Modification method of titanium lithium ion sieve
By doping nitrogen, sulfur or selenium into titanium lithium ion sieve and preparing modified materials using different synthetic methods, the problem of the reduction of adsorbent adsorption rate and capacity after pickling is solved, and the adsorption efficiency of lithium ions is significantly improved.
Patent Information
- Application Number
- CN202410993922.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-24
AI Technical Summary
After pickling, the existing titanium lithium ion sieve adsorbents have lower H+ radius than Li+, resulting in the shrinkage of the crystal plane spacing and the formation of interlayer hydrogen bonds, which reduces the adsorption rate and actual adsorption capacity.
Modified titanium-based lithium ion sieve is prepared by doping non-metallic ions such as nitrogen, sulfur or selenium into lithium metatitanate by solid-phase synthesis, sol-gel synthesis or hydrothermal synthesis to reduce interlayer hydrogen bonds. Open up some layer spacing to increase adsorption rate and adsorption capacity.
It effectively improves the adsorption rate and adsorption capacity of lithium ions, avoids crystal surface shrinkage and interlayer hydrogen bonding after pickling, and significantly improves the extraction efficiency of lithium ions.
Smart Images

Figure CN118904311A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of lithium extraction from salt lakes, in particular to a method for modifying a titanium-based lithium ion sieve. Background Art
[0002] Lithium is the lightest metal element. With the increasing application of lithium in the field of new energy materials, the mining of lithium resources has attracted widespread attention. my country has abundant reserves of lithium resources, and the lithium reserves in salt lake brine are as high as 70%. Therefore, the comprehensive development and utilization of salt lake brine lithium resources has become the main development direction of the lithium industry. The ion sieve adsorption method is based on the ion exchange mechanism, with high lithium recovery rate, good selectivity and short process. It is very suitable for extracting lithium from low-concentration salt lake brine. The use of lithium ion sieve for adsorption and lithium extraction is a green method with application prospects. It is not only simple in process, but also has high adsorption capacity. It is one of the most industrially potential lithium extraction methods. The key to the ion adsorption method is to study an adsorbent with excellent performance. The adsorbent is required to have excellent selective adsorption for lithium so as to eliminate the interference of a large number of alkali metal and alkaline earth metal ions coexisting in the brine. The adsorption and elution performance of the adsorbent should be stable and suitable for large-scale operation.
[0003] At present, the lithium ion sieve adsorbent of metatitanate (H2TiO3) obtained by acid washing of lithium metatitanate (Li2TiO3) has attracted much attention due to its high theoretical capacity and stable material structure. However, existing studies have found that after Li2TiO3 is acid washed, due to H + Radius smaller than Li + , which will lead to the contraction of the interplanar spacing of Li2TiO3, and the hydrogen bonds formed by the interlayer OH also lead to the contraction of the interplanar spacing, further hindering the Li + Enter the interlayer, thereby reducing the adsorption rate and actual adsorption capacity. Summary of the invention
[0004] In view of the problem that the adsorption rate and the actual adsorption capacity of the current titanium-based lithium ion sieve adsorbent are reduced after acid washing, the present invention provides a modification method for the titanium-based lithium ion sieve.
[0005] The modification method of the titanium-based lithium ion sieve provided by the present invention uses a titanium source and a lithium source as basic raw materials, and dopes a modifier, wherein the modifier is selected from any one of sulfur powder, thiourea, urea, ammonium sulfide, hexamethylenetetramine, and selenium powder; and prepares a modified lithium metatitanate precursor by a solid phase synthesis method, a sol-gel synthesis method, or a hydrothermal synthesis method.
[0006] The titanium source is selected from any one of titanium dioxide, industrial metatitanic acid, tetrabutyl titanate, titanium tetrachloride, isopropyl titanate, titanium sulfate and titanium nitrate.
[0007] The lithium source is selected from any one of lithium hydroxide, lithium chloride, lithium carbonate, lithium acetate dihydrate, lithium oxalate, lithium fluoride, lithium bromide, lithium nitrate and lithium sulfate.
[0008] Different modification methods are adopted according to the different types of titanium sources used.
[0009] When the titanium source used is titanium dioxide, industrial metatitanic acid, or titanium dioxide obtained by hydrolyzing any one of titanium tetrachloride, titanium sulfate, and titanium nitrate, a modified lithium metatitanate precursor is prepared by a solid phase synthesis method.
