Palladium-based catalyst for low-concentration methane oxidation as well as preparation method and application of palladium-based catalyst
By loading palladium metal onto a rare earth oxide support to form a La-O-Ce solid solution, the problem of reduced activity of palladium-based catalysts in aqueous environments was solved, and high-efficiency catalytic performance for low-temperature methane oxidation was achieved.
Patent Information
- Application Number
- CN202411120696.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-08
AI Technical Summary
Existing palladium-based methane oxidation catalysts exhibit reduced catalytic activity in aqueous environments, making it difficult to effectively treat low-concentration methane emissions.
A rare earth oxide support preparation method was adopted, and a La-O-Ce solid solution was formed by loading trace amounts of palladium metal, which improved the low-temperature activity and water resistance of the catalyst.
Under aqueous conditions, the catalyst exhibits good catalytic oxidation activity and water resistance, making it suitable for the purification of natural gas and vehicle exhaust.
Smart Images

Figure CN118904334A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of catalysts, and in particular relates to a palladium-based catalyst for low-concentration methane oxidation catalyst and a preparation method and application thereof. Background Art
[0002] Methane is the world's second largest greenhouse gas, with a high warming potential and a greenhouse effect 25 times that of CO. In November 2023, the Ministry of Ecology and Environment and 11 other departments issued a notice on the issuance of the "Methane Emission Control Action Plan" to strengthen methane emission control. Most methane emissions are caused by human production activities, such as coal mining, oil and gas production, agriculture, landfills and biomass burning, among which coal mining and oil / gas industries contribute the most.
[0003] Catalytic combustion of methane is one of the effective ways to reduce low-concentration methane emissions. There are many types of catalysts currently used for complete methane oxidation, which can be divided into non-precious metal catalysts and precious metal catalysts. According to the reported catalysts, the low-temperature activity of precious metal catalysts is higher than that of non-palladium (Pd) based catalysts. The supports of methane oxidation catalysts can be roughly divided into three categories: metal oxides, molecular sieves, and silicon dioxide (SiO2). The support affects the activity of the catalyst by changing the physicochemical properties of the Pd species. Therefore, the selection of the support is crucial for the development of highly active Pd-based catalysts. Compared with molecular sieves and SiO2, most metal oxides (such as CeO2, Co3O4) are reducible, and these active supports are conducive to establishing strong metal support interactions (SMSI) with Pd species, thereby improving catalyst performance. Therefore, metal oxide-supported palladium catalysts are generally considered to be one of the most advanced methane oxidation catalysts.
[0004] The Chinese invention patent with publication number CN 102626640 A discloses a monolithic catalyst for low-temperature oxidation reaction of methane, wherein the catalyst is composed of a cordierite honeycomb ceramic carrier and a coating coated on the carrier. The mesh number of the cordierite honeycomb ceramic carrier is 300-600 mesh; the coating expression is Pd / Co x Cr y -M / Al2O3, the molar ratio of cobalt to chromium is between 0.001 and 100, M is a doping metal (one or more of cerium, zirconium, lanthanum, iron, nickel, and manganese), and Al2O3 is γ-Al2O3 with high thermal stability, which has good methane oxidation activity and thermal stability.
[0005] A Chinese invention patent with publication number CN 107983401 A discloses a ZSM-5 encapsulated single atomic layer Pd catalyst for methane oxidation. The molecular sieve encapsulation can improve the stability of the active components, and the catalyst has a long service life. It is applied to the catalytic combustion process of low-concentration coalbed methane and can improve the ability to activate methane.
[0006] The Chinese invention patent with publication number CN 117414864 A discloses a palladium-based molecular sieve catalyst and its preparation and application. The catalyst is prepared by mixing a template, a silicon source and a palladium source in water, heating and crystallizing, and then drying and calcining. The palladium-based molecular sieve catalyst has a simple preparation process and has excellent methane oxidation activity and hydrothermal stability.
[0007] However, the above catalyst performance tests were all conducted in anhydrous reaction atmospheres, which cannot fully reflect their practical application value. In practical applications, water vapor is usually present in methane exhaust gas, and one of the key issues to be overcome in methane catalytic oxidation is to eliminate the influence of water. Water and methane will produce competitive adsorption on active sites, which may change the reaction path of methane oxidation and lead to a significant decrease in methane oxidation activity.
