the resin, improving its thermal stability and mechanical strength. Water vapor annealing also helps eliminate micropores and defects in the resin and improve its overall performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 This is a comparison chart of the results of the preparation method 1 of the present invention;

[0034] Figure 2 It is a comparison chart of the results of the exploration 2 of the regeneration method of the present invention;

[0035] Figure 3 It is a comparison chart of the results of the exploration 3 of the regeneration method of the present invention;

[0036] Figure 4 It is a schematic diagram of the device used in the preparation and regeneration method of the present invention. DETAILED DESCRIPTION

[0037] In order to further illustrate the method adopted by the present invention and the effect achieved, the technical solution of the present invention will be clearly and completely described in combination with experiments below.

[0038] Example 1: This example describes a method for preparing an ionic liquid loaded resin based on ultrasound, comprising the following steps:

[0039] The chloromethylated polystyrene resin is first pretreated, comprising the following steps:

[0040] The chloromethylated polystyrene resin is soaked in a 95% ethanol solution at a solid-liquid ratio of 1 g: 2 mL, filtered after soaking for 12 hours, and then the filtered chloromethylated polystyrene resin is rinsed with ultrapure water until no turbidity is generated, and then the rinsed chloromethylated polystyrene resin is dried in a vacuum drying oven at 62°C, and the pretreatment is completed;

[0041] S1. Ultrasonic mixing of chloromethylated polystyrene resin, glycine and ultrapure water at a solid-liquid ratio of 0.25 g:1 g:10 mL at 70° C. for 75 min, and simultaneously starting magnetic stirring to obtain a mixed solution; the particle size of the chloromethylated polystyrene resin is 140-160 mesh, the crosslinking degree of divinylbenzene is 1%, and the chlorine content is 3.4 mmol / g;

[0042] Among them, the ultrasonic power is 300W, and the speed of magnetic stirring is 250r / min;

[0043] S2. Filter the mixed solution obtained in S1 at room temperature 25° C. to obtain a resin, then rinse the resin four times with 20 mL of anhydrous ethanol, and dry the rinsed resin in a vacuum drying oven at 62° C. to obtain an ionic liquid-loaded resin.

[0044] Example 2: The ionic liquid loaded resin prepared by ultrasound in Example 1 was used for selective adsorption of phosphoric acid, that is, 4.5 mol / L phosphoric acid was adsorbed by the ionic liquid loaded resin, the liquid-solid ratio of phosphoric acid to the ionic liquid loaded resin was 20 mL:1 g, the oscillation frequency was 120 r / min, the time was 6 h, and the temperature was 25°C;

[0045] The ionic liquid loaded resin after selectively adsorbing phosphoric acid is regenerated, and the regeneration method is as follows:

[0046] Under the conditions of 300W ultrasonic power and 75°C, the ionic liquid loaded resin after selectively adsorbing phosphoric acid 100 times, glycine and ultrapure water were mixed at a solid-liquid ratio of 0.5g:1g:20mL, reacted for 2h and filtered to obtain the resin to be regenerated, rinsed the resin to be regenerated 4 times with 20mL of anhydrous ethanol, and dried the rinsed resin in a vacuum drying oven at 62°C to constant weight to obtain the regenerated ionic liquid loaded resin;

[0047] A device is provided for the above-mentioned preparation method and regeneration method, such as Figure 1 As shown, the device includes an ultrasonic generator 1, a magnetic stirrer 2, a double-layer glass reactor 3, an ultrasonic probe 4 and a constant temperature bath 5. The ultrasonic probe 4 extends into the double-layer glass reactor 3, and the ultrasonic probe 4 is electrically connected to the ultrasonic generator 1. The output end of the magnetic stirrer 2 is in contact with the bottom of the double-layer glass reactor 3. The side wall of the double-layer glass reactor 3 is provided with an interlayer for circulating water flow, and the constant temperature bath 5 is connected to the interlayer through a water pipe; the ultrasonic generator 1, the ultrasonic probe 4, the magnetic stirrer 2 and the constant temperature bath 5 are all existing equipment.

[0048] Example 3: This example is different from Example 1 in that, in the preparation method, the chloromethylated polystyrene resin is immersed in an ethanol solution with a mass fraction of 95% at a solid-liquid ratio of 1 g:1.5 mL, and filtered after soaking for 11 hours.