[0010] The steps of the solid phase synthesis method are as follows:
[0011] The titanium source, lithium source and modifier are mixed evenly, and calcined at 600-900° C. for 4-12 hours to obtain a modified lithium metatitanate precursor; the calcination atmosphere is air, argon, or nitrogen.
[0012] Alternatively, the titanium source and the modifier are mixed evenly, calcined at a constant temperature of 300-600°C for 2-10 hours, and then the calcined product is mixed evenly with the lithium source, and calcined at a constant temperature of 600-900°C for 4-12 hours to obtain a modified lithium titanate precursor; the calcination atmosphere is air, argon, or nitrogen, and the heating rate is 3-10°C / min.
[0013] When the titanium source used is tetrabutyl titanate or isopropyl titanate, the modified lithium metatitanate precursor is prepared by a sol-gel synthesis method.
[0014] The steps of the sol-gel synthesis method are as follows:
[0015] (1) adding tetrabutyl titanate or isopropyl titanate to ethanol to form solution A; dissolving the modifier in another portion of ethanol, and adding hydrochloric acid and deionized water to form solution B; dropping solution B into solution A and stirring at high speed for 12-48 hours, and standing at room temperature for 12-48 hours to obtain a gel; drying the gel at 60-100° C. for 6-24 hours to obtain a powder;
[0016] (2) Mixing the powder with a lithium source, calcining at 600-900° C. for 4-12 hours to obtain a modified lithium titanate precursor; the calcination atmosphere is air, argon, or nitrogen; the heating rate is 3-10° C. / min.
[0017] The step (2) may also be: first calcining the powder at 300-600° C. for 2-5 h, then mixing with a lithium source, and calcining at 600-900° C. for 4-12 h to obtain a modified lithium metatitanate precursor.
[0018] When the titanium source used is any one of titanium tetrachloride, titanium sulfate and titanium nitrate, the modified lithium metatitanate precursor is prepared by a hydrothermal synthesis method.
[0019] The steps of the hydrothermal synthesis method are as follows:
[0020] (1) adding a titanium source, phenol or resorcinol to deionized water, stirring and dissolving, adding formaldehyde, continuing to stir and dissolve, then adding a modifier, continuing to stir and dissolve, adding the obtained solution to a reactor, hydrothermally reacting at 60-120° C. for 4-24 hours, collecting the generated solid after cooling, and washing and drying; the titanium source is any one of titanium tetrachloride, titanium sulfate, and titanium nitrate;
[0021] (2) The dried solid product is mixed evenly with a lithium source, and calcined at 600-900° C. for 4-12 hours to obtain a modified lithium metatitanate precursor; wherein the calcination atmosphere is air, argon, or nitrogen.
[0022] Compared with the prior art, the present invention is beneficial in that:
[0023] (1) The present invention replaces a small amount of O in lithium titanate by doping with non-metallic ions such as nitrogen (N), sulfur (S) or selenium (Se), which can reduce interlayer hydrogen bonds, open up some interlayer spacing, and improve adsorption rate and adsorption capacity. The inventor's research shows that the interface modification of introducing N active sites can effectively accelerate the adsorption of Li + Extraction, and the hydrogen bond energy formed by N is smaller than that formed by O, so N is selected as the doping source. S and Se, as elements of the same group as O, have similar properties and do not form hydrogen bonds, which can reduce the shrinkage of the crystal surface after pickling and promote Li + extraction process, thereby improving the adsorption rate and adsorption capacity.
[0024] (2) The modification method of the present invention avoids the problem that the existing Li2TiO3 is washed with H + Radius smaller than Li + The resulting H2TiO3 interplanar spacing contraction and the hydrogen bonds formed by the interlayer OH also cause the interplanar spacing contraction, hindering the Li + The technical defect is that it enters the interlayer, thereby reducing the adsorption rate and actual adsorption capacity.
[0025] Other advantages, objectives and features of the present invention will be embodied in part through the following description, and in part will be understood by those skilled in the art through study and practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 This is a diagram of the adsorption capacity of the Se-doped H2TiO3 ion sieve of Example 1 at different times.
[0027] Figure 2 This is a diagram of the adsorption capacity of the S-doped H2TiO3 ion sieve of Example 2 at different times.