[0008] Rare earth oxides have rich electronic structures and are highly efficient active carriers, which are widely used in the field of catalysis. At present, the preparation methods of rare earth oxides are generally divided into the following categories: (1) The corresponding rare earth carbonate salts (such as cerium carbonate, lanthanum carbonate, or lanthanum cerium carbonate mixture, etc.) are directly calcined to obtain rare earth oxides. The rare earth oxides prepared by this method have a small specific surface area and poor thermal stability, and are not suitable as catalyst carriers; (2) The corresponding rare earth solution (such as cerium chloride, lanthanum chloride, or lanthanum cerium chloride mixed solution, etc., or the corresponding nitric acid solution, etc.) is precipitated with an alkaline solution (such as sodium hydroxide, sodium carbonate, ammonia water, etc.) under certain conditions, and the corresponding rare earth oxides are obtained after filtering, washing, and calcining. The rare earth oxides prepared by this method also have a relatively small specific surface area and poor thermal stability.
[0009] How to improve the catalytic performance of palladium-based methane oxidation catalysts has always been a research hotspot, and the development of active carriers is one of the key factors affecting catalyst activity. Summary of the invention
[0010] The main purpose of the present invention is to overcome the deficiencies in the prior art and provide a palladium-based catalyst for low-concentration methane oxidation and its preparation method and application. The present invention provides a method for preparing a rare earth oxide carrier, and improves the low-temperature methane oxidation performance of the rare earth oxide carrier by loading a trace amount of palladium metal. The palladium-based catalyst for low-concentration methane oxidation provided by the present invention has a simple preparation process, good low-temperature oxidation activity and excellent water resistance stability, and has good application prospects in the field of catalytic purification of natural gas or automobile exhaust.
[0011] A first aspect of the present invention provides a palladium (Pd)-based catalyst for low-concentration methane oxidation. The Pd-based catalyst comprises a lanthanum-cerium oxide carrier and a Pd oxide supported on the surface of the carrier.
[0012] The lanthanum-cerium oxide is a La-O-Ce solid solution, which belongs to a defective fluorite structure and contains a large number of oxygen vacancies on the surface. Its specific surface area is 100-150m 2 g -1 .
[0013] In the Pd-based catalyst, the content of Pd is 0.5-1.5 wt %; preferably, the content of Pd is 1 wt %.
[0014] In the lanthanum-cerium oxide, La2O3 accounts for 5-50% of the weight of the lanthanum-cerium oxide; preferably, La2O3 accounts for 10-30% of the weight of the lanthanum-cerium oxide; more preferably, La2O3 accounts for 10-20% of the weight of the lanthanum-cerium oxide; most preferably, La2O3 accounts for 10% of the weight of the lanthanum-cerium oxide.
[0015] The second aspect of the present invention provides a method for preparing the above-mentioned palladium-based catalyst for low-concentration methane oxidation, comprising the following process: 1. Preparation process of rare earth mixed oxides S1. According to the weight percentage of theoretically generated oxides La2O3 and CeO2, weigh tetravalent Ce(NO3)4 solution and trivalent La(NO3)3 solution respectively, add them into the reactor and dilute with deionized water, so that the concentration of theoretical total oxide (REO) in the rare earth nitrate mixed solution is 30g-REO / L.
[0016] In step S1, the weight ratio of La2O3 / CeO2 oxides is 5~50% / 95~50%, preferably 10~40% / 90~60%, more preferably 10~20% / 90~80%; and most preferably 10% / 90%.
[0017] S2. Perform a hydrolysis reaction at a temperature of 100 to 120° C. for 20 to 24 hours. After the hydrolysis reaction is completed, cool the solution to room temperature, add ammonia water to adjust the pH of the solution to alkaline, and continue stirring for 10 to 60 minutes.
[0018] The mass fraction of the ammonia water is 25-28%; the pH value of the solution is adjusted to 7.0-8.0 by adding ammonia water.
[0019] S3, filtering, washing with deionized water and drying to obtain a dried filter cake.
[0020] In step S3, the drying conditions include drying at a temperature of 80-150°C for more than 10 hours, preferably 100-120°C.
[0021] S4. The dried filter cake is calcined in a muffle furnace under air atmosphere at 400-600° C. for 5-15 hours, and cooled to obtain lanthanum-cerium oxide powder.
[0022] In step S4, the calcination temperature is preferably 450-550° C.; and the calcination time is preferably 8-12 hours.
[0023] 2. Palladium metal impregnation process Lanthanum-cerium oxide was used as a carrier and a supported palladium-based catalyst was obtained by an equal volume impregnation method.