[0049] Example 4: This example is different from Example 1 in that, in the preparation method, the chloromethylated polystyrene resin is immersed in an ethanol solution with a mass fraction of 95% at a solid-liquid ratio of 1 g:2.5 mL, and filtered after immersion for 13 hours.

[0050] Example 5: This example is different from Example 1 in that, in the preparation method, the particle size of the chloromethylated polystyrene resin is 100-140 mesh, the crosslinking degree of divinylbenzene is 0.8%, and the chlorine content is 3.2 mmol / g.

[0051] Example 6: This example is different from Example 1 in that, in the preparation method, the particle size of the chloromethylated polystyrene resin is 160-200 mesh, the crosslinking degree of divinylbenzene is 1.2%, and the chlorine content is 3.6 mmol / g.

[0052] Example 7: This example is different from Example 1 in that, in the preparation method, the chloromethylated polystyrene resin, glycine and ultrapure water are ultrasonically mixed at 50° C. at a solid-liquid ratio of 0.2 g:1 g:10 mL.

[0053] Example 8: This example is different from Example 1 in that, in the preparation method, the chloromethylated polystyrene resin, glycine and ultrapure water are ultrasonically mixed at 95° C. at a solid-liquid ratio of 0.3 g:1 g:10 mL.

[0054] Example 9: This example is different from Example 1 in that, in the preparation method, the ultrasonic power is 100 W and the ultrasonic mixing is 30 min.

[0055] Example 10: This example is different from Example 1 in that, in the preparation method, the ultrasonic power is 500 W and the ultrasonic mixing is 120 min.

[0056] Example 11: This example is different from Example 1 in that, in the preparation method, the rotation speed of the magnetic stirring is 200 r / min.

[0057] Example 12: This example is different from Example 1 in that, in the preparation method, the rotation speed of the magnetic stirring is 300 r / min.

[0058] Example 13: This example is different from Example 1 in that, in the preparation method, the resin is rinsed three times with 10 mL of anhydrous ethanol and dried in a vacuum drying oven at 60°C.

[0059] Example 14: This example is different from Example 1 in that, in the preparation method, the resin is rinsed 5 times with 30 mL of anhydrous ethanol and dried in a vacuum drying oven at 65°C.

[0060] Example 15: This example is different from Example 1 in that, in the preparation method, the immersion is carried out in a container, and the air pressure in the container is set to 3MPa during the first 1 / 4 to 1 / 3 of the immersion period; the air pressure in the container is set to 9MPa during the last 1 / 4 to 1 / 3 of the immersion period, and the air pressure in the container is set to 1MPa during the remaining immersion period.

[0061] Example 16: The difference between this example and Example 15 is that during the first 1 / 4 to 1 / 3 of the soaking period, the air pressure in the container is set to 2.5 MPa; during the last 1 / 4 to 1 / 3 of the soaking period, the air pressure in the container is set to 8 MPa; during the remaining time period of the soaking, the air pressure in the container is set to 0.5 MPa.

[0062] Example 17: This example differs from Example 15 in that, during the first 1 / 4 to 1 / 3 of the soaking period, the air pressure in the container is set to 3.5 MPa; during the second 1 / 4 to 1 / 3 of the soaking period, the air pressure in the container is set to 10 MPa; and during the remaining soaking period, the air pressure in the container is set to 1.5 MPa.

[0063] Example 18: This example is different from Example 2 in that, in the regeneration method, the used ionic liquid loaded resin, glycine and ultrapure water are mixed under the conditions of 250 W ultrasonic power and 70°C.

[0064] Example 19: This example is different from Example 2 in that, in the regeneration method, the used ionic liquid loaded resin, glycine and ultrapure water are mixed under the conditions of 350 W ultrasonic power and 80°C.

[0065] Example 20: This example is different from Example 2 in that, in the regeneration method, the ionic liquid loaded resin after selectively adsorbing phosphate once, glycine and ultrapure water are mixed at a solid-liquid ratio of 0.4 g: 1 g: 20 mL, and filtered after reacting for 1.5 hours.

[0066] Example 21: This example is different from Example 2 in that, in the regeneration method, the ionic liquid loaded resin after selectively adsorbing phosphate 100 times, glycine and ultrapure water are mixed at a solid-liquid ratio of 0.6 g: 1 g: 20 mL, and filtered after reacting for 2.5 hours.