[0028] Figure 3 This is a diagram of the adsorption capacity of the N-doped H2TiO3 ion sieve of Example 3 at different times.
[0029] Figure 4 This is a diagram of the adsorption capacity of the Se-doped H2TiO3 ion sieve of Example 4 at different times. DETAILED DESCRIPTION
[0030] The preferred embodiments of the present invention are described below in conjunction with the accompanying drawings. It should be understood that the preferred embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.
[0031] Example 1
[0032] A modification method for titanium-based lithium ion sieve:
[0033] 10g of Ti(SO4)2 was added to 250mL of deionized water, stirred for 20min, and then hydrothermally reacted at 85℃ for 12h. The solid obtained was collected, which was the titanium dioxide obtained by hydrolysis, washed several times, and then dried at 60℃ for 12h. 1.25g of dried titanium dioxide was mixed with 0.0988g of selenium powder, calcined at 300℃ for 6h in an argon environment, and then calcined at 500℃ for 2h at a heating rate of 5℃ / min to obtain Se-doped TiO2. 1g of Se-doped TiO2 was mixed with 0.934g of Li2CO3 and calcined at 700℃ for 4h in an argon environment at a heating rate of 5℃ / min. After cooling to room temperature, Se-doped Li2TiO3 powder was obtained. The obtained powder was eluted in 0.25mol / L HCl solution for 24h, washed several times, and dried at 60℃ for 24h to obtain Se-doped H2TiO3 ion sieve, which was recorded as HTO-Se-1.
[0034] According to the same method as above, the amount of selenium powder added was changed to 0.2964g and 0.4941g respectively. The Se-doped H2TiO3 ion sieves finally prepared were recorded as HTO-Se-2 and HTO-Se-3 respectively.
[0035] An ion sieve without selenium powder was prepared under the same conditions and was denoted as HTO.
[0036] The adsorption experiment was carried out by placing 0.3 g of ion sieve in 100 mL of 1000 mg / L Li solution. Samples were taken at different times. The concentration of the solution was tested by a flame photometer and the adsorption capacity was calculated. The change of adsorption capacity over time is shown in Figure 1It can be seen that compared with the ion sieve HTO not doped with selenium powder, the Se-doped H2TiO3 ion sieve of the present invention significantly improves the adsorption rate and adsorption capacity, and the adsorption capacity of HTO-Se-2 is the highest.
[0037] Example 2
[0038] A modification method for titanium-based lithium ion sieve:
[0039] 10ml of tetrabutyl titanate was added to 20ml of ethanol to form solution A; 2.2052g of thiourea was added to 20ml of ethanol, and then 1ml of 12M HCl and 3ml of deionized water were added to form solution B; solution B was dropped into solution A and stirred at high speed for 24h, and then kept at room temperature for 24h to obtain a gel. The gel was dried at 100℃ for 12h, and the dried powder was calcined at 500℃ in air for 2h at a heating rate of 5℃ / min to obtain S-doped TiO2. 1g of S-doped TiO2 and 0.934g of Li2CO3 were mixed evenly and calcined at 700℃ under argon for 4h at a heating rate of 5℃ / min. After cooling to room temperature, S-doped Li2TiO3 powder was obtained. The obtained S-doped Li2TiO3 was eluted in 0.25mol / L HCl solution for 24h, washed and dried to obtain S-doped H2TiO3 ion sieve, recorded as HTO-S-1.
[0040] According to the same preparation method as above, the amount of thiourea was changed to 4.4103g and 6.6155g to prepare S-doped H2TiO3 ion sieves, which were recorded as HTO-S-2 and HTO-S-3 respectively.
[0041] The undoped ion sieve was prepared under the same conditions and was denoted as HTO-sol.
[0042] 0.3 g of ion sieve was adsorbed in 100 mL of 1000 mg / L Li solution, and samples were taken at different times. The adsorption capacity was tested using a flame photometer. The change of adsorption capacity over time is shown in Figure 2 It can be seen that the doped ion sieve significantly improves the adsorption capacity and adsorption rate, and HTO-S-2 has the highest adsorption capacity.