[0024] S5. Take an appropriate amount of palladium nitrate dihydrate solution, evenly disperse the lanthanum cerium oxide powder in the palladium nitrate impregnation solution so that the Pd content in the carrier is 0.5-1.5 wt %, stir at room temperature for 2-8 hours, and stand in the dark for 10-20 hours for aging.
[0025] In step S5, the immersion conditions are as follows: the stirring time is preferably 2 to 4 hours, and the aging time is preferably 10 to 15 hours.
[0026] S6. After the aged catalyst impregnation liquid is dried, it is placed in a muffle furnace and calcined at 300-600°C for 2-5 hours under aerobic conditions and then naturally cooled to room temperature. The obtained powder is a supported palladium-based catalyst.
[0027] In step S6, the drying condition is drying at a temperature of 80-150°C for 4-8 hours, preferably, the drying temperature is 100-120°C; the calcination is carried out under aerobic conditions, preferably in air; the calcination temperature is preferably 400-500°C, and the calcination time is preferably 2-3 hours.
[0028] The third aspect of the present invention provides the use of the above-mentioned Pd-based catalyst in the catalytic oxidation of low-concentration methane. In some exemplary embodiments of the present invention, the catalytic activity of the Pd-based catalyst in the catalytic oxidation of low-concentration methane in the presence or absence of water was evaluated, and the results showed that the Pd-based catalyst provided by the present invention has good catalytic oxidation activity, water resistance stability and regeneration. And it was unexpectedly found that the catalytic oxidation activity of the Pd-based catalyst provided by the present invention was significantly improved under the condition of water vapor. It is suggested that the catalyst of the present invention is suitable for methane oxidation under dry conditions and in a water-containing environment. That is, the catalyst of the present invention has practical application significance in the field of catalytic oxidation of natural gas and automobile exhaust containing water vapor.
[0029] Compared with the prior art, the beneficial effects of the present invention are as follows: the present invention uses tetravalent cerium nitrate and trivalent lanthanum nitrate as starting raw materials, obtains a precursor of a mixture of water and lanthanum cerium oxide through a high-temperature hydrolysis reaction, and obtains a lanthanum cerium mixed oxide with a large specific surface area and strong thermal stability after ammonia precipitation, filtration, washing, and roasting. As a carrier of a methane oxidation catalyst, its catalytic performance can be improved. The methane oxidation catalyst provided by the present invention can effectively alleviate the poisoning effect of water vapor in the reaction atmosphere on the catalyst activity, prevent water poisoning, and exhibit good activity and excellent water resistance stability in the reaction process of catalytic oxidation of low-concentration methane. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 The present invention is a flow chart for preparing the catalyst.
[0031] Figure 2 CeO2, La2O3 and (La-Ce) O x (La2O3 / CeO2=10% / 90%) XRD pattern before and after Pd loading.
[0032] Figure 3 1%Pd / (La-Ce)O x Transmission electron microscope image of (La2O3 / CeO2=10% / 90%) catalyst.
[0033] Figure 4 are (a) CeO2, (b) La2O3 and (c) 1%Pd / (La-Ce) O x Scanning electron microscope image of (La2O3 / CeO2=10% / 90%) catalyst.
[0034] Figure 5 1%Pd / (La-Ce)O x (La2O3 / CeO2=10% / 90%) catalyst stability and water resistance test results in methane oxidation reaction. DETAILED DESCRIPTION
[0035] The present invention is described in detail below in conjunction with the embodiments, but they should not be construed as limiting the scope of protection of the present invention. Example 1
[0036] S1. Weigh a tetravalent Ce(NO3)4 rare earth solution and a trivalent La(NO3)3 solution so that the weight percentage of their oxides is La2O3 / CeO2=10% / 90%, add them into a 1L three-necked flask and dilute with deionized water so that the concentration of the theoretical total oxide (REO) in the rare earth nitrate mixed solution is 30g-REO / L.
[0037] S2. Perform hydrolysis reaction under reflux condition at 100°C for 24 hours. After the hydrolysis reaction is completed, cool to room temperature, add 25-28% ammonia solution until the pH of the solution is 7.5, and continue stirring for 15 minutes.
[0038] S3. After filtering and washing with deionized water, drying at 110°C for more than 10 hours.