[0067] Example 22: This example is different from Example 2 in that, in the regeneration method, after the resin to be regenerated is rinsed three times with 10 mL of anhydrous ethanol, the rinsed resin is dried in a vacuum drying oven at 60° C. to constant weight.

[0068] Example 23: This example is different from Example 2 in that, in the regeneration method, after the resin to be regenerated is rinsed 5 times with 30 mL of anhydrous ethanol, the rinsed resin is dried in a vacuum drying oven at 65° C. to constant weight.

[0069] Example 24: This example is different from Example 2 in that, in the regeneration method, the ionic liquid loaded resin after selectively adsorbing phosphoric acid is first activated, and the activation method is:

[0070] First, the used ionic liquid loaded resin is moisture cured at a temperature of 20°C, an air humidity of 70%, and a time of 30 hours. After moisture curing, a charge regulator (K2483 charge regulator) accounting for 0.065% of the resin mass is added and mixed for 12 minutes. The air humidity is then adjusted to 82%, and moisture curing is continued for 18 hours. After moisture curing, a charge regulator accounting for 0.015% of the resin mass is added for 12 minutes, and then water vapor annealing is performed. The relative humidity of the water vapor annealing is 60%, the temperature is 190°C, and the time is 20 minutes. The activation treatment is completed.

[0071] Example 25: This example is different from Example 24 in that the moisture curing temperature is 18°C, the air humidity is 65%, and the time is 25 hours.

[0072] Example 26: This example differs from Example 24 in that the moisture curing temperature is 22°C, the air humidity is 75%, and the time is 35 hours.

[0073] Example 27: This example differs from Example 24 in that after moisture curing, a charge regulator accounting for 0.05% of the resin mass is added and mixed for 10 minutes.

[0074] Example 28: This example differs from Example 24 in that a charge regulator accounting for 0.08% of the resin mass is added after moisture curing and mixed for 15 minutes.

[0075] Example 29: This example differs from Example 24 in that the air humidity is adjusted to 80% and moisture curing is continued for 20 hours.

[0076] Example 30: This example differs from Example 24 in that the air humidity is adjusted to 85% and moisture curing is continued for 20 hours.

[0077] Example 31: This example differs from Example 24 in that a charge regulator accounting for 0.01% of the resin mass is added for 10 minutes after moisture curing.

[0078] Example 32: This example differs from Example 24 in that a charge regulator accounting for 0.02% of the resin mass is added for 15 minutes after moisture curing.

[0079] Example 33: This example is different from Example 24 in that the relative humidity of the water vapor annealing is 55%, the temperature is 180°C, and the time is 10 minutes.

[0080] Example 34: This example is different from Example 24 in that the relative humidity of the water vapor annealing is 65%, the temperature is 200°C, and the time is 30 minutes.

[0081] Example 35: This example is different from Example 1 in that the charge regulator comprises, by mass percentage, 12.5% ​​diethanolamine, 2% sulfonyloxy ketone and the remainder vinyl acetate.

[0082] Example 36: This example is different from Example 35 in that the charge regulator comprises, by mass percentage, 10% diethanolamine, 1% sulfonyloxy ketone and the remainder vinyl acetate.

[0083] Example 37: This example is different from Example 35 in that the charge regulator comprises, by mass percentage, 15% diethanolamine, 3% sulfonyloxy ketone and the remainder vinyl acetate.

[0084] Experimental Example: The description of this experimental example is based on the scheme described in Example 1, and is intended to illustrate the practical application effect of the present invention.

[0085] 1. The conventional method was used to prepare and regenerate the ionic liquid loaded resin, and the ionic liquid loaded resin prepared and regenerated by the present method was subjected to comparative adsorption under the same conditions, and the adsorption amount was calculated. The results are as follows:

[0086] Depend on Figure 1 As shown, the ionic liquid loaded resin prepared in Example 1 selectively adsorbed phosphoric acid once in the application mode of Example 2, and the adsorption amount reached 312 mg / g. Control Example 1 was conventionally synthesized, and the optimal conditions were temperature of 105°C and time of 8 h. The maximum adsorption amount of the prepared ionic liquid loaded resin was 260 mg / g. It can be seen that the ultrasonically prepared ionic liquid loaded resin significantly shortened the preparation time, reduced the preparation temperature, and effectively increased the adsorption performance of the resin.