[0043] Example 3
[0044] A modification method for titanium-based lithium ion sieve:
[0045] 5g titanium sulfate and 0.8g resorcinol were dissolved in 50mL deionized water and stirred for 20min, 2mL formaldehyde was added and stirred for 30min, then 0.6256g urea was added and stirred until dissolved, hydrothermally reacted at 85℃ for 12h, cooled naturally to room temperature, the obtained solid was collected, washed several times, and then dried at 60℃ for 12h to obtain a hydrothermal solid product. The hydrothermal fixed product was mixed evenly with Li2CO3, the mixing ratio was controlled to control the Li:Ti molar ratio to 2.02:1, and then calcined at 700℃ for 4h under argon, and then calcined at 500℃ for 2h in air, with a heating rate of 5℃ / min; after cooling to room temperature, N-doped Li2TiO3 powder was obtained.
[0046] The method for determining the mixing ratio of the hydrothermal fixed product and Li2CO3 is: quantitatively taking a portion of the hydrothermal solid product and calcining it at 500°C in air for 2 hours at a heating rate of 5°C / min to obtain the product titanium dioxide, and calculating the yield of titanium dioxide. The amount of the hydrothermal solid product mixed with Li2CO3 in the subsequent steps can be deduced based on the calculated yield.
[0047] The obtained N-doped Li2TiO3 was eluted in 0.25mol / L HCl solution for 24h, washed and dried to obtain N-doped H2TiO3 ion sieve, recorded as HTO-N-1.
[0048] According to the same preparation method as above, the amount of urea was changed to 1.2512g and 1.8768g respectively, and the N-doped H2TiO3 ion sieves were obtained, which were recorded as HTO-N-2 and HTO-N-3 respectively.
[0049] The undoped ion sieve was prepared under the same conditions and was denoted as HTO-h.
[0050] 0.3 g of ion sieve was adsorbed in 100 mL of 1000 mg / L Li solution, and samples were taken at different times. The adsorption capacity was tested using a flame photometer. The results are shown in Figure 3 The N-doped ion sieve significantly improved the adsorption capacity and adsorption rate. HTO-N-2 had the highest adsorption capacity. Although the equilibrium capacity of HTO-N-3 decreased, the adsorption rate was faster in the first 2 hours.
[0051] Example 4
[0052] A modification method for titanium-based lithium ion sieve:
[0053] 1g TiO2 was mixed with 0.934g Li2CO3, and then mixed with 0.0988g selenium powder, calcined at 700℃ for 4h under argon, with a heating rate of 5℃ / min, and cooled to room temperature to obtain Se-doped Li2TiO3 powder. The obtained powder was eluted in 0.25mol / LHCl solution for 24h, washed several times, and dried at 60℃ for 24h to obtain Se-doped H2TiO3 ion sieve, which was recorded as HTO-Se-1-step.
[0054] According to the same preparation method as above, the amount of selenium powder was changed to 0.2964g and 0.4941g respectively, and Se-doped H2TiO3 ion sieves were prepared, which were respectively recorded as HTO-Se-2-one step and HTO-Se-3-one step.
[0055] Undoped ion sieves were prepared under the same conditions, denoted as HTO-one step.
[0056] 0.3 g of ion sieve was adsorbed in 100 mL of 1000 mg / L Li solution, and samples were taken at different times. The solution concentration was tested using a flame photometer and the adsorption capacity was calculated. The results are shown in Figure 4 The figure shows that Se-doped H2TiO3 ion sieve significantly improves the adsorption rate and adsorption capacity. The adsorption capacity of HTO-Se-2-step is the highest, but the overall change is small.
[0057] The above description is only a preferred embodiment of the present invention and does not constitute any form of limitation to the present invention. Although the present invention has been disclosed as a preferred embodiment as above, it is not intended to limit the present invention. Any technician familiar with the profession can make some changes or modifications to equivalent embodiments of equivalent changes using the technical contents disclosed above without departing from the scope of the technical solution of the present invention. However, any simple modification, equivalent change and modification made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention still falls within the scope of the technical solution of the present invention.
Claims
1. A method for modifying a titanium-based lithium ion sieve, characterized in that: A titanium source and a lithium source are used as basic raw materials, and a modifier is doped to prepare a modified lithium metatitanate precursor through a solid phase synthesis method, a sol-gel synthesis method, or a hydrothermal synthesis method; the modifier is selected from any one of sulfur powder, thiourea, urea, ammonium sulfide, hexamethylenetetramine, and selenium powder.