[0039] S4, calcining the dried filter cake in a muffle furnace at 500°C for 8 hours under air atmosphere, and obtaining rare earth mixed oxide precursor powder after cooling, expressed as (La-Ce) O x (La2O3 / CeO2=10% / 90%). Example 2
[0040] The preparation method described in Example 1 was followed, except that the weight percentage of the oxides in the nitric acid rare earth mixed solution was La2O3 / CeO2=20% / 80%. The obtained rare earth mixed oxide precursor was (La-Ce) O x (La2O3 / CeO2=20% / 80%). Example 3
[0041] The preparation method described in Example 1 was followed, except that the weight percentage of the oxides in the nitric acid rare earth mixed solution was La2O3 / CeO2=30% / 70%. The obtained rare earth mixed oxide precursor was (La-Ce) O x (La2O3 / CeO2=30% / 70%). Example 4
[0042] The precursor prepared in Example 1 was used as a carrier to obtain a supported palladium-based catalyst by an equal volume impregnation method. The specific impregnation steps are as follows: S1. Dissolve palladium nitrate dihydrate in a 20 mL volumetric flask with deionized water to obtain a palladium nitrate solution of a certain concentration. The palladium content is set to 1 wt%, corresponding to the required palladium nitrate impregnation solution of 5 mL; 5g of rare earth mixed oxide precursor powder is evenly dispersed in the prepared palladium nitrate impregnation solution, stirred at room temperature for 4 hours, and aged for 12 hours in a dark place; S2. The aged catalyst impregnation liquid was dried at 110°C for 6 hours, placed in a muffle furnace, calcined at 450°C for 3 hours in an air atmosphere, and then naturally cooled to room temperature. The final catalyst was expressed as 1% Pd / (La-Ce) O x (La2O3 / CeO2=10% / 90%). Example 5
[0043] The impregnation method described in Example 4 was followed, except that the precursor prepared in Example 2 was used as the carrier. The final catalyst was expressed as 1% Pd / (La-Ce) O x (La2O3 / CeO2=20% / 80%). Example 6
[0044] The impregnation method described in Example 4 was followed, except that the precursor prepared in Example 3 was used as the carrier. The final catalyst was expressed as 1% Pd / (La-Ce) O x (La2O3 / CeO2=30% / 70%). Comparative Example 1
[0045] The cerium carbonate was calcined at 800° C. in an air atmosphere in a muffle furnace for 8 hours, and after cooling, the rare earth oxide precursor was cerium oxide, expressed as 100% CeO2. Comparative Example 2
[0046] Lanthanum carbonate was calcined in a muffle furnace at 800° C. for 8 hours in an air atmosphere, and after cooling, a rare earth oxide precursor was obtained, namely lanthanum oxide, which was expressed as 100% La2O3. Comparative Example 3
[0047] The 100% CeO2 obtained in Comparative Example 1 and the 100% La2O3 obtained in Comparative Example 2 were physically mixed in a weight ratio of La2O3 / CeO2=10% / 90%, and the final catalyst was expressed as 10% La2O3 + 90% CeO2. Comparative Example 4
[0048] The precursor prepared in Comparative Example 1 was used as a carrier and the equal volume impregnation method described in Example 4 was followed. The final catalyst was represented by 1% Pd / 100% CeO2. Comparative Example 5
[0049] The precursor prepared in Comparative Example 2 was used as a carrier and the equal volume impregnation method described in Example 4 was followed. The final catalyst was represented by 1% Pd / 100% La2O3. Comparative Example 6
[0050] The 10% La2O3 + 90% CeO2 catalyst obtained in Comparative Example 3 was used as a carrier and the equal volume impregnation method described in Example 4 was followed. The final catalyst was expressed as 1% Pd / (10% La2O3 + 90% CeO2).
[0051] 1. For 1%Pd / (La-Ce) O x (La2O3 / CeO2=10% / 90%) the morphology and composition of the catalyst were characterized.
[0052] 1. Figure 2 1%Pd / (La-Ce)O x XRD analysis of the catalyst (La2O3 / CeO2=10% / 90%). The pure CeO2 and La2O3 are basically consistent with the standard diffraction peaks of CeO2 (PDF#34-0394) and La2O3 (PDF#05-0602), respectively. Pure CeO2 has obvious diffraction peaks at 28.3°, 32.8°, 47.1°, 55.9° and 58.9°, corresponding to (111), (200), (220), (311) and (400) planes, respectively. La doping causes the CeO2 peak to move to a lower diffraction angle. x (La2O3 / CeO2=10% / 90%) and 1%Pd / (La-Ce) O x No diffraction peak of La2O3 was found in the XRD diffraction pattern of (La2O3 / CeO2=10% / 90%), indicating that La atoms were successfully integrated into the CeO2 lattice, indicating the formation of La-O-Ce solid solution. x On the carrier, due to its high dispersion, no diffraction peak of PdO was found in the XRD spectrum.