[0087] Depend on Figure 2 As shown, after the ionic liquid loaded resin prepared in Example 1 selectively adsorbed phosphoric acid 100 times in the application mode of Example 2, the adsorption amount significantly decreased to 208 mg / g. Example 2 is the ionic liquid loaded resin regenerated by ultrasonic enhanced, and the adsorption amount of the regenerated ionic liquid loaded resin reached 285 mg / g, which is higher than the newly prepared ionic liquid loaded resin under normal conditions. However, when regenerated by conventional method, i.e., Control Example 2, it is necessary to react at 105°C for 8 hours, and the adsorption amount of the regenerated ionic liquid loaded resin is only 229 mg / g, which is only 88% of the new resin synthesized conventionally;

[0088] Therefore, ultrasonic regeneration of ionic liquid-loaded resin can significantly reduce the regeneration time and temperature, and can restore the adsorption amount of the resin after selective adsorption of phosphoric acid to the initial level, or even the adsorption amount is greater than the initial value.

[0089] 2. Investigate the influence of ultrasonic preparation parameters of ionic liquid loaded resin on its adsorption capacity.

[0090] Depend on Figure 1 Comparing Examples 1 to 14, it can be seen that if the soaking parameters are too small or too large, the parameters of the chloromethylated polystyrene resin are too small or too large, the mixing temperature is too small or too large, the ultrasonic parameters are too small or too large, the stirring speed is too small or too large, and the drying parameters are too small or too large, the adsorption amount of the ionic liquid loaded resin will be reduced. Therefore, the parameter effect of Example 1 is better;

[0091] By comparing Examples 1 and 15 to 17, it can be seen that linking the immersion time with the pressure during immersion can significantly increase the adsorption capacity of the ionic liquid-loaded resin, but too small or too large a pressure change will also reduce the improvement rate. Therefore, the parameter effect of Example 15 is relatively better.

[0092] 3. Investigate the influence of the parameters of ultrasonically regenerated ionic liquid loaded resin on its adsorption capacity.

[0093] Depend on Figure 2 By comparing Examples 2 and 18 to 23, it can be seen that too small or too large ultrasonic parameters, too small or too large mixing parameters, and too small or too large drying parameters will reduce the adsorption amount of the ionic liquid loaded resin, so the parameter effect of Example 2 is better.

[0094] 4. Investigate the influence of activation treatment parameters during ultrasonic regeneration on its adsorption capacity.

[0095] The difference between Control Example 3 and Example 24 is that the parameters of the two moisture curings remain unchanged;

[0096] The difference between Control Example 4 and Example 24 is that the amount of charge adjuster added twice remains unchanged;

[0097] The difference between Control Example 5 and Example 24 is that no steam annealing is performed.

[0098] Depend on Figure 3 As a result, it can be seen that Examples 24 to 34 significantly increase the adsorption amount of the ionic liquid-loaded resin compared to Example 2, while Control Examples 3 and 4 lack the regular changes before and after twice, and Control Example 5 lacks steam annealing, which reduces the improvement rate of Examples 24 to 34. Therefore, the regular changes and scheme effects of Examples 24 to 34 are better;

[0099] By comparing Examples 24 to 37, it can be seen that the parameters of the two moisture curings that are too small or too large, the amount of charge regulator added that is too small or too large, and the parameters of the water vapor annealing that are too small or too large will all reduce the adsorption amount of the ionic liquid-loaded resin. Therefore, in a comprehensive comparison, the parameter effect of Example 24 is relatively better; and Examples 35 to 37 provide charge regulators that are more suitable for this method, which further improve the adsorption amount of the ionic liquid-loaded resin compared to Example 24, but the proportion of vinyl acetate that is too small or too large will also reduce the improvement rate. Therefore, in a comprehensive comparison, the effect of Example 35 is relatively better.

Claims

1. A method for preparing ionic liquid loaded resin based on ultrasound, characterized in that: The following steps are involved: S1. Ultrasonic mixing of chloromethylated polystyrene resin, glycine and ultrapure water at a solid-liquid ratio of 0.2-0.3 g:1 g:10 mL at 50-95° C. for 30-120 min, and simultaneously starting magnetic stirring to obtain a mixed solution; Among them, the ultrasonic power is 100-500W, and the speed of magnetic stirring is 200-300r / min; S2. Filter the mixed solution obtained in S1 at room temperature to obtain a resin, then rinse the resin 3 to 5 times with 10 to 30 mL of anhydrous ethanol, and dry the rinsed resin in a vacuum drying oven at 60 to 65° C. to a constant weight to obtain an ionic liquid-loaded resin.