2. The method for modifying a titanium-based lithium ion sieve according to claim 1, characterized in that: The titanium source is selected from any one of titanium dioxide, industrial metatitanic acid, tetrabutyl titanate, titanium tetrachloride, isopropyl titanate, titanium sulfate and titanium nitrate.
3. The method for modifying a titanium-based lithium ion sieve according to claim 2, characterized in that: The lithium source is selected from any one of lithium hydroxide, lithium chloride, lithium carbonate, lithium acetate dihydrate, lithium oxalate, lithium fluoride, lithium bromide, lithium nitrate and lithium sulfate.
4. The method for modifying a titanium-based lithium ion sieve according to claim 2, characterized in that: The steps of the solid phase synthesis method are as follows: The titanium source, lithium source and modifier are mixed evenly, and calcined at 600-900° C. for 4-12 hours to obtain a modified lithium metatitanate precursor; the calcination atmosphere is air, argon, or nitrogen.
5. The method for modifying the titanium-based lithium ion sieve according to claim 2, characterized in that: The steps of the solid phase synthesis method are as follows: The titanium source and the modifier are mixed evenly, and calcined at a constant temperature of 300-600°C for 2-10 hours. Then, the calcined product is mixed evenly with the lithium source, and calcined at a constant temperature of 600-900°C for 4-12 hours to obtain a modified lithium metatitanate precursor; the calcination atmosphere is air, argon, or nitrogen.
6. The method for modifying a titanium-based lithium ion sieve according to claim 4 or 5, characterized in that: The titanium source is titanium dioxide or industrial metatitanic acid or titanium dioxide obtained by hydrolyzing any one of titanium tetrachloride, titanium sulfate and titanium nitrate.
7. The method for modifying a titanium-based lithium ion sieve according to claim 3, characterized in that: The steps of the sol-gel synthesis method are as follows: (1) adding tetrabutyl titanate or isopropyl titanate to ethanol to form solution A; dissolving the modifier in another portion of ethanol, and adding hydrochloric acid and deionized water to form solution B; dropping solution B into solution A and stirring at high speed for 12-48 hours, and standing at room temperature for 12-48 hours to obtain a gel; drying the gel at 60-100° C. for 6-24 hours to obtain a powder; (2) Mixing the powder with a lithium source, and calcining at 600-900° C. for 4-12 hours to obtain a modified lithium metatitanate precursor; the calcination atmosphere is air, argon, or nitrogen.
8. The method for modifying a titanium-based lithium ion sieve according to claim 7, characterized in that: In the step (2), the powder is first calcined at 300-600° C. for 2-5 hours, then mixed with a lithium source, and calcined at 600-900° C. for 4-12 hours to obtain a modified lithium metatitanate precursor.
9. The method for modifying a titanium-based lithium ion sieve according to claim 2, characterized in that: The steps of the hydrothermal synthesis method are as follows: (1) adding a titanium source, phenol or resorcinol to deionized water, stirring and dissolving, adding formaldehyde, continuing to stir and dissolve, then adding a modifier, continuing to stir and dissolve, adding the obtained solution to a reactor, hydrothermally reacting at 60-120° C. for 4-24 hours, collecting the generated solid after cooling, and washing and drying; the titanium source is any one of titanium tetrachloride, titanium sulfate, and titanium nitrate; (2) The solid product is mixed evenly with a lithium source, and calcined at 600-900° C. for 4-12 hours to obtain a modified lithium metatitanate precursor; wherein the calcination atmosphere is air, argon, or nitrogen.
Citation Information
Patent Citations
Method for preparing lithium titanate ceramic powder by hydrothermal method
CN102746000A
Porous doped titanium-based lithium adsorbent and preparation method thereof
CN112705156A
Nitrogen-doped carbon-packaged lithium ion sieve membrane electrode for electrochemical extraction of dissolved lithium resources
CN113337735A
Preparation method of titanium-based lithium ion exchanger
CN114100560A
Preparation method of H2TiO3 lithium ion sieve with large specific surface area
CN117361613A
Cited By
High-temperature lithium extraction adsorbent as well as preparation method and application thereof
CN119549108A
A high-temperature lithium extraction adsorbent, its preparation method and application
CN119549108B
Cerium-nitrogen synergistically modified composite lithium ion sieve, and preparation method and application thereof
CN122745831A
Titanium-based lithium ion adsorbent and method for preparing the same
CN122850093A
A titanium-based lithium-ion adsorbent and its preparation method
CN122850093B