[0053] 2. Figure 3 1%Pd / (La-Ce) O was photographed using a transmission electron microscope. x The HRTEM image of the (La2O3 / CeO2=10% / 90%) catalyst clearly depicts the coexistence of three metal oxides, PdO, La2O3 and CeO2. The catalyst mainly exposes the (110), (100), (101) crystal planes of La2O3 and the (200) and (111) crystal planes of CeO2, with a plane spacing of 0.27-0.34nm, indicating that the introduction of La species effectively forms the La-O-Ce lattice interface, and the PdO (100) crystal plane with a plane spacing of 0.30nm is found on the catalyst.
[0054] 3. The specific surface area of the carrier was tested by BET method, and the results are shown in Table 1. It can be seen that the preparation method of the present invention greatly improves the specific surface area of the rare earth mixed oxide.
[0055] Table 1 Specific surface area results of carriers
[0056] Second, the catalyst provided by the present invention can effectively alleviate the poisoning effect of water vapor in the reaction atmosphere on the catalyst activity, prevent water poisoning, and show good activity and excellent water resistance stability in the process of catalytic oxidation of low-concentration methane. The following two types of experiments were mainly conducted.
[0057] 1. Methane performance evaluation test Catalyst activity evaluation A fixed bed tubular flow reactor was filled with 200 mg (40-60 mesh) of catalyst particles and operated at atmospheric pressure. The reactor was supplied with a gas mixture of 1 vol.% methane, 10 vol.% oxygen and 89 vol.% nitrogen at a rate of 100 mL / min, equivalent to a gas hourly space velocity (GHSV) of 30,000 mL·g -1 ·h -1 . The temperature in the reactor was gradually increased at a rate of 10°C / min. During the heating process, the reactor was kept at several selected temperature points for 30 minutes to allow the reaction to reach a stable state. The methane in the product gas was analyzed online by a GC9790Ⅱ gas chromatograph equipped with a TCD detector. The evaluation of the water resistance of the catalyst was also based on the above experimental equipment and steps. The evaluation atmosphere supplied a gas mixture of 1 vol.% methane, 10 vol.% oxygen, 1 vol.% water vapor and 88 vol.% nitrogen as a water reaction condition. The reaction activity is expressed as methane conversion rate. At the same conversion rate, the lower the reaction temperature, the better the activity of the catalyst. The temperature corresponding to 50% conversion rate (T 50 ) and the temperature corresponding to 90% conversion rate (T 90 ) as the evaluation test results, as shown in Table 2.
[0058] Table 2 Evaluation results of methane oxidation activity of precursors and supported palladium catalysts
[0059] As can be seen from Table 2, loading 1wt% Pd can significantly increase the (La-Ce)O x The low temperature activity of the catalysts supported by Pd / (La-Ce) O x (La2O3 / CeO2=10% / 90%) as an example, at 290℃, 1%Pd / (La-Ce) O x The CH4 conversion rate of (La2O3 / CeO2=10% / 90%) reaches 50%, and the CH4 conversion rate reaches 90% at 400℃. 50 and T 90 Ratio (La-Ce) O x (La2O3 / CeO2=10% / 90%) carriers decreased by 226℃ and more than 300℃ respectively.
[0060] Doping with 10% La2O3 can improve the low temperature activity and water resistance of 100% CeO2. x (La2O3 / CeO2=10% / 90%) and 100% CeO2, (La-Ce) O x (La2O3 / CeO2=10% / 90%) T of catalyst under anhydrous conditions 50 The methane oxidation activity of 100% CeO2 in the presence of water was not significantly different from that in the absence of water, while that of (La-Ce) O x (La2O3 / CeO2=10% / 90%) Catalyst T 50 The temperature of the catalyst was 166℃ lower than that of the anhydrous catalyst and 100% CeO2 catalyst. 50 Low 225℃.
[0061] The methane oxidation performance of the physically mixed 10% La2O3+90% CeO2 catalyst and the physically mixed 1% Pd / (10% La2O3+90% CeO2) loaded with Pd is significantly lower than that of the series of catalysts obtained by the carrier preparation method described in Example 1.