2. A method for preparing and regenerating ionic liquid-loaded resin based on ultrasound according to claim 1, characterized in that: The particle size of the chloromethylated polystyrene resin is 100-200 meshes, the crosslinking degree of divinylbenzene is 0.8-1.2%, and the chlorine content is 3.2-3.6 mmol / g.

3. A method for preparing and regenerating ionic liquid-loaded resin based on ultrasound according to claim 1, characterized in that: Before S1, the chloromethylated polystyrene resin is pretreated, including the following steps: The chloromethylated polystyrene resin is soaked in a 95% ethanol solution at a solid-liquid ratio of 1 g: 1.5-2.5 mL, filtered after soaking for 11-13 hours, and then the filtered chloromethylated polystyrene resin is rinsed with ultrapure water until no turbidity is produced, and then the rinsed chloromethylated polystyrene resin is dried in a vacuum drying oven at 60-65° C., and the pretreatment is completed.

4. The method for preparing ionic liquid loaded resin based on ultrasound according to claim 3, characterized in that: The immersion is carried out in a container. During the first 1 / 4 to 1 / 3 of the immersion period, the air pressure in the container is set to 2.5 to 3.5 MPa; during the last 1 / 4 to 1 / 3 of the immersion period, the air pressure in the container is set to 8 to 10 MPa; during the remaining time period of the immersion, the air pressure in the container is set to 0.5 to 1.5 MPa.

5. The use of the ionic liquid loaded resin prepared by the method according to any one of claims 1 to 4, characterized in that: It was applied to the selective adsorption of phosphoric acid.

6. The use according to claim 5, characterized in that The ionic liquid loaded resin after selectively adsorbing phosphoric acid is regenerated.

7. The use according to claim 6, characterized in that The regeneration method is: Under the conditions of 250-350W ultrasonic power and 70-80℃, the ionic liquid loaded resin after selective adsorption of phosphate, glycine and ultrapure water are mixed in a solid-liquid ratio of 0.4-0.6g:1g:20mL, reacted for 1.5-2.5h and filtered to obtain the resin to be regenerated, rinsed the resin to be regenerated 3-5 times with 10-30mL anhydrous ethanol, and dried the rinsed resin in a vacuum drying oven at 60-65℃ to constant weight to obtain the regenerated ionic liquid loaded resin.

8. The use according to claim 7, characterized in that The ionic liquid loaded resin after selectively adsorbing phosphoric acid is first activated, and the activation method is as follows: The ionic liquid loaded resin after selective adsorption of phosphoric acid is subjected to moisture curing, the moisture curing temperature is 18-22° C., the air humidity is 65-75%, and the time is 25-35 hours. After moisture curing, a charge regulator accounting for 0.05-0.08% of the resin mass is added and mixed for 10-15 minutes, and then the air humidity is adjusted to 80-85%, and moisture curing is continued for 15-20 hours. After moisture curing, a charge regulator accounting for 0.01-0.02% of the resin mass is added for 10-15 minutes, and then water vapor annealing is performed to complete the activation treatment.

9. A method for preparing and regenerating ionic liquid-loaded resin based on ultrasound according to claim 8, characterized in that: The charge regulator comprises, by mass percentage, 10-15% of diethanolamine, 1-3% of sulfonyloxy ketone and the balance of vinyl acetate.

10. The method for preparing and regenerating ionic liquid loaded resin based on ultrasound according to claim 8, characterized in that: The relative humidity of the water vapor annealing is 55-65%, the temperature is 180-200° C., and the time is 10-30 minutes.

Citation Information

Patent Citations

  • Method and device for rapidly producing ion liquid by promoting synthesis reaction with ultrasonic wave

    CN102372676A

  • Resin for separating and purifying tabersonine and applications thereof

    CN103554309A

  • Heavy metal ion adsorbent for grafting glycine to chloromethylated polystyrene, preparation method and application thereof

    CN104209102A

  • Amino acid ionic liquid and preparation method and application thereof

    CN110293119A

  • Phosphorus removal material as well as preparation method and application thereof

    CN111644154A