[0062] 2. Water resistance and stability test In order to study the effect of H2O on the catalytic performance, the water resistance and stability of 1% Pd / (La-Ce) Ox (La2O3 / CeO2=10% / 90%) catalyst were tested at a reaction temperature of 350°C. Figure 5 The test results of CH4 conversion rate within 15 hours are described. Under anhydrous conditions, CH4 conversion rate is basically stable at about 80%. If water is introduced into the reaction mixture (H2O is turned on), CH4 conversion rate is significantly improved to 94-98%. When the introduction of water is stopped (H2O is turned off), CH4 conversion rate drops back to around 80%.
[0063] No deactivation of the catalyst was observed during the entire water resistance and stability test, and after the addition of water was stopped, the activity of the catalyst immediately recovered to the state without water addition, indicating that the catalyst not only has excellent water resistance and stability, but also has a certain regeneration ability.
[0064] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A palladium-based catalyst for low-concentration methane oxidation, characterized in that: The palladium-based catalyst uses lanthanum cerium oxide as a carrier, and the surface of the carrier is loaded with palladium oxide; the specific surface area of the lanthanum cerium oxide is 100-150 m 2 g ‒1 , La2O3 accounts for 5~50% of the weight of lanthanum cerium oxide.
2. The palladium-based catalyst for low-concentration methane oxidation according to claim 1, characterized in that In the lanthanum-cerium oxide, La2O3 accounts for 10-30% of the weight of the lanthanum-cerium oxide.
3. The palladium-based catalyst for low-concentration methane oxidation according to claim 2, characterized in that The lanthanum-cerium oxide is a La-O-Ce solid solution and has a defective fluorite structure.
4. The palladium-based catalyst for low-concentration methane oxidation according to claim 1, characterized in that In the palladium-based catalyst, the content of palladium is 0.5-1.5 wt%.
5. The method for preparing a palladium-based catalyst for low-concentration methane oxidation according to any one of claims 1 to 4, characterized in that: The specific steps include: S1. According to the weight percentage of the theoretically generated oxide La2O3 in the theoretical lanthanum cerium oxide, respectively weigh the tetravalent Ce(NO3)4 solution and the trivalent La(NO3)3 solution, add them to the reactor and dilute them with deionized water, so that the concentration of the theoretical lanthanum cerium oxide in the mixed solution is 30g-REO / L; S2, hydrolyzing the mixed solution of step S1 under heating conditions of 100-120° C., cooling to room temperature after the reaction, adding ammonia water to adjust the pH of the solution to alkaline, and continuing stirring for 10-60 minutes; filtering, washing, and drying to obtain a dried filter cake; S3, calcining the dried filter cake in an oxygen atmosphere to obtain lanthanum-cerium oxide; S4, using the lanthanum-cerium oxide obtained in step S3 as a carrier, impregnating the palladium solution by an equal volume impregnation method, aging and drying, and then calcining under aerobic conditions to obtain a supported palladium-based catalyst.
6. The method for preparing a palladium-based catalyst for low-concentration methane oxidation according to claim 5, characterized in that: In step S3, the calcination temperature is 400-600° C. and the calcination time is 5-15 hours.
7. The method for preparing a palladium-based catalyst for low-concentration methane oxidation according to claim 5, wherein: The specific steps of S4 are as follows: calculate the volume of palladium nitrate impregnation solution by equal volume impregnation method, evenly disperse lanthanum cerium oxide in the palladium nitrate impregnation solution, stir at room temperature for 2 to 8 hours, and stand in the dark for aging for 10 to 20 hours; after drying, calcine under aerobic conditions to obtain a supported palladium-based catalyst.
8. The method for preparing a palladium-based catalyst for low-concentration methane oxidation according to claim 5, characterized in that: The calcination is carried out in an air atmosphere, the calcination temperature is 300-600° C., and the calcination time is 2-5 hours.
9. Use of the palladium-based catalyst for low-concentration methane oxidation according to any one of claims 1 to 4 in catalytic oxidation of methane.
10. The use according to claim 9, characterized in that: The palladium-based catalyst is used for improving the catalytic oxidation activity of methane in a water-containing environment.
Citation Information
Cited By
Rare earth oxide modified supported palladium catalyst for catalyzing methane oxidation at low temperature and preparation method of rare earth oxide modified supported palladium catalyst
CN120155181A